High-adhesion potting adhesive for multi-material interface of smart ring and preparation method thereof

By combining silane coupling agents with multi-coordinated titanate coupling agents, the problems of low bonding strength and insufficient electrical safety at the interface of multiple materials in smart rings are solved, achieving improved bonding strength, resistance to damp heat and humidity, and electrical safety, and making it suitable for automated potting processes of smart rings.

CN123131965APending Publication Date: 2026-11-20GUANGDONG JIUZHI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611324685.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-20

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The application discloses a high-adhesion potting adhesive for adapting to a multi-material interface of a smart ring and a preparation method thereof, and belongs to the technical field of electronic packaging epoxy potting adhesives. The potting adhesive is composed of A and B components which are independently packaged, and the A and B components are mixed according to a weight ratio of (2-4):1 during use. The A component contains 70-100 parts of epoxy resin, 1-30 parts of active diluent and 1-5 parts of a compounded coupling agent. The B component contains 60-90 parts of an amine curing agent, 1-10 parts of a toughening agent, 1-10 parts of a reaction promoter and 1-10 parts of an auxiliary agent. The compounded coupling agent is formed by directional compounding of a silane coupling agent and a multi-ligand titanate coupling agent according to a weight ratio of (1-3):(0.5-2), and the proportion of the titanate is lower than that of the silane. The application can simultaneously improve the adhesion performance of a titanium alloy metal interface and a PCBA organic interface by relying on the synergistic coordination of the two types of coupling agents, and meanwhile, the application has low process viscosity, excellent moisture and heat resistance, high electrical safety and good storage stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of epoxy potting compound technology for electronic packaging, specifically to a high-adhesion potting compound adapted to the multi-material interface of smart rings and its preparation method. Background Technology

[0002] As a mainstream miniaturized wearable electronic device, the smart ring consists of a titanium alloy shell, an internal PCB circuit board, and surface-mount / microelectronic components. The manufacturing process requires the use of epoxy potting compound to complete structural bonding, cavity filling, electrical insulation, and component protection.

[0003] Currently, conventional epoxy potting compounds and modification solutions in the industry suffer from the following technical defects: Insufficient adhesion to multiple material interfaces: A dense, chemically inert titanium dioxide oxide layer forms on the surface of titanium alloys. Ordinary epoxy adhesives rely solely on physical wetting, making it difficult to achieve high-strength bonding. Long-term use can easily lead to interface delamination, delamination, and interface delamination failure. Single silane coupling agents have weak effects on modifying metal oxide interfaces, and single titanate coupling agents have poor compatibility with PCBA (Printed Circuit Board Assembly) and component packaging materials, making it impossible to simultaneously support both metal and organic substrates.

[0004] Insufficient adaptability of adhesive flow: The internal cavity of the smart ring is small and the structure is complex. Some modified epoxy adhesives have a high viscosity and cannot fully fill the tiny gaps, which can easily lead to defects such as incomplete filling and internal voids.

[0005] Existing compounding technologies have shortcomings: Some existing patents disclose schemes for compounding silane coupling agents and titanate coupling agents in epoxy resins, but most of them use ordinary monoalkoxy titanates, which have a fast hydrolysis rate and are prone to transesterification reactions that cause thickening and gelation of the adhesive. Moreover, they have not optimized the formula for the specific working conditions of smart ring titanium alloy + PCBA + micro components, and there is no clear ratio and performance data to support them, making it difficult to directly mass-produce and apply them.

[0006] Therefore, the market urgently needs a special epoxy potting compound that is low in viscosity, high in adhesion, hydrolysis resistant, electrically safe, and can be adapted to multiple material interfaces such as titanium alloys, PCBAs, and micro-components. Summary of the Invention

[0007] In view of this, the purpose of this invention is to provide a high-adhesion potting compound adapted to the multi-material interface of smart rings and its preparation method. It can effectively overcome the defects of existing epoxy potting compounds, such as low bonding strength at multi-material interfaces, easy hydrolysis and thickening, and poor filling performance in narrow cavities. It can simultaneously improve the bonding performance between the titanium alloy metal interface and the PCBA organic interface, while also having low process viscosity, excellent resistance to damp heat, high electrical safety and good storage stability. It is perfectly adapted to the automated potting conditions and long-term wear requirements of the narrow cavity of smart rings.

