High-toughness epoxy resin binder for steel bridge deck pavement and method for preparing the same

By improving the wetting and bonding stability of epoxy adhesives with modified toughening agents and composite amine curing agents, the problem of unstable bonding of steel bridge deck pavement in slightly humid or salty environments was solved, and a high-toughness and crack-resistant pavement layer was formed to adapt to complex service conditions.

CN123131968APending Publication Date: 2026-11-20WUHAN LUSHENG MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611650185.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-23
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing epoxy adhesives for steel bridge deck paving are unstable in slightly humid or salty environments, and are prone to interfacial debonding and corrosive debonding. Furthermore, their bond strength decreases under humid heat aging and vehicle loads.

Method used

By introducing a modified toughening agent containing carboxy-betaine groups and a composite amine curing agent, the wetting ability and interfacial bonding stability of the epoxy system are improved. Polyester fiber and steel fiber are used to reinforce the structure, forming a pavement layer with high toughness and crack resistance.

Benefits of technology

It improves the interfacial bonding stability and salt water erosion resistance of epoxy adhesives in slightly humid or salty environments, enhances the crack resistance and fatigue resistance of the pavement layer, and meets the usage requirements under complex service conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123131968A_ABST
    Figure CN123131968A_ABST
Patent Text Reader

Abstract

The application provides a high-toughness epoxy resin binder for steel bridge deck pavement and a preparation method thereof, and comprises the following raw materials in parts by mass: 100 parts of bisphenol A type epoxy resin, 8-12 parts of active diluent, 10-20 parts of modified toughening agent, 1-2.5 parts of polyester fiber, 25-45 parts of composite amine curing agent, 1-3 parts of accelerator and 800-1200 parts of filler; wherein the modified toughening agent comprises a polyether compound containing a carboxyl betaine group and an epoxy group; the composite amine curing agent is obtained by mixing polyether amine, cashew phenol amine epoxy curing agent and gamma-aminopropyl triethoxysilane at a mass ratio of 50:(20-40):(0.5-1.5); and the filler is obtained by mixing steel fibers and natural crushed stones at a mass ratio of 1:300-500, so that the obtained steel bridge deck pavement binder has high toughness, hot and humid durability, salt water erosion resistance and long-term service stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of epoxy resin technology, specifically to a high-toughness epoxy resin binder for steel bridge deck paving and its preparation method. Background Technology

[0002] Epoxy resin pavement binder is a two-component thermosetting composite material composed of epoxy resin as the main agent and curing agent as the crosslinking agent (often combined with modified asphalt or fillers). It is used in roads, bridge decks or heavy-duty pavements to play a role in bonding, waterproofing and structural reinforcement. After curing, it forms a high-strength, high-durability and deformation-resistant mesh structure.

[0003] Steel bridge deck pavement is subjected to complex environments such as vehicle loads, temperature changes, rainwater erosion, de-icing salt erosion, and bridge vibration over long periods. The interfacial bonding performance between the pavement layer and the steel bridge deck directly affects the durability and service life of the steel bridge deck pavement structure. Epoxy resin adhesives, due to their high bonding strength, mechanical strength, and chemical corrosion resistance, have been widely used in steel bridge deck pavement materials to improve the reliability of the bond between the pavement layer and the steel bridge deck. Existing epoxy adhesives for steel bridge deck pavement typically require the steel bridge deck and aggregate to be fully dry before construction. The steel bridge deck generally needs to undergo sandblasting to remove rust, cleaning, and drying before paving. However, in actual engineering projects, trace amounts of moisture may remain on the sandblasted rough surface of the steel bridge deck, the micropores in the oxide layer, the pores on the surface of the aggregate, and in the construction environment. During service, rainwater, humid and hot environments, and de-icing salt can also easily penetrate into the pavement interface, creating a slightly damp or salty interface between the steel bridge deck and the epoxy adhesive.

[0004] Ordinary epoxy adhesives are mostly hydrophobic, and while they can form high bond strength on dry steel plate surfaces, their wetting ability and interfacial water replacement capacity are insufficient for slightly damp steel bridge decks, micropores in oxide layers, and surfaces of water-containing mineral materials. When trace amounts of moisture or salt are present at the interface, epoxy adhesives cannot fully wet the rough surfaces of the steel plate and mineral materials, easily forming a weak boundary layer at the interface. This leads to unstable initial bonding and problems such as bond strength decay, interfacial debonding, and even corrosive debonding under humid heat aging, salt water corrosion, and repeated vehicle loads.

