High-heat-resistance low-thermal-expansion amorphous alloy strip composite adhesive and preparation method thereof
By combining a composite modified epoxy resin matrix and fillers, a high heat-resistant and low thermal expansion adhesive layer is constructed, which solves the problems of high thermal expansion coefficient and thermal mismatch stress of amorphous alloy strips at high temperatures, and achieves N-level heat resistance, low thermal expansion and high insulation adhesive performance.
Patent Information
- Application Number
- CN202611535378.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-20
AI Technical Summary
Existing amorphous alloy strip adhesives are prone to deformation and stress concentration at high temperatures, have a high coefficient of thermal expansion, and are difficult to meet the requirements of Class N heat resistance. Furthermore, the thermal mismatch stress between the adhesive layer and the strip is difficult to eliminate.
A composite modified epoxy resin matrix, negative thermal expansion filler, insulating reinforcing filler, and thermally conductive-insulating bifunctional filler are combined to construct a high heat-resistant and low thermal expansion adhesive layer through chemical bonding and cross-linking network. Combined with flexible segment modification and high cross-linking density, KH-560 interface modifier is used to improve the compatibility between the filler and resin interface.
It achieves high heat resistance, low thermal expansion and high insulation for long-term service at 200℃, effectively eliminates thermal mismatch stress between the adhesive layer and the tape, and significantly improves bonding strength and thermal conductivity.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of adhesive technology, and more specifically to a high heat-resistant, low thermal expansion amorphous alloy strip composite adhesive and its preparation method. Background Technology
[0002] Amorphous alloy materials possess a microstructure characterized by short-range order and long-range disorder, exhibiting excellent soft magnetic properties. With their high permeability and low iron loss, they are widely used in the manufacture of electromagnetic components such as distribution transformers, instrument transformers, and motor stator cores. Amorphous alloy strips are typically prepared using a single-roll rapid solidification process, with thicknesses generally ranging from 10 to 50 μm. In practical applications, multiple layers of amorphous alloy strips need to be laminated to form thicker cores, requiring interlayer adhesives to possess excellent bonding strength, electrical insulation properties, heat resistance, and dimensional stability.
[0003] However, existing epoxy adhesives used for laminating amorphous alloy strips still face several technical bottlenecks. First, conventional adhesives on the market have a high coefficient of thermal expansion, resulting in poor thermal compatibility with the strip and a tendency to deform and concentrate under temperature variations. Second, the smooth and chemically inert surface of amorphous strips makes it difficult for conventional adhesives to form a strong interfacial bond, easily leading to micro-defects and delamination. Third, the curing process of epoxy resin involves significant shrinkage and residual stress, resulting in stress concentration within the cured adhesive layer, which can severely cause warping and deformation of the iron core. Furthermore, the operating temperature of amorphous alloy iron cores in equipment such as transformers and motors can reach above 150℃, and even 200℃ in some conditions, placing stringent requirements on the heat resistance of interlayer adhesives. Existing amorphous strip adhesives generally have low heat resistance ratings (mostly Class F, below 155℃), making them prone to thermal aging, bond strength degradation, and decreased insulation performance under long-term high-temperature service conditions.
[0004] To address the aforementioned issues, researchers have made relevant attempts. For example, CN121343525A discloses an adhesive for amorphous ribbons and its preparation method. This scheme uses a compound of bisphenol F type epoxy resin and epoxidized epoxy resin, combined with calcium carbonate powder and titanate coupling agent. Although this scheme solves the basic requirements of adhesion and insulation, the crosslinking density and rigid structure of its resin system are limited, making it difficult to meet the N-level heat resistance requirements, and it does not involve active control of the coefficient of thermal expansion. CN122104140A discloses a gradient-curing adhesive for polyarylamide amorphous ribbons, using a combination of CTBN-modified E51 epoxy resin and compounded phenolic epoxy resin, combined with a gradient curing process. Although this scheme improves crack resistance through CTBN toughening, the introduction of CTBN significantly reduces the glass transition temperature and heat distortion temperature of the resin. Its heat resistance improvement mainly depends on the phenolic epoxy resin, but the brittleness of phenolic epoxy is relatively high, which contradicts the toughening effect of CTBN, and it also does not solve the problem of excessively high coefficient of thermal expansion.
[0005] None of the above solutions incorporate negative thermal expansion fillers to actively regulate the thermal expansion coefficient of the adhesive layer, making it difficult to eliminate thermal mismatch stress between the adhesive layer and the strip under wide temperature range conditions. How to achieve high heat resistance (N-class), low thermal expansion, and high insulation while maintaining the flexibility of the adhesive layer, and how to improve the thermal conductivity of the adhesive layer to facilitate heat dissipation from the iron core without significantly affecting insulation performance, remain pressing technical challenges in this field. Summary of the Invention
[0006] The purpose of this invention is to provide a high heat-resistant, low thermal expansion amorphous alloy strip composite adhesive and its preparation method, so as to solve the problems mentioned in the background art.
[0007] To achieve the above objectives, on the one hand, the present invention provides a high heat-resistant and low thermal expansion amorphous alloy strip composite adhesive, comprising, by weight parts: 67-83 parts of composite modified epoxy resin matrix, 5-18 parts of composite filler, 15-25 parts of heat-resistant curing agent, 1-4 parts of curing accelerator, 0.1-0.4 parts of interface modifier, 2-10 parts of reactive diluent, and 0.5-1.5 parts of antioxidant;
[0008] The composite modified epoxy resin matrix comprises epoxy-flexible segment modified bisphenol A type epoxy resin, phenolic epoxy resin and alicyclic modified epoxy resin in a mass ratio of (32-38):(10-15):(25-30).
[0009] The surface of the composite filler has active hydroxyl groups, including negative thermal expansion filler, insulating reinforcement filler and thermally conductive-insulating bifunctional filler with a mass ratio of (2-8):(2-6):(1-4);
[0010] The interface modifier is γ-glycidyl etheroxypropyltrimethoxysilane (KH560), whose alkoxy group at one end of the molecule can undergo a dehydration condensation reaction with the active hydroxyl groups on the surface of the composite filler after hydrolysis to form a chemical bond.