[0008] In a first aspect, the present invention provides a highly adhesive potting compound that is compatible with multiple material interfaces of smart rings, comprising separately packaged components A and B, which are mixed and cured in proportion before use.

[0009] Component A comprises the following raw materials in parts by weight: 70-100 parts epoxy resin, 1-30 parts reactive diluent, and 1-5 parts complex coupling agent; The compound coupling agent is composed of a silane coupling agent and a multi-coordinate titanate coupling agent in a weight ratio of (1-3):(0.5-2), and the weight fraction of the multi-coordinate titanate coupling agent is less than the weight fraction of the silane coupling agent.

[0010] Component B comprises the following raw materials in parts by weight: 60-90 parts of amine curing agent, 1-10 parts of toughening agent, 1-10 parts of reaction accelerator, and 1-10 parts of additives.

[0011] The weight ratio of component A to component B is (2-4):1, preferably 3:1.

[0012] The complex coupling agent is the core functional component of the formulation. The silane coupling agent is responsible for bonding the organic interface of PCBA and micro-components, while the multi-coordinated titanate is responsible for bonding the metal outer ring interface. By controlling the proportion of multi-coordinated titanate to be lower than that of silane coupling agent, problems such as interface peeling, poor hydrolysis resistance, and increased adhesive viscosity can be avoided.

[0013] Optionally, the epoxy resin is selected from one or more combinations of bisphenol A type epoxy resins E-54, E-51, and E-44, and bisphenol F type epoxy resins E-51F, E-44F, and E-20F.

[0014] Optionally, the active diluent is selected from one or more combinations of phenyl glycidyl ether, allyl glycidyl ether, p-methyl phenyl glycidyl ether, p-isobutyl phenyl glycidyl ether, turpentine, dibutyl phthalate, and dioctyl phthalate.

[0015] Optionally, the silane coupling agent is selected from one of 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, phenyltrimethoxysilane, diphenyldiethoxysilane, and diphenyldimethoxysilane. The multi-coordinate titanate coupling agent is selected from one of bis(acetylacetonyl)ethoxyisopropoxy titanate, bis(acetylacetonyl)diisopropyl titanate, tetraisopropyl bis(dioctylphosphite)titanate, and neoalkoxytris(p-aminophenoxy)titanate.

[0016] Optionally, the amine curing agent is selected from one or more combinations of polyetheramines D230, D400, D2000, T403, T5000, and diethyltoluene diamine.

[0017] The toughening agent is selected from one or more combinations of CTBN-terminated carboxyl-terminated butadiene-acrylonitrile rubber, ATBN-terminated amino-terminated butadiene-acrylonitrile rubber, epoxy polyether flexible toughening agent, acrylic core-shell microspheres, and liquid polysulfide rubber.

[0018] The reaction promoter is selected from one or more combinations of DMP-30 (2,4,6-tris(dimethylaminomethyl)phenol (abbreviated as DMP-30)), benzyldimethylamine, and 2-ethyl-4-methylimidazole.

[0019] The additives are selected from one or more combinations of silicone-modified defoamers, polyether leveling agents, and fluorinated transparent defoamers.

[0020] Secondly, the present invention provides a method for preparing the above-mentioned highly adhesive potting compound adapted to the multi-material interface of smart rings, comprising the following steps: Preparation of Component A: Epoxy resin, reactive diluent, and complex coupling agent are mixed evenly in parts by weight to obtain Component A; the complex coupling agent is added after premixing silane coupling agent and multi-coordinate titanate coupling agent in a certain proportion. Preparation of Component B: The amine curing agent, toughening agent, reaction accelerator, and additives are mixed evenly in parts by weight to obtain Component B; Before use, the A component and the B component are mixed at a weight ratio of (2-4):1, and then subjected to vacuum degassing treatment to obtain the high-adhesion potting compound.