[0005] Therefore, how to ensure the mechanical properties of epoxy resin binders while avoiding unstable bonding of the binders at slightly moist / salt-containing interfaces remains a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0006] This application provides a high-toughness epoxy resin binder for steel bridge deck paving and its preparation method. The binder improves the wetting ability and toughness of the epoxy system on slightly wet steel bridge decks and mineral surfaces by using a modified toughening agent, and improves the interfacial bonding stability, water damage resistance and salt water erosion debonding ability of the material in slightly wet or salty environments by using a composite amine curing agent.

[0007] In a first aspect, this application provides a high-toughness epoxy resin binder for steel bridge deck paving, comprising the following raw materials in parts by weight: 100 parts bisphenol A type epoxy resin, 8-12 parts reactive diluent, 10-20 parts modified toughening agent, 1-2.5 parts polyester fiber, 25-45 parts composite amine curing agent, 1-3 parts accelerator, 800-1200 parts filler. The modified toughening agent includes a polyether compound containing carboxyl betaine groups and epoxy groups; The composite amine curing agent is obtained by mixing polyether amine, cashew phenol amine epoxy curing agent, and γ-aminopropyltriethoxysilane in a mass ratio of 50:(20-40):(0.5-1.5). The filler is obtained by mixing steel fibers and natural crushed stone at a mass ratio of 1:300-500.

[0008] According to this application, bisphenol A type epoxy resin is used as the main resin to provide the binder with bonding strength, cohesive strength, and chemical resistance. The reactive diluent is used to reduce the viscosity of the system, improve the workability of the mixed material, and enhance its wetting and encapsulation capabilities for steel bridge decks, natural gravel, and steel fibers. Polyester fibers can form a microfiber-reinforced structure in the adhesive system, improving the adhesive's anti-flow, crack resistance, and tensile deformation capabilities. The modified toughening agent contains carboxyl betaine groups and residual epoxy groups. On the one hand, it can participate in the curing reaction and integrate into the curing network through residual epoxy and hydroxyl groups, utilizing the flexible polyether segments to improve the toughness of the cured product. On the other hand, it can utilize the carboxyl betaine groups to improve the adhesive's wetting and adsorption capabilities on the slightly damp steel bridge deck oxide layer, rough surface micropores, and water-containing mineral surfaces. The composite amine curing agent is a compound of polyetheramine, cashew phenolamine epoxy curing agent, and γ-aminopropyltriethoxysilane. It is not solely used to cure the epoxy resin, but also works synergistically with the carboxybetaine-type modified toughening agent: the flexible polyether segments of the polyetheramine and the modified toughening agent enhance the deformation coordination of the cured network; the cashew phenolamine epoxy curing agent provides hydrophobic long chains to reduce the continuous penetration of moisture and salt ions into the highly polar zwitterionic region; and the γ-aminopropyltriethoxysilane enhances the interfacial coupling between the resin system and the oxide layer and mineral aggregate surface of the steel bridge deck. Accelerators are used to regulate the curing speed and early strength development. Natural crushed stone in the filler forms the mineral aggregate skeleton of the pavement layer, and steel fibers improve the crack resistance, tensile strength, and fatigue resistance of the pavement layer.