[0011] In alicyclic modified epoxy resins, the epoxy groups are directly attached to the alicyclic rings, forming a high-crosslink density rigid network together with the multifunctional structure of phenolic epoxy resins. Combined with a heat-resistant curing agent, this results in a tightly bound rigid crosslinked network after curing, exhibiting high crosslink density and high heat distortion temperature, maintaining structural stability at 200℃ for extended periods. This structural feature endows the adhesive layer with excellent high-temperature dimensional stability and heat aging resistance, enabling it to operate under N-class (200℃) high-temperature conditions in amorphous iron cores. Epoxy-flexible segment modified bisphenol A epoxy resins, by introducing flexible segments (such as the rubber segments of carboxyl-terminated nitrile butadiene rubber (CTBN)) into the bisphenol A epoxy resin backbone, reduce the rigidity of the epoxy molecular chain, giving the adhesive layer excellent flexibility and impact resistance. During curing, CTBN forms micro-phase-separated rubber particles dispersed within the continuous epoxy phase. These rubber particles act as stress concentration points, inducing shear bands and crazing, effectively absorbing impact energy. Alicyclic modified epoxy resin and phenolic epoxy resin together provide a high crosslinking density rigid skeleton, while CTBN modified epoxy resin provides a flexible toughening phase. These three are blended in a specific ratio. The flexible segments provide toughening and vibration absorption, while the alicyclic structure and phenolic epoxy skeleton provide high heat resistance, low thermal expansion, and high insulation. The introduction of flexible segment modified epoxy will increase the system's coefficient of thermal expansion to some extent, but the low CTE of the alicyclic epoxy and the negative thermal expansion effect of the filler can jointly offset this adverse effect, keeping the overall CTE of the system at a low level. Simultaneously, the high crosslinking density of the heat-resistant curing agent further enhances the degree of crosslinking and thermal stability of the system, ensuring the long-term reliability of the adhesive layer at 200℃.
[0012] Specifically, the curing accelerator is 2-ethyl-4-methylimidazole, and the reactive diluent is butyl glycidyl ether and / or phenyl glycidyl ether.
[0013] The alkoxy group at one end of KH-560 undergoes hydrolysis to generate silanol groups, which then chemically bond with the hydroxyl groups on the surface of the composite filler, forming a stable silanized layer on the filler surface. Under the action of a latent curing agent / curing accelerator curing system, the epoxy group at its end participates in the ring-opening polymerization reaction together with the epoxy group of the epoxy resin, introducing the composite filler into the cross-linking network through chemical bonds.
[0014] Preferably, the negative thermal expansion filler is nano-zirconium tungstate with an average particle size of 50-200 nm and a negative thermal expansion coefficient of -8.0 × 10⁻⁶. -6 ~-10.0×10 -6 ℃ -1This invention selects nano-zirconium tungstate (ZrW2O8) as a negative thermal expansion filler, which exhibits isotropic negative thermal expansion characteristics over a wide temperature range of -270-750℃, effectively counteracting the positive thermal expansion of the epoxy resin matrix during heating. By adjusting the amount of ZrW2O8 added, its contribution to negative thermal expansion is matched with the increase in positive thermal expansion introduced by CTBN modification, achieving precise control of the coefficient of thermal expansion even with low filler content.
[0015] Preferably, the insulating reinforcing filler is nano-silica with a specific surface area of 150-300 m². 2 / g. Nano-silica possesses an extremely high specific surface area, and even a low addition amount can form numerous filler-resin interfaces in the resin matrix. These interfaces act as "deep traps," restricting carrier movement and effectively improving the density and volume resistivity of the adhesive layer. Simultaneously, nano-silica, as an inorganic filler, exhibits excellent thermal stability, further enhancing the heat resistance of the composite material.
[0016] Preferably, the thermally conductive and electrically insulating bifunctional filler is hydroxylated hexagonal boron nitride nanosheets, with an average sheet diameter of 100-500 nm. Hexagonal boron nitride (h-BN) possesses excellent thermal conductivity and electrical insulation properties. After hydroxylation and KH-560 modification, its interfacial compatibility with the resin matrix is significantly improved, forming an effective thermally conductive network even with low filler content, greatly increasing the thermal conductivity of the adhesive layer and facilitating heat dissipation during amorphous iron core operation. h-BN itself has excellent thermal stability (withstanding temperatures above 1000℃ in air), and hydroxylation modification does not change its intrinsic heat resistance; its addition further enhances the heat aging resistance of the adhesive layer. The hydroxylated hexagonal boron nitride nanosheets and silica form a complementary filler system—silica mainly contributes high insulation strength and low thermal expansion, while h-BN mainly contributes high thermal conductivity and auxiliary insulation, jointly improving the overall performance and heat resistance of the adhesive layer.
[0017] Preferably, the epoxy-flexible segment modified bisphenol A epoxy resin is prepared by modifying bisphenol A epoxy resin with carboxyl-terminated nitrile butadiene rubber (CTBN), wherein the amount of carboxyl-terminated nitrile butadiene rubber (CTBN) added is 5-15% of the mass of the bisphenol A epoxy resin. During the curing process, the rubber segments of CTBN can form a micro-phase-separated "island structure," effectively absorbing impact energy and significantly improving the fracture toughness and fatigue resistance of the adhesive layer.
[0018] Preferably, the alicyclic modified epoxy resin is 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester and / or bis((3,4-epoxycyclohexyl)methyl)adipate. These two types of alicyclic epoxy resins do not contain unsaturated double bonds in their molecular structure and possess characteristics such as low viscosity, high reactivity, good physical and mechanical properties of the cured product, excellent weather resistance, and excellent electrical insulation properties. The rigidity of their alicyclic structure endows the adhesive layer with high heat resistance, a low coefficient of thermal expansion, and excellent dimensional stability, forming a structural complement to the flexible segment modified epoxy resin.
[0019] Preferably, the heat-resistant curing agent is 4,4'-diaminodiphenyl sulfone (DDS) and / or nadic anhydride. The crosslinking network of DDS-cured resin has excellent thermal stability, and the thermal decomposition temperature can reach above 350°C when combined with the post-curing process, which can meet the heat resistance requirements of N-class (200°C) for long-term use.
[0020] On the other hand, the present invention also discloses a method for preparing the above-mentioned high heat resistance and low thermal expansion amorphous alloy strip composite adhesive, comprising the following steps:
[0021] (1) The negative thermal expansion filler, the insulating reinforcement filler and the thermally conductive-insulating bifunctional filler were modified with γ-glycidyl ether oxypropyltrimethoxysilane to obtain the modified composite filler.
[0022] (2) Epoxy-flexible segment modified bisphenol A type epoxy resin, phenolic epoxy resin and alicyclic modified epoxy resin and antioxidant are mixed evenly, and an active diluent is added. After mixing, a composite modified epoxy resin matrix mixture is obtained.