[0021] Optionally, when preparing component A, the stirring speed is 800-1200 r / min and the stirring time is 3-10 min; when preparing component B, the stirring speed is 600-1000 r / min and the stirring time is 3-10 min.

[0022] The technical solution provided by this invention includes, but is not limited to, the following beneficial effects: Compared with existing technologies, this invention has the following technical advantages: Significantly improved multi-material bonding capability: The epoxy silane coupling agent and multi-coordinate titanate compound system are used to act on the organic interface of PCBA and the metal interface of titanium alloy respectively to form a continuous molecular bridge. The bonding strength is significantly better than that of a single coupling agent and a blank system, which completely solves the problem of multi-material debonding and delamination in smart rings.

[0023] High electrical safety: The compounded coupling agent has low volatility, is non-corrosive, and does not release conductive ions. Its volume resistivity meets electronic packaging standards and will not corrode PCBA circuits or micro-components.

[0024] High process adaptability: The adhesive has low overall viscosity, good fluidity and leveling properties, making it suitable for precision encapsulation of micro-cavities in smart rings; the preparation process is simple, requiring only stirring and mixing, making it suitable for automated production lines.

[0025] Good formulation stability: The compound system has good compatibility with epoxy resin and modified amine curing agent, and there is no layering, thickening or gelation during storage, resulting in a long shelf life. Detailed Implementation

[0026] The present invention will be further described in detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited to the content described.

[0027] In the following examples and comparative examples, all "parts" refer to parts by weight; components A and B were mixed at a weight ratio of 3:1 before performance testing.

[0028] I. Test Methods and Reference Standards Mixed viscosity: The viscosity after mixing was tested using a viscometer, reference standard: GB / T 2794-2013; Initial shear strength: The adhesive strength was tested using a universal tensile testing machine, the test substrate was a PCBA ink-coated substrate + titanium alloy, reference standard: ASTM D1002; Shear strength after damp heat aging: The adhesive strength was tested using a universal tensile testing machine after being placed in an environment of 55℃ / 95%RH for 14 days, the test substrate was a PCBA ink-coated substrate + titanium alloy, reference standard: ASTM D1002; All shear strengths in this document in megapascals (including strength after damp heat aging) are absolute strength values, and the shear strength reduction rate is a relative attenuation index, calculated and listed separately.

[0029] Volume resistivity: A circular film with a diameter greater than 50 mm is made using a mold and tested using a volume resistivity tester. Reference standard: ASTM D257.

[0030] II. General Preparation Method The following general preparation steps are used in all embodiments and comparative examples of this invention: Preparation of Component A: Weigh each raw material of Component A according to the weight parts and put them into a container. After the compounding agent is pre-mixed evenly according to the corresponding ratio, it is added to the mixture of epoxy resin and reactive diluent. The mixture is placed in a homogenizer and stirred at 1000 r / min for 5 min. After mixing evenly, Component A is obtained. Preparation of component B: Weigh each raw material of component B according to the weight parts and put them into a container. Place the container into a homogenizer and stir at 800 r / min for 5 min. After mixing evenly, component B is obtained. When using, components A and B are mixed in a 3:1 weight ratio, and after vacuum degassing, performance testing is performed.

[0031] Process description: The compound coupler should be mixed evenly in the corresponding proportion before being added to the A component system; the A and B components are not degassed after being prepared separately, but are vacuum degassed after being mixed in proportion before use.

[0032] III. Examples Example 1 The high-adhesion potting compound adapted for multi-material interfaces in this embodiment consists of separately packaged component A and component B: Component A (by weight): 88 parts of bisphenol F type epoxy resin (epoxy equivalent of 185 g / eq), 10 parts of p-isobutylphenyl glycidyl ether (BPGE), and 2 parts of complex coupling agent; wherein the silane coupling agent in the complex coupling agent is 3-glycidyl etheroxypropyltriethoxysilane (epoxysilane coupling agent), and the titanate coupling agent is tetraisopropyl di(dioctylphosphite) titanate (multi-coordinate titanate), and the weight ratio of the two is 1:2.