[0009] During the research process, this application found that existing epoxy binders for steel bridge deck paving typically require the steel bridge deck and aggregate to be fully dry. However, in actual construction and service, trace amounts of moisture and salt may exist on the sandblasted rough surface of the steel bridge deck, the micropores of the oxide layer, the surface of the aggregate, and in external environments such as rainwater and snow melting salt. Although ordinary bisphenol A type epoxy resin systems have high dry bond strength and structural strength, they are generally hydrophobic and lack sufficient wetting ability and interfacial water replacement capacity for slightly damp steel bridge decks, micropores of the oxide layer, and the surface of water-containing aggregates. This easily leads to the formation of a weak boundary layer at the steel plate interface or aggregate interface, resulting in unstable initial bonding. Under humid heat aging, salt water corrosion, and repeated vehicle loads, problems such as decreased interfacial bond strength, debonding, and even corrosive debonding may occur. At the same time, ordinary epoxy cured products have a high crosslinking density and are relatively brittle. Under the temperature deformation of the steel bridge deck, bridge vibration, and repeated vehicle loads, they are prone to cracking or fatigue damage due to insufficient deformation adaptability. To address the aforementioned issues of insufficient wetting and toughness at micro-wet interfaces, this application first introduces a polyether reaction product containing carboxyl betaine groups and possessing residual epoxy reactivity as a modified toughening agent. The hydroxyl and residual epoxy groups in this modified toughening agent enable it to participate in the curing reaction, integrating into the epoxy curing network as a reactive component, thus reducing its risk of free migration during service. The flexible polyether segments introduce deformable segments into the curing network, improving the adhesive's elongation at break, low-temperature deformation capability, and fatigue crack resistance. The carboxyl betaine groups possess strong polarity and hydration capabilities, improving the adhesive's wetting and adsorption capacity on the oxide layer, rough micropores, and water-containing mineral surfaces of micro-wet steel bridge decks. This transforms the interfacial moisture from a weak, free water boundary layer unfavorable to adhesion into a confined hydration layer, thereby improving initial bond stability and construction tolerance at micro-wet interfaces. Therefore, the modified toughening agent not only improves the toughness of epoxy systems but also addresses the problem of insufficient wetting in ordinary hydrophobic epoxy adhesives at micro-wet interfaces.

[0010] However, this application further discovers that while introducing a modified toughening agent containing carboxyl betaine groups alone can improve the wettability and toughness of the micro-wet interface, the strong polarity and hydration ability of the carboxyl betaine groups, when existing in a free or weakly constrained state in the epoxy network, may lead to an increased water absorption tendency of the system. In rainwater, snow melting salt, or salt spray environments, it may also increase the risk of water and salt ion migration within the adhesive and at the interface, affecting the adhesive's wet heat durability and resistance to salt water erosion and debonding. In other words, the modified toughening agent solves the problems of insufficient wettability and insufficient toughness at the micro-wet interface, but its highly polar structure may bring new problems such as increased water absorption, enhanced salt ion migration, and decreased long-term interface durability. To address the water absorption and ion migration problems that may arise after the introduction of carboxyl betaine-type modified toughening agents, this application further employs a composite amine curing agent composed of polyetheramine, cashew phenolamine epoxy curing agent, and γ-aminopropyltriethoxysilane. The polyether amine in this composite amine curing agent provides amine curing activity and flexible polyether segments, forming a good segmental compatibility with the flexible polyether segments of the modified toughening agent, which is beneficial to improving the toughness and deformation coordination of the cured network. The cashew phenol amine epoxy curing agent contains hydrophobic long chains and phenol amine structures, which can introduce hydrophobic shielding units into the epoxy curing network, reducing the continuous penetration of water and salt ions into the highly polar carboxylic acid betaine region and the steel plate interface region, while improving the system's adhesion adaptability to moist interfaces. The amino group in γ-aminopropyltriethoxysilane can participate in and promote the curing of the epoxy system. Its alkoxysilane structure can form silicon-oxygen bonds, condensations, or couplings with the hydroxylation sites on the surface of the steel bridge deck oxide layer and the mineral material after hydrolysis, thereby improving the interfacial bonding stability between the adhesive and the steel plate and the mineral material.

[0011] Therefore, the composite amine curing agent is not used merely as a regular amine curing agent, but rather to address the potential side effects of water absorption and salt ion migration caused by carboxybetaine-type modified toughening agents through a combination of regulation. On one hand, polyetheramine can form a flexible curing network with the modified toughening agent, allowing the modified toughening agent to stably integrate into the epoxy system and exert its toughening effect. On the other hand, the hydrophobic long chains provided by the cashew phenol amine epoxy curing agent can reduce long-term water absorption and salt water penetration, inhibiting the water migration channels that may be formed by the highly polar zwitterionic structure. At the same time, γ-aminopropyltriethoxysilane can enhance the interfacial coupling of the steel plate oxide layer and the surface of the mineral material, enabling the adhesive to maintain good interfacial bonding in slightly humid or saline environments. In other words, the composite amine curing agent can not only alleviate the water absorption and ion migration problems that may occur when carboxybetaine-type modified toughening agents are introduced alone, but also, through flexible curing, hydrophobic shielding, and interfacial coupling, can conversely enhance the wetting, adsorption, and toughening effects of this modified toughening agent at slightly humid interfaces.