[0023] (3) The modified composite filler is mixed with the composite modified epoxy resin matrix mixture, dispersed and ground to obtain a resin mixture in which the filler is uniformly dispersed;
[0024] (4) Add the heat-resistant curing agent and curing accelerator to the resin mixture, stir, degas under vacuum and filter to obtain the composite adhesive.
[0025] Preferably, in step (3), the dispersion and grinding include:
[0026] Disperse at high speed for 60-120 minutes at 60-80℃ and 800-1500rpm, then use a three-roll mill for assisted dispersion, grinding 2-4 times with a grinding gap of 10-50μm, and the temperature during grinding is ≤60℃.
[0027] Preferably, in step (1), the negative thermal expansion filler, the insulating reinforcing filler, and the thermally conductive-insulating bifunctional filler are modified with γ-glycidyl etheroxypropyltrimethoxysilane to obtain a modified composite filler, including:
[0028] The negative thermal expansion filler, the insulating reinforcement filler, and the thermally conductive-insulating bifunctional filler were vacuum dried separately.
[0029] γ-glycidyl etheroxypropyltrimethoxysilane was dissolved in an ethanol / water mixture to prepare a modified solution;
[0030] The dried fillers were added to the modification liquid, stirred and ultrasonically dispersed for surface modification, and then vacuum dried to obtain modified negative thermal expansion fillers, modified insulating and reinforcing fillers, and modified thermally conductive and insulating bifunctional fillers. The three modified fillers were then mixed evenly to obtain modified composite fillers.
[0031] The beneficial effects of this invention are as follows:
[0032] (1) This invention constructs a high heat-resistant composite modified epoxy resin matrix that combines rigidity and flexibility by compounding alicyclic modified epoxy resin, phenolic epoxy resin and epoxy-flexible segment modified bisphenol A type epoxy resin. The multifunctional rigid structure of alicyclic modified epoxy resin and phenolic epoxy resin provides a high crosslinking density skeleton, giving the adhesive layer N-level heat resistance; epoxy-flexible segment modified bisphenol A type epoxy resin provides a flexible toughening phase, and the flexible segment provides toughening and vibration absorption function. The high crosslinking density characteristics of the heat-resistant curing agent ensure the full formation of the crosslinking network. From the resin matrix itself, it solves the contradiction between N-level high heat resistance, flexible bonding and low thermal expansion insulation in the amorphous ribbon stacking scenario.
[0033] (2) The present invention combines negative thermal expansion filler, insulating reinforcing filler and thermally conductive-insulating dual-function filler. Under the premise of ensuring the continuous and dense film formation of ultra-thin coating, it effectively reduces the thermal expansion coefficient of the adhesive layer by relying on the triple synergistic effect of "thermal expansion offset", "pore filling" and "thermal conductivity enhancement", while maintaining high insulation performance and excellent thermal conductivity. It achieves a balance of high heat resistance, low thermal expansion, high insulation and good heat dissipation with low filler content.
[0034] (3) This invention uses KH-560 interface modifier to modify the surface of three types of fillers. The epoxy groups at the end of KH-560 participate in the ring-opening polymerization reaction together with the epoxy groups of epoxy resin during the curing process, introducing the filler into the cross-linking network through chemical bonds, effectively improving the compatibility of the filler / resin interface, significantly improving the bonding strength, and eliminating interlayer delamination and leakage. The composite filler system of nano-silica and hexagonal boron nitride utilizes the high specific surface area of nano-silica to provide a dense insulating barrier and the plate-like structure of hexagonal boron nitride to provide a longer insulating path and thermal conduction channel, achieving simultaneous improvement of insulation performance and thermal conductivity with low filler content. Detailed Implementation
[0035] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.
[0036] It should be noted that all reagents and raw materials used in this invention are commercially available, and the reagents are of analytical grade.
[0037] Bisphenol A type epoxy resin is from Shandong Deyuan Epoxy Technology Co., Ltd., grade E-51. Carboxyl-terminated butadiene-acrylonitrile rubber is from Shenzhen Masni Elastomer Co., Ltd., grade CTBN. 3,4-Epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester is from Jiangsu Taiter New Material Technology Co., Ltd., grade TTA21. Bis((3,4-epoxycyclohexyl)methyl)adipate is from Jiangsu Taiter New Material Technology Co., Ltd., grade TTA26. Zirconium tungstate is from Hunan Yuxiling New Material Co., Ltd., CAS number 16853-74-0. Nano-silica is from Jiangsu Xianfeng Nanomaterials Technology Co., Ltd., model XFI03, specific surface area 160m². 2 / g. Hydroxylated hexagonal boron nitride nanosheets are from Jiangsu Xianfeng Nanomaterials Technology Co., Ltd., model number XFBN03-2. Hexagonal boron nitride nanosheets are from Jiangsu Xianfeng Nanomaterials Technology Co., Ltd., model number XFBN03-1. Phenolic epoxy resin is from Guangzhou Taiji New Materials Co., Ltd., model number F-51.
[0038] Preparation of epoxy-flexible segment modified bisphenol A epoxy resin (parts by weight): 90 parts of bisphenol A epoxy resin and 10 parts of carboxyl-terminated butadiene-acrylonitrile rubber were added to a reaction vessel and stirred at 135℃ and 400rpm for 3 hours under nitrogen protection. The reaction was monitored by infrared spectroscopy at 1735cm. -1 The reaction endpoint is determined when the peak area no longer increases, based on the appearance of the characteristic peak of the ester bond, thus obtaining epoxy-flexible segment modified bisphenol A type epoxy resin.
[0039] Example 1
[0040] This embodiment provides a high heat-resistant, low thermal expansion amorphous alloy strip composite adhesive, which, by weight, comprises: 35 parts of epoxy-flexible segment modified bisphenol A type epoxy resin, 12 parts of phenolic epoxy resin, 28 parts of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester, 4 parts of nano-zirconium tungstate, 3 parts of nano-silica, 2 parts of hydroxylated hexagonal boron nitride nanosheets, 20 parts of DDS, 2.0 parts of 2-ethyl-4-methylimidazolium, 0.18 parts of KH-560, 4 parts of butyl glycidyl ether, and 1.0 parts of antioxidant 1010.