[0033] This embodiment employs a dual-function coupling agent design: a silane coupling agent primarily acts on the interface between the organic substrate of the PCBA and micro-components, enhancing the adhesion between the adhesive layer and the organic material; a multi-coordinated titanate coupling agent primarily acts on the interface of the titanium alloy outer ring, strengthening the bond between the adhesive layer and the metal oxide layer. By controlling the proportion of the multi-coordinated titanate coupling agent in the formulation to be lower than that of the silane coupling agent, problems such as interfacial delamination, decreased hydrolysis resistance, and increased adhesive viscosity caused by excessive titanate are avoided, achieving synergistic optimization of the adhesion performance of multiple material interfaces.

[0034] Component B (by weight): 90 parts polyetheramine (molecular weight 230, i.e., polyetheramine D230), 5 parts ATBN-terminated aminobutadiene nitrile rubber, 4 parts 2,4,6-tris(dimethylaminomethyl)phenol (DMP-30), and 1 part silicone-modified defoamer.

[0035] The preparation method adopts the general preparation method described above.

[0036] Example 2 This embodiment is basically the same as Example 1, except that the weight ratio of silane coupling agent to multi-coordinate titanate coupling agent in the complex coupling agent is 1:1. The remaining components, dosages, and preparation methods are the same as in Example 1.

[0037] Example 3 This embodiment is basically the same as Example 1, except that the weight ratio of silane coupling agent to multi-coordinate titanate coupling agent in the complex coupling agent is 2:1. The remaining components, dosages, and preparation methods are the same as in Example 1.

[0038] Example 4 This embodiment is basically the same as Example 1, except that the weight ratio of silane coupling agent to multi-coordinate titanate coupling agent in the complex coupling agent is 3:1. The remaining components, dosages, and preparation methods are the same as in Example 1.

[0039] Example 5 This embodiment is basically the same as Example 1, except that the weight ratio of silane coupling agent to multi-coordinate titanate coupling agent in the complex coupling agent is 2:0.5. The remaining components, dosages, and preparation methods are the same as in Example 1.

[0040] IV. Comparative Examples Comparative Example 1 (Blank Control Group) This comparative example is basically the same as Example 1, except that no complex coupling agent is added to component A. That is, component A consists of 89 parts of bisphenol F epoxy resin and 11 parts of p-isobutylphenyl glycidyl ether. Component B and its preparation method are the same as in Example 1.

[0041] Comparative Example 2 (Single silane coupling agent group) This comparative example is basically the same as Example 1, except that: only a single silane coupling agent is added to component A, and no titanate coupling agent is added. The total weight parts of the coupling agent are 2 parts, namely 2 parts of 3-glycidyl etheroxypropyltriethoxysilane. Component B and its preparation method are the same as in Example 1.

[0042] Comparative Example 3 (single titanate coupling agent group) This comparative example is basically the same as Example 1, except that: only a single multi-coordinate titanate coupling agent is added to component A, and no silane coupling agent is added. The total weight parts of the coupling agent are 2 parts, namely 2 parts of tetraisopropyl di(dioctylphosphite)titanate. Component B and its preparation method are the same as in Example 1.

[0043] V. Performance Test Results The samples from Examples 1-5 and Comparative Examples 1-3 were subjected to performance tests according to a unified testing standard. The test results are shown in the table below:

[0044] Based on the data in the table above, the impact of the compounding ratio on each performance item is analyzed as follows: 1. Effect of compounding ratio on mixed viscosity As the proportion of multi-coordinated titanate in the composite coupling agent increases, the overall viscosity of the mixed adhesive shows a significant upward trend. Example 5 (silane: titanate = 2:0.5) exhibits the lowest viscosity, at 305 mPa. s; Example 1 (silane: titanate = 1:2) viscosity increased to 526 mPa Comparative Example 3, with only a single titanate added, had a viscosity as high as 643 mPa. s.

[0045] Based on the analysis of the formulation design logic, titanate molecules tend to form partial coordination associations with epoxy resin. Excessive titanate will increase the cohesive force of the system, leading to increased viscosity. High viscosity reduces the self-leveling and capillary penetration capabilities of the adhesive, hindering the filling of the tiny gaps in the narrow cavities of the smart ring and easily causing defects such as voids and insufficient adhesive.