[0012] Furthermore, this application first mixes epoxy resin, modified toughening agent, composite amine curing agent, and other raw materials to form an epoxy adhesive, and then mixes it with filler to form a steel bridge deck pavement binder. Natural crushed stone can provide a dense mineral skeleton, and steel fibers can form a fiber reinforcement effect between the mineral skeleton and the epoxy adhesive, improving the crack resistance, tensile strength, and fatigue resistance of the pavement layer. Since the modified toughening agent improves the adhesive's wetting and toughening ability on slightly wet steel plates and mineral surfaces, and the composite amine curing agent further improves the interfacial stability in humid, hot, and salty environments through polyether flexible curing, cashew phenol amine hydrophobic shielding, and silane interfacial coupling, the resulting binder can maintain high bond strength and tensile strength while improving elongation at break, low-temperature crack resistance, humid heat bond retention rate, salt water erosion resistance, and salt water erosion debonding resistance, thus better adapting to the service requirements of steel bridge deck pavement under complex service conditions such as vehicle loads, temperature changes, bridge deck vibration, rainwater, and snow melt salt erosion.

[0013] In some embodiments, the preparation method of the modified toughening agent includes the following steps: Polypropylene glycol diglycidyl ether is mixed and reacted with N,N-dimethylethanolamine, so that the hydroxyl groups in N,N-dimethylethanolamine react with some of the epoxy groups in polypropylene glycol diglycidyl ether to undergo a ring-opening reaction, thereby obtaining a polyether intermediate containing tertiary amine groups and having residual epoxy groups. Sodium chloroacetate is added to the polyether intermediate to cause the tertiary amine group to undergo a quaternization reaction with sodium chloroacetate, forming a carboxybetaine group, and obtaining a polyether compound containing carboxybetaine group and epoxy group as a modified toughening agent.

[0014] In some of the above methods, the hydroxyl groups in N,N-dimethylethanolamine act as nucleophilic active sites to attack some of the epoxy groups in polypropylene glycol diglycidyl ether, causing the epoxy ring to open and form ether bonds and hydroxyl structures. This allows the N,N-dimethylethanolamine fragment containing tertiary amine groups to be grafted onto the polypropylene glycol diglycidyl ether segment, resulting in a polyether intermediate containing tertiary amine groups and the remaining terminal epoxy groups. In this step, by controlling the amount of N,N-dimethylethanolamine added and the reaction time, only a portion of the epoxy groups in the polypropylene glycol diglycidyl ether undergo a ring-opening reaction, preventing the complete consumption of the terminal epoxy groups. This ensures that the resulting intermediate still possesses the terminal epoxy reactivity to participate in the subsequent epoxy-amine curing reaction. Subsequently, sodium chloroacetate is added to the above polyether intermediate, causing the tertiary amine groups on the polyether intermediate to undergo a quaternization reaction with sodium chloroacetate. The nitrogen atoms of the tertiary amine undergo a substitution reaction with the chloromethylene groups in sodium chloroacetate, forming a quaternary ammonium salt structure. At the same time, carboxylate groups are introduced, thereby forming carboxybetaine zwitterionic groups on the polyether segments. After these two steps, the resulting modified toughening agent simultaneously possesses polypropylene glycol flexible segments, the remaining terminal epoxy groups, and carboxybetaine zwitterionic groups.

[0015] In some embodiments, the preparation method of the modified toughening agent includes the following steps: 100 parts of polypropylene glycol diglycidyl ether were added to a reaction vessel and heated to 55-75°C. 4-10 parts of N,N-dimethylethanolamine were added under stirring and the reaction was maintained at this temperature for 2-4 hours to obtain a polyether intermediate containing tertiary amine groups and having residual epoxy groups. Dissolve 6-12 parts of sodium chloroacetate in 20-40 parts of deionized water, mix with 40-70 parts of ethanol, and add to the polyether intermediate. React at 65-85°C for 3-6 hours to form carboxybetaine groups. After the reaction is complete, remove ethanol and water under reduced pressure, and remove inorganic salts and unreacted small molecules to obtain the modified toughening agent.

[0016] The above methods specifically illustrate the reaction conditions and dosage ratios of each step in the preparation of the modified toughening agent. Under these conditions, toughening materials containing terminal epoxy groups, flexible segments, and zwitterionic groups can be obtained as modified toughening agents.