[0041] The preparation method of the composite adhesive is as follows:
[0042] (1) Pretreatment of fillers: Nano-zirconium tungstate was vacuum dried at 120℃ and vacuum degree -0.095MPa for 6h; KH-560 was dissolved in a mixed solvent of ethanol / water volume ratio of 95:5 and hydrolyzed at 60℃ for 30min to prepare a 6wt% hydrolysate; each dried filler was added to the hydrolysate and surface modified by stirring at 80℃ and 300rpm for 2h (ultrasonic-assisted dispersion, power 300W, frequency 30kHz, time 20min), and then vacuum dried at 100℃ for 4h to obtain modified nano-zirconium tungstate filler; nano-silica and hydroxylated hexagonal boron nitride nanosheets were pretreated in the same way to obtain modified nano-silica filler and modified hydroxylated hexagonal boron nitride nanosheet filler, and then the three were mixed evenly to obtain a modified filler mixture;
[0043] (2) Preparation and dilution of resin matrix: Epoxy-flexible segment modified bisphenol A type epoxy resin, phenolic epoxy resin, 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester and antioxidant 1010 are added to the reaction vessel and stirred at 80℃ and 300rpm for 60min until uniform. Then the temperature is lowered to 55℃, butyl glycidyl ether is added, and stirring is continued for 20min to obtain a composite modified epoxy resin matrix mixture.
[0044] (3) Filler dispersion: The modified filler mixture is added to the composite modified epoxy resin matrix mixture and dispersed at high speed for 90 min at 70℃ and 1200 rpm. Then, it is ground 3 times with a three-roll mill for 10 min each time, with a grinding gap of 30 μm (to prevent agglomeration). During the grinding process, the material temperature is controlled at 50±2℃ to obtain a resin mixture with uniformly dispersed filler.
[0045] (4) Introduction of curing system: DDS and 2-ethyl-4-methylimidazolium were added to the resin mixture and stirred at 85°C and 500 rpm for 50 min. The mixture was then degassed under vacuum at -0.095 MPa for 20 min and then filtered under pressure through a 150-mesh filter to obtain the composite adhesive.
[0046] Example 2
[0047] This embodiment provides a high heat-resistant, low thermal expansion amorphous alloy strip composite adhesive, which, by weight, comprises: 32 parts of epoxy-flexible segment modified bisphenol A type epoxy resin, 10 parts of phenolic epoxy resin, 25 parts of bis((3,4-epoxycyclohexyl)methyl)adipate, 2 parts of nano zirconium tungstate, 2 parts of nano silica, 1 part of hydroxylated hexagonal boron nitride nanosheets, 15 parts of DDS, 1.0 part of 2-ethyl-4-methylimidazolium, 0.1 part of KH-560, 2 parts of butyl glycidyl ether, and 0.5 parts of antioxidant 1010.
[0048] The preparation method of the composite adhesive is as follows:
[0049] (1) Pretreatment of fillers: Nano-zirconium tungstate was vacuum dried at 110℃ and vacuum degree -0.095MPa for 7h; KH-560 was dissolved in a mixed solvent of ethanol / water volume ratio of 95:5 and hydrolyzed at 60℃ for 30min to prepare a 6wt% hydrolysate; each dried filler was added to the hydrolysate and surface modified by stirring at 70℃ and 300rpm for 2.5h (ultrasonic-assisted dispersion, power 250W, frequency 30kHz, time 25min), and then vacuum dried at 100℃ for 4h to obtain modified nano-zirconium tungstate filler; nano-silica and hydroxylated hexagonal boron nitride nanosheets were pretreated in the same way to obtain modified nano-silica filler and modified hydroxylated hexagonal boron nitride nanosheet filler, and then the three were mixed evenly to obtain a modified filler mixture;
[0050] (2) Preparation and dilution of resin matrix: Epoxy-flexible segment modified bisphenol A type epoxy resin, phenolic epoxy resin, bis((3,4-epoxycyclohexyl)methyl) adipate and antioxidant 1010 are added to the reactor and stirred at 78°C and 300 rpm for 60 min until uniform. Then the temperature is lowered to 52°C, butyl glycidyl ether is added, and stirring is continued for 20 min to obtain a composite modified epoxy resin matrix mixture.
[0051] (3) Filler dispersion: The modified filler mixture is added to the composite modified epoxy resin matrix mixture and dispersed at high speed for 100 min at 75℃ and 1000 rpm. Then, it is ground 4 times with a three-roll mill for 10 min each time, with a grinding gap of 20 μm. The material temperature is controlled at 50±2℃ during the grinding process to obtain a resin mixture with uniformly dispersed filler.
[0052] (4) Introduction of curing system: DDS and 2-ethyl-4-methylimidazolium were added to the resin mixture and stirred at 80°C and 500 rpm for 45 min. The mixture was then degassed under vacuum at -0.095 MPa for 15 min and then filtered under pressure through a 200-mesh filter to obtain the composite adhesive.
[0053] Example 3
[0054] This embodiment provides a high heat-resistant, low thermal expansion amorphous alloy strip composite adhesive, which, by weight, comprises: 38 parts of epoxy-flexible segment modified bisphenol A type epoxy resin, 15 parts of phenolic epoxy resin, 30 parts of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester, 8 parts of nano-zirconium tungstate, 6 parts of nano-silica, 4 parts of hydroxylated hexagonal boron nitride nanosheets, 25 parts of DDS, 4 parts of 2-ethyl-4-methylimidazolium, 0.3 parts of KH-560, 10 parts of phenyl glycidyl ether, and 1.5 parts of antioxidant 1010.
[0055] The preparation method of the composite adhesive is as follows:
[0056] (1) Pretreatment of fillers: nano-zirconium tungstate was vacuum dried at 140℃ and vacuum degree -0.095MPa for 4h; KH-560 was dissolved in a mixed solvent of ethanol / water volume ratio of 95:5 and hydrolyzed at 60℃ for 30min to prepare a 6wt% hydrolysate; each dried filler was added to the hydrolysate and surface modified by stirring at 95℃ and 300rpm for 1.5h (ultrasonic-assisted dispersion, power 450W, frequency 30kHz, time 12min), and then vacuum dried at 100℃ for 4h to obtain modified nano-zirconium tungstate filler; nano-silica and hydroxylated hexagonal boron nitride nanosheets were pretreated in the same way to obtain modified nano-silica filler and modified hydroxylated hexagonal boron nitride nanosheet filler, and then the three were mixed evenly to obtain a modified filler mixture;
[0057] (2) Preparation and dilution of resin matrix: Epoxy-flexible segment modified bisphenol A type epoxy resin, phenolic epoxy resin, 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester and antioxidant 1010 are added to the reaction vessel and stirred at 85℃ and 300rpm for 60min until uniform. Then the temperature is lowered to 58℃, phenyl glycidyl ether is added, and stirring is continued for 20min to obtain a composite modified epoxy resin matrix mixture.