[0046] 2. Effect of compounding ratio on initial shear strength Overall, as the proportion of silane coupling agent increases, the initial shear strength shows a gradual upward trend; under the premise of reasonable ratio, the compound system can achieve a synergistic bonding effect that is better than that of a single coupling agent.

[0047] The initial shear strength of the blank control group was only 10.3 MPa, indicating that without coupling agent, physical wetting alone cannot form a high-strength interfacial bond; the single silane group was 18.6 MPa and the single titanate group was 16.5 MPa, indicating that a single coupling agent can only enhance the interfacial bond of the corresponding single material.

[0048] When the proportion of titanate is too high (Examples 1 and 2), the initial bond strength is lower than that of the single silane group. This is because excessive titanate will crowd out the binding sites of the silane coupling agent at the organic substrate interface, thus weakening the interfacial bonding force on the PCBA side. When the ratio of silane to titanate is adjusted to 2:1 (Example 3), the initial shear strength can reach 20.1 MPa, which is 95% higher than the blank group and 8.1% and 21.8% higher than the two types of single coupling agents, respectively. The two types of coupling agents work together: the silane coupling agent acts on the organic interface of PCBA and micro-components, and the multi-coordinated titanate acts on the titanium alloy metal interface, together forming a continuous bonding structure between heterogeneous interfaces, achieving a synergistic improvement in bond strength.

[0049] When the proportion of silane continues to increase to 3:1 or 2:0.5, the improvement in initial strength narrows, remaining only at 21.0–21.2 MPa, and the improvement in adhesive performance is close to saturation.

[0050] 3. Effect of compounding ratio on resistance to damp heat The strength retention rate after damp heat aging decreased significantly with the decrease of the proportion of multi-coordinated titanate, that is, the higher the proportion of silane, the more severe the strength degradation after damp heat aging.

[0051] The shear strength reduction rate of Examples 1 to 3 was less than 5.1%, and the strength retention rate was over 94.9%. When the proportion of silane was further increased (Examples 4 and 5), the reduction rate increased to 9.05% to 10.85%, and the damp heat resistance performance showed a significant decline.

[0052] The reason is that multi-coordinated titanates have a chelating steric hindrance structure, which can effectively inhibit hydrolysis reaction and improve the moisture and heat resistance of the interfacial bonding. However, when the proportion of silane coupling agent is too high, the Si-OC bond in its molecule is prone to hydrolysis and breakage under high temperature and high humidity environment, resulting in the destruction of the interfacial bonding network and rapid decay of the bonding strength.

[0053] Compared with the single silane group (11.29%) and the single titanate group (7.88%), the optimal compound group (2:1) has better damp heat resistance than the two single coupling agent systems.

[0054] 4. Effect of compounding ratio on volume resistivity The volume resistivity of all embodiments and comparative examples is within 2.0 × 10¹. 4 ~2.4×10¹ 4 Ω Within the cm range, there were no significant differences among the groups, all of which were far higher than the insulation safety requirements for wearable electronic devices.

[0055] The results indicate that the composite system of silane and multi-coordinate titanate does not introduce free conductive ions and does not negatively affect the electrical insulation performance of the potting compound, thus ensuring the long-term electrical safety of the internal circuitry and micro-components of the smart ring.

[0056] 5. Demonstration of the optimal ratio for comprehensive performance Considering all four performance aspects, Example 3, with a silane:titanate ratio of 2:1, represents the optimal ratio for overall performance, achieving the best balance between bond strength, resistance to damp heat, process compatibility, and electrical safety. The reasons are as follows: Excellent bonding performance: The initial shear strength reaches 20.1MPa, which is 95% higher than the blank group, with significant synergistic effect, which can fully meet the high-strength bonding requirements of titanium alloy-PCBA multi-material interface; It exhibits the best performance in resisting damp heat: the strength reduction rate after damp heat aging is only 4.48%, and the retention rate reaches 95.5%, which can adapt to the wearing environment of smart rings that are in long-term contact with sweat and fluctuating temperature and humidity, ensuring the long-term reliability of the product. The process viscosity is moderate: the mixed viscosity is 358 mPa. s, which has both good fluidity and capillary filling properties, can fully penetrate the tiny gaps in the narrow cavity of the smart ring, and is suitable for automated potting process and vacuum degassing process; Electrical performance meets standards: volume resistivity is 2.4 × 10¹ 4 Ω cm, meeting the insulation safety standards for wearable electronic devices, with no risk of ion precipitation corrosion.