[0058] (3) Filler dispersion: The modified filler mixture is added to the composite modified epoxy resin matrix mixture and dispersed at high speed for 70 min at 65℃ and 1400 rpm. Then, it is ground twice with a three-roll mill for 10 min each time, with a grinding gap of 45 μm. During the grinding process, the material temperature is controlled at 50±2℃ to obtain a resin mixture with uniformly dispersed filler.
[0059] (4) Introduction of curing system: DDS and 2-ethyl-4-methylimidazolium were added to the resin mixture and stirred for 60 min at 90℃ and 550 rpm. The mixture was then degassed under vacuum at -0.095 MPa for 25 min and then filtered under pressure through a 100-mesh filter to obtain the composite adhesive.
[0060] Example 4
[0061] This embodiment provides a high heat-resistant, low thermal expansion amorphous alloy strip composite adhesive, which, by weight, comprises: 36 parts of epoxy-flexible segment modified bisphenol A type epoxy resin, 13 parts of phenolic epoxy resin, 26 parts of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester, 5 parts of nano-zirconium tungstate, 3 parts of nano-silica, 2 parts of hydroxylated hexagonal boron nitride nanosheets, 22 parts of DDS, 2.5 parts of 2-ethyl-4-methylimidazolium, 0.2 parts of KH-560, 5 parts of butyl glycidyl ether, and 1.2 parts of antioxidant 1010.
[0062] The preparation method of the composite adhesive is as follows:
[0063] (1) Pretreatment of fillers: Nano-zirconium tungstate was vacuum dried at 135℃ and vacuum degree -0.095MPa for 5h; KH-560 was dissolved in a mixed solvent of ethanol / water volume ratio of 95:5 and hydrolyzed at 60℃ for 30min to prepare a 6wt% hydrolysate; each dried filler was added to the hydrolysate and surface modified by stirring at 85℃ and 300rpm for 2h (ultrasonic-assisted dispersion, power 350W, frequency 30kHz, time 18min), and then vacuum dried at 100℃ for 4h to obtain modified nano-zirconium tungstate filler; nano-silica and hydroxylated hexagonal boron nitride nanosheets were pretreated in the same way to obtain modified nano-silica filler and modified hydroxylated hexagonal boron nitride nanosheet filler, and then the three were mixed evenly to obtain a modified filler mixture;
[0064] (2) Preparation and dilution of resin matrix: Epoxy-flexible segment modified bisphenol A type epoxy resin, phenolic epoxy resin, 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester and antioxidant 1010 are added to the reaction vessel and stirred at 82℃ and 300rpm for 60min until uniform. Then the temperature is lowered to 50℃, butyl glycidyl ether is added, and stirring is continued for 20min to obtain a composite modified epoxy resin matrix mixture.
[0065] (3) Filler dispersion: The modified filler mixture was added to the composite modified epoxy resin matrix mixture and dispersed at high speed for 80 min at 78℃ and 1300 rpm. Then, it was ground 3 times with a three-roll mill for 10 min each time, with a grinding gap of 25 μm. The material temperature was controlled at 50±2℃ during the grinding process to obtain a resin mixture with uniformly dispersed filler.
[0066] (4) Introduction of curing system: DDS and 2-ethyl-4-methylimidazolium were added to the resin mixture and stirred at 88°C and 450 rpm for 55 min. The mixture was then degassed under vacuum at -0.095 MPa for 18 min and then filtered under pressure through a 150-mesh filter to obtain the composite adhesive.
[0067] Comparative Example 1
[0068] Compared with Example 1, the difference is that the composite filler does not include nano-zirconium tungstate, and the composite filler contains 6 parts of nano-silica and 3 parts of hydroxylated hexagonal boron nitride nanosheets.
[0069] Comparative Example 2
[0070] Compared with Example 1, the difference is that the composite filler does not include hydroxylated hexagonal boron nitride nanosheets, and the composite filler contains 5 parts of nano-silica and 4 parts of nano-zirconium tungstate.
[0071] Comparative Example 3
[0072] Compared with Example 1, the difference is that the composite filler does not include nano-silica, and the composite filler contains 4 parts of nano-zirconium tungstate and 5 parts of hydroxylated hexagonal boron nitride nanosheets.
[0073] Comparative Example 4
[0074] The difference from Example 1 is that the hydroxylated hexagonal boron nitride nanosheets in the composite filler are replaced with an equal mass of unhydroxylated hexagonal boron nitride nanosheets.
[0075] Comparative Example 5
[0076] Compared with Example 1, the difference is that the composite filler does not include nano-silica and hydroxylated hexagonal boron nitride nanosheets, but only includes 9 parts of nano-zirconium tungstate.
[0077] Comparative Example 6
[0078] The difference compared to Example 1 is that the interface modifier KH-560 is not added. The composite filler in the preparation method does not undergo KH-560 surface modification treatment.
[0079] Comparative Example 7
[0080] Compared to Example 1, the difference lies in that the resin matrix comprises only 75 parts of epoxy-flexible segment modified bisphenol A type epoxy resin, excluding 3,4-epoxycyclohexylformic acid-3',4'-epoxycyclohexylmethyl ester and phenolic epoxy resin. The resin matrix preparation and dilution steps in the preparation method use only epoxy-flexible segment modified bisphenol A type epoxy resin.
[0081] Comparative Example 8
[0082] Compared to Example 1, the difference lies in that the resin matrix comprises only 75 parts of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester, excluding epoxy-flexible segment modified bisphenol A type epoxy resin and phenolic epoxy resin. The resin matrix preparation and dilution steps in the preparation method use only 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester.
[0083] Comparative Example 9
[0084] Compared with Example 1, the difference is that the epoxy-flexible segment modified bisphenol A epoxy resin is replaced with an equal part by weight of bisphenol A epoxy resin E-51.
[0085] Comparative Example 10
[0086] Compared to Example 1, the difference lies in that the resin matrix consists only of 75 parts of phenolic epoxy resin, excluding epoxy-flexible segment modified bisphenol A type epoxy resin and 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester. The resin matrix preparation and dilution steps in the preparation method use only phenolic epoxy resin.
[0087] The composite adhesives prepared in Examples 1-4 and Comparative Examples 1-10 were subjected to performance testing. The curing conditions for the composite adhesives were as follows: After preparing test samples of the corresponding specifications according to the requirements of each testing standard, the composite adhesives were placed in an air-circulating oven and cured according to the following segmented gradient heating program: First stage: heating from room temperature to 110°C at a heating rate of 2°C / min and holding for 75 min; Second stage: heating to 165°C at a heating rate of 2°C / min and holding for 100 min; Third stage: heating to 240°C at a heating rate of 2°C / min and holding for 150 min; Fourth stage: heating to 255°C at a heating rate of 1°C / min and holding for 5 h; and then cooling to below 60°C at a cooling rate of 1°C / min before removing from the oven.
[0088] The test metrics and methods are as follows:
[0089] Surface resistivity: Measured according to IEC 60404-11:2021 "Magnetic materials—Part 11: Method for measurement of surface insulation resistance of electrical steel strips and sheets". After the composite adhesive sample was coated onto the surface of the amorphous alloy strip and cured, the surface insulation resistance was measured using a surface insulation resistance tester. The results are expressed in Ω·mm. 2 / lam. indicates.
[0090] Peel strength of the floating roller: The test was conducted according to DIN EN 1464:2010-6 "Adhesives - Determination of peel strength of high-strength adhesives - Floating roller method". The sample width was 25 mm. Rigid amorphous alloy strip and flexible metal were bonded together using a composite adhesive sample. The sample was then subjected to a peel test at a constant speed of 100 mm / min on a floating roller peel tester. The peel force was recorded and the peel strength was calculated. The results are expressed in N / mm².
[0091] T-peel strength: The test was performed according to GB / T 2791-1995 "Test method for T-peel strength of adhesives, flexible materials to flexible materials". Two amorphous alloy strips coated with composite adhesive were peeled off in a T-shape, and the average peel force (N) and peel strength (N / mm) were recorded.
[0092] Coefficient of thermal expansion (CTE): Measured using a thermomechanical analyzer (TMA) according to GB / T 2572-2005 "Test Method for Average Linear Expansion Coefficient of Fiber Reinforced Plastics". Temperature range: 30~200℃, heating rate: 5℃ / min. Results are expressed as ×10⁻⁶. -6 ℃ -1 express.
[0093] Volume resistivity: The volume resistivity was measured in accordance with GB / T 31838.2-2019 "Dielectric and resistive properties of solid insulating materials - Part 2: Resistive properties (DC method) - Volume resistivity and volume resistivity". A high-resistivity meter was used for the measurement. The test conditions were temperature 23±2℃, relative humidity 50±5%, and test voltage 500V. The results are expressed in Ω·cm.
[0094] Thermal conductivity: The test method for determining thermal diffusivity was performed using the laser flash method, in accordance with ASTM E1461-13 (2022) "Standard Test Method for Determination of Thermal Diffusivity by Flash Method". The results are expressed as W / (m·K).
[0095] Glass transition temperature (Tg): The glass transition temperature was determined in accordance with GB / T 19466.2-2025 "Differential scanning calorimetry (DSC) for plastics - Part 2: Determination of glass transition temperature and step height". A differential scanning calorimeter was used for the determination, with a heating rate of 10℃ / min. The results are expressed in ℃.
[0096] Thermogravimetric analysis temperature (Td, 5% thermogravimetric analysis): determined by thermogravimetric analysis instrument according to GB / T 27761-2011 "Test method for weight loss and residual amount by thermogravimetric analysis", with a heating rate of 10℃ / min and a nitrogen atmosphere. The results are expressed in ℃.
[0097] Heat resistance rating: The heat resistance rating is determined according to GB / T 11021-2014 "Heat Resistance and Representation Method of Electrical Insulation". Standard samples of the composite adhesive are prepared and tested according to the heat aging test procedures and evaluation criteria specified in GB / T 11021-2014 to determine its heat resistance rating. The heat resistance ratings, from lowest to highest, are: Y (90℃), A (105℃), E (120℃), B (130℃), F (155℃), H (180℃), N (200℃), and R (220℃).
[0098] The test results are shown in Table 1.
[0099] Table 1 Performance Test Results
[0100] As shown in the table above, the coefficient of thermal expansion of Examples 1-4 of this invention is 22.6~38.6×10⁻⁴. -6 ℃ -1 The CTE (22.6 × 10⁻⁶ °C) of Example 3 -1 The total filler content in Example 3 was significantly lower than in other examples, directly reflecting the effect of the total filler content on the coefficient of thermal expansion. Example 3 had the highest total filler content (18 parts), including 8 parts of the negative thermal expansion filler ZrW2O8, which significantly enhanced the negative thermal expansion offsetting effect of the system. The composite adhesives prepared in these examples outperformed the comparative examples in key performance aspects, as detailed below:
[0101] The significantly increased CTE in Comparative Example 1 (without ZrW2O8) directly demonstrates that the nano-zirconium tungstate negative thermal expansion filler undergoes volume shrinkage during heating through changes in lattice thermal vibration modes, thus offsetting the positive thermal expansion of the resin matrix—a "thermal expansion cancellation" effect. The absence of ZrW2O8 causes the CTE to return to near the intrinsic values of alicyclic epoxy, phenolic epoxy, and flexible epoxy composite systems, indicating that ZrW2O8 is a key functional component for achieving low thermal expansion. Simultaneously, the increased CTE leads to increased residual thermal stress within the cured adhesive layer and a slight decrease in peel strength.
[0102] The thermal conductivity of Comparative Example 2 (without h-BN) decreased significantly, demonstrating that the lamellar structure of h-BN can form an effective thermally conductive percolation network at low addition levels, thereby improving phonon transport efficiency. Simultaneously, the lamellar structure of h-BN provides a longer insulation path, and its absence leads to a decrease in both surface resistivity and volume resistivity.
[0103] Comparative Example 3 (without SiO2) showed lower surface resistivity and volume resistivity than Example 1, demonstrating that the high specific surface area of nano-SiO2 can form numerous filler-resin interfaces even at low addition levels. These interfaces act as "deep traps," restricting carrier movement, and the insulation performance decreases after the absence of SiO2. Simultaneously, SiO2 nanoparticles can improve the dispersion state of h-BN in the resin, making the thermally conductive network of h-BN more complete; its absence leads to a slight decrease in thermal conductivity. The contribution of SiO2 to peel strength lies in its nanoparticles acting as physical crosslinking points, enhancing the cohesive strength of the resin matrix.