[0057] Other formulations all have significant performance drawbacks: when the proportion of titanate is too high (1:2, 1:1), the viscosity of the adhesive is too high, the self-leveling filling ability of the cavity decreases, and the initial bond strength does not reach the optimal level; when the proportion of silane is too high (3:1, 2:0.5), the resistance to damp heat decreases significantly, and the reliability for long-term use is insufficient. Therefore, a 2:1 formulation is the optimal compounding ratio of this invention.

[0058] VI. Formulation Conclusion This invention, through the directional compounding of silane coupling agents and multi-coordinate titanate coupling agents, can simultaneously improve the adhesion performance between the titanium alloy metal interface and the PCBA organic interface, while also taking into account damp heat stability, process flowability, and electrical safety. The overall conclusion is as follows: 1. The compound system with reasonable proportions has a significant synergistic bonding effect. The initial shear strength is 95% higher than that of the blank group and 8%~22% higher than that of the single coupling agent system. It can effectively solve the industry pain point of debonding and delamination at the interface of multiple materials in smart rings. 2. The chelated steric structure of multi-coordinate titanate can significantly inhibit hydrolysis reaction. Under the optimal ratio, the strength retention rate can reach more than 95% after 14 days of wet heat aging, which is far superior to the blank system and the single coupling agent system, and is suitable for the temperature and humidity alternating environment of long-term wear of smart rings. 3. The ratio of silane to titanate needs to balance the bonding strength, resistance to damp heat and the process viscosity. The ratio of silane to titanate of 2:1 is the optimal ratio for comprehensive performance, which can simultaneously meet the requirements of multiple working conditions such as high adhesion, hydrolysis resistance and low viscosity. 4. No free conductive ions are released in the entire compound system. After curing, the volume resistivity meets the insulation safety standards for wearable electronic devices and there is no risk of corroding PCBA microcircuits and micro-components.

[0059] The above specific embodiments are merely explanations of the present invention and are not intended to limit the present invention. After reading this specification, those skilled in the art can make modifications to the present invention without contributing any inventive step, but all such modifications should be covered within the protection scope of the present invention.

Claims

1. A high-adhesion potting compound suitable for multi-material interfaces of smart rings, characterized in that, Includes separately packaged components A and B; Component A comprises the following raw materials in parts by weight: 70-100 parts epoxy resin, 1-30 parts reactive diluent, and 1-5 parts complex coupling agent; The compound coupling agent is composed of a silane coupling agent and a multi-coordinate titanate coupling agent in a weight ratio of (1-3):(0.5-2), and the weight fraction of the multi-coordinate titanate coupling agent is less than the weight fraction of the silane coupling agent. Component B comprises the following raw materials in parts by weight: 60-90 parts of amine curing agent, 1-10 parts of toughening agent, 1-10 parts of reaction accelerator, and 1-10 parts of additives; The weight ratio of component A to component B is (2-4):

1.

2. The potting compound according to claim 1, characterized in that, The epoxy resin is selected from one or more combinations of bisphenol A type epoxy resins E-54, E-51, E-44 and bisphenol F type epoxy resins E-51F, E-44F, E-20F; The active diluent is selected from one or more combinations of phenyl glycidyl ether, 4-allyl glycidyl ether, p-methyl phenyl glycidyl ether, p-isobutyl phenyl glycidyl ether, turpentine, dibutyl phthalate, and dioctyl phthalate.