[0104] The properties of Comparative Example 4 (h-BN without hydroxylation) were all lower than those of Example 1. This is because the surface hydroxyl density of unhydroxylated h-BN is extremely low, making effective grafting of KH-560 difficult. The interfacial compatibility between the filler and the resin matrix is poor, and h-BN exists as aggregates in the resin. This results in an incomplete thermal conductivity network (decreased thermal conductivity), defects in the insulation path (decreased surface and volume resistivity), and interfacial defects becoming stress concentration points (significantly reduced peel strength). This directly demonstrates the crucial role of the pre-hydroxylation → KH-560 grafting modification process chain in the functionality of h-BN.
[0105] Comparative Example 5 (ZrW2O8 only) exhibited the lowest CTE, demonstrating that the negative thermal expansion effect of ZrW2O8 can also be utilized in a single filler system. However, its insulation and thermal conductivity were significantly lower than those of Example 1. Although the CTE of Comparative Example 5 could be reduced to a low level, its insulation and thermal conductivity were severely insufficient, failing to meet the comprehensive performance requirements of amorphous iron cores. The addition of nano-SiO2 and h-BN was not intended to further reduce CTE, but rather to improve insulation performance by utilizing the "deep trap" interface effect of SiO2 and to construct a thermally conductive percolation network using the lamellar structure of h-BN, while maintaining a low CTE. Through a synergistic mechanism of each component performing its specific function and complementing each other, the ternary composite filler system achieved a comprehensive improvement in insulation, thermal conductivity, and mechanical properties within an acceptable CTE range.
[0106] Comparative Example 6 (without KH-560) exhibited the lowest peel strength, demonstrating that the mechanism by which the KH-560 interfacial modifier participates in the curing reaction through its terminal epoxy groups and introduces the filler into the cross-linking network via chemical bonds is crucial for ensuring interfacial bond strength. Without KH-560, only physical intercalation exists between the filler and resin, without chemical bonding, resulting in the weakest interfacial adhesion. Simultaneously, the surface resistivity decreased to 1962 Ω·mm. 2 / lam. indicates that interface defects also directly degrade insulation performance.
[0107] The results of Comparative Examples 1-6 fully demonstrate the synergistic mechanism among the components of the filler and interface modification system of this invention: ZrW2O8 provides thermal expansion compensation, nano-SiO2 provides insulation and mechanical reinforcement, and h-BN provides thermal conductivity and insulation assistance. The particle size differences among the three components form a multi-level gradation filling structure, jointly achieving the multiple objectives of "low thermal expansion, high insulation, and enhanced thermal conductivity." Simultaneously, the pre-hydroxylation treatment of h-BN and the KH-560 interface modifier are key process guarantees for achieving the filler-resin chemical bonding interface and ensuring peel strength. The absence of any single component or the omission of any key treatment step will lead to a significant decrease in overall performance, making it impossible to simultaneously meet the amorphous iron core's requirements for a balance of high heat resistance, low thermal expansion, high insulation, and good heat dissipation.
[0108] Comparative Example 7 (single flexible epoxy) had a Tg of only 159°C and a heat resistance rating of only F, demonstrating that alicyclic modified epoxy resin is an irreplaceable component for achieving an N-level heat resistance rating. The epoxy groups in the alicyclic modified epoxy resin are directly linked to the alicyclic rings, forming a tight, rigid cross-linked network after curing together with the multifunctional structure of the phenolic epoxy resin. This network exhibits high cross-linking density and a high heat distortion temperature (Martin heat resistance ≥190°C). The absence of this network significantly reduces the cross-linking density and consequently lowers the heat resistance. Simultaneously, the rigidity of the alicyclic structure imparts low thermal expansion to the adhesive layer; its absence leads to an increase in CTE to 44.8 × 10⁻⁶. -6 ℃ -1 This further proves that the alicyclic structure is an important source of low thermal expansion.
[0109] While Comparative Example 8 (single alicyclic epoxy) exhibited excellent heat resistance (Tg = 232°C, Grade H), its peel strength was only 0.06 N / mm, significantly lower than Example 1. This demonstrates that CTBN flexible segment modified epoxy resin is a key component ensuring flexibility and impact resistance. During curing, CTBN forms a micro-phase separation island structure, with rubber particles acting as stress concentration points, inducing shear bands and crazing, effectively absorbing impact energy. Without this structure, the adhesive layer becomes brittle, failing to meet the processing and usage requirements of multilayer tape lamination. Simultaneously, the slightly lower thermal conductivity of the single alicyclic epoxy indicates that the introduction of flexible epoxy helps improve filler dispersion.
[0110] The properties of Comparative Example 9 (ordinary E-51 replacing flexible modified epoxy) were significantly lower than those of Example 1, with a Tg of only 178°C (F grade) and a CTE as high as 58.6 × 10⁻⁶. -6 ℃ -1 (Approaching the intrinsic value of pure epoxy), proving that epoxy-flexible segment modified bisphenol A type epoxy resin is not merely a simple physical blend of ordinary epoxy and CTBN. The chemical reaction between CTBN and bisphenol A type epoxy resin (ring-opening esterification reaction of carboxyl and epoxy groups) is the prerequisite for its excellent properties. Ordinary E-51 does not contain CTBN modified segments and cannot form a block copolymer structure. It lacks both the toughening effect of flexible segments and the ability to form an optimized ternary crosslinking network structure with phenolic epoxy resin and alicyclic epoxy resin. As a result, even with DDS curing agent, the Tg cannot be increased to above 200, and the heat resistance, low thermal expansion, and adhesion properties are all reduced. At the same time, the chemical bonding structure introduced by reactive CTBN modification also makes a positive contribution to filler dispersion and interfacial bonding.
[0111] Comparative Example 10 (phenolic epoxy resin only) exhibits a glass transition temperature as high as 220°C, a heat resistance rating of N, and a thermogravimetric temperature of 403°C, all superior to Example 1. However, its floating roll peel strength is only 0.05 N / mm, and its average T-peel force is only 0.9 N, far lower than Example 1. This demonstrates that although phenolic epoxy resin possesses excellent multifunctional rigid structure and heat resistance, its high crosslinking density and extreme brittleness when used alone result in extremely low peel strength, failing to meet the interlayer adhesion strength requirements of multilayer amorphous ribbon lamination composites. This also proves the necessity of this invention to perform a ternary compounding of phenolic epoxy resin with flexible segment-modified epoxy and alicyclic epoxy.