3. The potting compound according to claim 1, characterized in that, The silane coupling agent is selected from one of 3-glycidyl etheroxypropyltriethoxysilane, 3-glycidyl etheroxypropyltrimethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, phenyltrimethoxysilane, diphenyldiethoxysilane, and diphenyldimethoxysilane. The multi-coordinate titanate coupling agent is selected from one of bis(acetylacetonyl)ethoxyisopropoxy titanate, bis(acetylacetonyl)diisopropyl titanate, tetraisopropyl bis(dioctylphosphite)titanate, and neoalkoxytris(p-aminophenoxy)titanate.

4. The potting compound according to claim 1, characterized in that, The amine curing agent is selected from one or more combinations of polyetheramines D230, D400, D2000, T403, T5000, and diethyltoluene diamine; the toughening agent is selected from one or more combinations of CTBN-terminated carboxyl-terminated butadiene-acrylonitrile rubber, ATBN-terminated amino-terminated butadiene-acrylonitrile rubber, epoxy polyether flexible toughening agent, acrylic core-shell microspheres, and liquid polysulfide rubber. The reaction promoter is selected from one or more combinations of DMP-30, benzyldimethylamine, and 2-ethyl-4-methylimidazole; The additives are selected from one or more combinations of silicone-modified defoamers, polyether leveling agents, and fluorinated transparent defoamers.

5. The potting compound according to claim 1, characterized in that, The weight ratio of component A to component B is 3:

1.

6. A method for preparing a highly adhesive potting compound for multi-material interfaces of a smart ring as described in any one of claims 1 to 5, characterized in that, Includes the following steps: Preparation of Component A: By weight, 70-100 parts of epoxy resin, 1-30 parts of reactive diluent, and 1-5 parts of complex coupling agent are mixed evenly to obtain Component A; the complex coupling agent is composed of silane coupling agent and multi-coordinate titanate coupling agent in a weight ratio of (1-3):(0.5-2), and the weight of the multi-coordinate titanate coupling agent is less than the weight of the silane coupling agent; Preparation of component B: Mix 60-90 parts of amine curing agent, 1-10 parts of toughening agent, 1-10 parts of reaction accelerator and 1-10 parts of additive evenly to obtain component B; The high-adhesion potting compound is obtained by mixing component A and component B at a weight ratio of (2-4):1 and then performing vacuum degassing treatment.

7. The preparation method according to claim 6, characterized in that, The epoxy resin is selected from one or more combinations of bisphenol A type epoxy resins E-54, E-51, E-44 and bisphenol F type epoxy resins E-51F, E-44F, E-20F; The active diluent is selected from one or more combinations of phenyl glycidyl ether, allyl glycidyl ether, p-methyl phenyl glycidyl ether, p-isobutyl phenyl glycidyl ether, turpentine, dibutyl phthalate, and dioctyl phthalate.

8. The preparation method according to claim 6, characterized in that, The silane coupling agent is selected from one of 3-glycidyl etheroxypropyltriethoxysilane, 3-glycidyl etheroxypropyltrimethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, phenyltrimethoxysilane, diphenyldiethoxysilane, and diphenyldimethoxysilane. The multi-coordinate titanate coupling agent is selected from one of bis(acetylacetonyl)ethoxyisopropoxy titanate, bis(acetylacetonyl)diisopropyl titanate, tetraisopropyl bis(dioctylphosphite)titanate, and neoalkoxytris(p-aminophenoxy)titanate.

9. The preparation method according to claim 6, characterized in that, The amine curing agent is selected from one or more combinations of polyetheramines D230, D400, D2000, T403, T5000, and diethyltoluene diamine; The toughening agent is selected from one or more combinations of CTBN-terminated carboxyl butadiene nitrile rubber, ATBN-terminated amino butadiene nitrile rubber, epoxy polyether flexible toughening agent, acrylic core-shell microspheres, and liquid polysulfide rubber. The reaction promoter is selected from one or more combinations of DMP-30, benzyldimethylamine, and 2-ethyl-4-methylimidazole; The additives are selected from one or more combinations of silicone-modified defoamers, polyether leveling agents, and fluorinated transparent defoamers.

10. The preparation method according to claim 6, characterized in that, When preparing component A, the stirring speed is 800-1200 r / min and the stirring time is 3-10 min; When preparing component B, the stirring speed is 600-1000 r / min and the stirring time is 3-10 min.