[0112] The results of Comparative Examples 7-10 fully demonstrate the importance of the rigid-flexible design of the composite modified epoxy resin matrix of this invention: the alicyclic modified epoxy resin and the phenolic epoxy resin together provide a high crosslinking density rigid network, giving the adhesive layer N-grade heat resistance and low thermal expansion characteristics; the epoxy-flexible segment modified bisphenol A type epoxy resin, through the CTBN chemical reaction, introduces flexible segments that provide toughness and impact resistance. The three are compounded in a specific ratio to achieve a balance between high heat resistance and high adhesive strength. The single flexible epoxy (Comparative Example 7) has insufficient heat resistance, only reaching F-grade; the single alicyclic epoxy (Comparative Example 8) is too brittle and has extremely low peel strength; the single phenolic epoxy resin (Comparative Example 10), although having excellent heat resistance, has a peel strength of only 0.05 N / mm, which cannot meet the adhesive requirements of laminated composites; the ordinary E-51 + alicyclic epoxy compound (Comparative Example 9), due to the lack of CTBN chemical modification, has a Tg of only 178℃, which also cannot meet the N-grade heat resistance requirements. Only by blending epoxy-flexible segment modified bisphenol A type epoxy resin, alicyclic modified epoxy resin and phenolic epoxy resin in a specific ratio can a synergistic balance between N-grade high heat resistance and excellent flexibility be achieved, with comprehensive performance superior to any single resin system or ordinary epoxy compound system.
[0113] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details of the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solutions of the present invention, and these simple modifications all fall within the protection scope of the present invention. Furthermore, it should be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not further describe the various possible combinations.
[0114] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.
Claims
1. A high-heat-resistant, low-thermal-expansion amorphous alloy strip composite adhesive, characterized in that, The product comprises, by weight parts: 67-83 parts of composite modified epoxy resin matrix, 5-18 parts of composite filler, 15-25 parts of heat-resistant curing agent, 1-4 parts of curing accelerator, 0.1-0.4 parts of interface modifier, 2-10 parts of reactive diluent, and 0.5-1.5 parts of antioxidant. The composite modified epoxy resin matrix comprises epoxy-flexible segment modified bisphenol A type epoxy resin, phenolic epoxy resin and alicyclic modified epoxy resin in a mass ratio of (32-38):(10-15):(25-30). The surface of the composite filler has active hydroxyl groups, including negative thermal expansion filler, insulating reinforcement filler and thermally conductive-insulating bifunctional filler with a mass ratio of (2-8):(2-6):(1-4); The interface modifier is γ-glycidyl etheroxypropyltrimethoxysilane.
2. The high heat-resistant, low thermal expansion amorphous alloy strip composite adhesive according to claim 1, characterized in that, The negative thermal expansion filler is nano-zirconium tungstate with an average particle size of 50-200 nm and a negative thermal expansion coefficient of -8.0 × 10⁻⁶. -6 ~-10.0×10 -6 ℃ -1 .
3. The high heat-resistant, low thermal expansion amorphous alloy strip composite adhesive according to claim 1, characterized in that, The insulating reinforcing filler is nano-silica with a specific surface area of 150-300 m². 2 / g.
4. The high heat-resistant, low thermal expansion amorphous alloy strip composite adhesive according to claim 1, characterized in that, The thermally conductive and insulating bifunctional filler is hydroxylated hexagonal boron nitride nanosheets, and the average sheet diameter of the hexagonal boron nitride is 100-500 nm.
5. The high heat-resistant, low thermal expansion amorphous alloy strip composite adhesive according to claim 1, characterized in that, The epoxy-flexible segment modified bisphenol A epoxy resin is prepared by modifying bisphenol A epoxy resin with carboxyl-terminated butadiene-acrylonitrile rubber, wherein the amount of carboxyl-terminated butadiene-acrylonitrile rubber added is 5-15% of the mass of bisphenol A epoxy resin.
6. The high heat-resistant, low thermal expansion amorphous alloy strip composite adhesive according to claim 1, characterized in that, The alicyclic modified epoxy resin is 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester and / or bis((3,4-epoxycyclohexyl)methyl) adipate.
7. The high heat-resistant, low thermal expansion amorphous alloy strip composite adhesive according to claim 1, characterized in that, The heat-resistant curing agent is 4,4'-diaminodiphenyl sulfone and / or nadic anhydride.
8. A method for preparing a high heat-resistant, low thermal expansion amorphous alloy strip composite adhesive as described in any one of claims 1-7, characterized in that, Includes the following steps: (1) The negative thermal expansion filler, the insulating reinforcement filler and the thermally conductive-insulating bifunctional filler were modified with γ-glycidyl etheroxypropyltrimethoxysilane to obtain the modified composite filler. (2) Epoxy-flexible segment modified bisphenol A type epoxy resin, phenolic epoxy resin and alicyclic modified epoxy resin and antioxidant are mixed evenly, and an active diluent is added. After mixing, a composite modified epoxy resin matrix mixture is obtained. (3) The modified composite filler is mixed with the composite modified epoxy resin matrix mixture, dispersed and ground to obtain a resin mixture in which the filler is uniformly dispersed; (4) Add the heat-resistant curing agent and curing accelerator to the resin mixture, stir, degas under vacuum and filter to obtain the composite adhesive.
9. The preparation method of the high heat-resistant, low thermal expansion amorphous alloy strip composite adhesive according to claim 8, characterized in that, In step (3), the dispersion and grinding include: Disperse at high speed for 60-120 minutes at 60-80℃ and 800-1500rpm, then use a three-roll mill for assisted dispersion, grinding 2-4 times with a grinding gap of 10-50μm, and the temperature ≤60℃ during the grinding process.
10. The preparation method of the high heat-resistant, low thermal expansion amorphous alloy strip composite adhesive according to claim 8, characterized in that, In step (1), the negative thermal expansion filler, the insulating reinforcing filler, and the thermally conductive-insulating bifunctional filler are modified with γ-glycidyl etheroxypropyltrimethoxysilane to obtain a modified composite filler, including: The negative thermal expansion filler, the insulating reinforcement filler, and the thermally conductive-insulating bifunctional filler were vacuum dried separately. A modified solution was prepared by dissolving γ-glycidyl etheroxypropyltrimethoxysilane in a mixed solvent of ethanol and water. The dried fillers were added to the modification liquid, stirred and ultrasonically dispersed for surface modification, and then vacuum dried to obtain modified negative thermal expansion fillers, modified insulating and reinforcing fillers, and modified thermally conductive and insulating bifunctional fillers. The three modified fillers were then mixed evenly to obtain modified composite fillers.
Citation Information
Patent Citations
Adhesive for amorphous strip and preparation method thereof
CN121343525A
Gradient curing and bonding aromatic polyamide amorphous strip adhesive as well as preparation method and application thereof
CN122104140A