[0017] In some embodiments, the polyetheramine is an amino-terminated polyether.

[0018] In some embodiments, the polyetheramine is a primary amine-terminated polyoxypropylene ether diamine with a number average molecular weight of 300 to 500.

[0019] In some embodiments, the bisphenol A type epoxy resin is a liquid bisphenol A type epoxy resin with an epoxy value of 0.45 to 0.55 mol / 100g.

[0020] In some embodiments, the reactive diluent is a reactive glycidyl ether, including one or more of 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, and polypropylene glycol diglycidyl ether.

[0021] In some embodiments, the polyester fiber includes chopped polyester fiber.

[0022] In some embodiments, the accelerator is a tertiary amine accelerator.

[0023] Secondly, this application provides a method for preparing a high-toughness epoxy resin binder for steel bridge deck paving, comprising the following steps: Component A is obtained by mixing bisphenol A type epoxy resin, reactive diluent, modified toughening agent and polyester fiber, and component B is obtained by mixing composite amine curing agent and accelerator. Component A and component B are mixed at an equivalent ratio of epoxy groups to active hydrogen in amines of 1:0.8 to 1.2 to obtain a mixed adhesive. The mixed adhesive is mixed with filler to obtain a high-toughness epoxy resin binder for steel bridge deck paving.

[0024] According to this application, by first preparing an epoxy adhesive and then mixing it with natural crushed stone and steel fibers, the bisphenol A type epoxy resin, reactive diluent, and modified toughening agent in component A can fully contact and initiate a curing reaction with the composite amine curing agent in component B, thereby forming an adhesive system with good wetting and encapsulation properties. Subsequently, mixing with fillers facilitates the uniform coating of the adhesive onto the surfaces of the natural crushed stone and steel fibers, improving the interfacial bonding strength between the mineral skeleton and the resin system. Controlling the mass ratio of the mixed adhesive to fillers at 1:5–7 ensures that the mineral and steel fibers are fully wetted and coated, reducing porosity and interfacial defects, while avoiding excessive adhesive usage that could lead to increased costs, excessive fluidity, or decreased high-temperature stability. This results in a binder with good workability, density, bond strength, and toughness.

[0025] Compared with the prior art, the beneficial effects of this application are at least as follows: 1. This application introduces a polyether reaction product containing carboxyl betaine groups and residual epoxy reactivity, enabling it to simultaneously perform reactive grafting, flexible toughening, and micro-wetting interface effects, thereby improving the wetting and adsorption capacity of epoxy adhesives on micro-wet steel bridge decks, oxide layer micropores, and water-containing mineral surfaces. Recognizing that the zwitterionic structure may introduce risks of water absorption and salt ion migration, this application further employs a composite amine curing agent composed of polyetheramine, cashew phenolamine epoxy curing agent, and γ-aminopropyltriethoxysilane. This agent participates in epoxy curing while simultaneously adjusting flexibility, improving water and salt resistance, and enhancing the interface bonding between the steel plate and mineral material. This suppresses water and salt migration that may be caused by the zwitterionic structure and stably exerts the wetting, adsorption, and toughening effects of the modified toughening agent at the micro-wet interface, improving the interfacial bonding stability, wet-heat adhesion retention rate, and resistance to salt water erosion and debonding in micro-wet or salt-containing environments.

[0026] 2. This application does not simply improve the hydrophilicity or flexibility of the epoxy system, but rather improves the wettability of the micro-wet interface while also considering the interfacial durability under humid, hot, and saline environments. The modified toughening agent is used in combination with the composite amine curing agent to achieve a balance between micro-wet interface adaptability, cured product toughness, water and salt resistance stability, and interfacial bond retention in the epoxy adhesive. Polyester fibers, steel fibers, and natural crushed stone work together to improve the compactness, crack resistance, and fatigue resistance of the pavement layer, resulting in a steel bridge deck pavement binder that possesses high toughness, humid heat durability, salt water erosion resistance, and long-term service stability. Attached Figure Description

[0027] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.

[0028] Figure 1 Infrared spectrum of the modified toughening agent prepared in Example 1. Detailed Implementation

[0029] The various embodiments or implementation schemes in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments.

[0030] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with an embodiment or example is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0031] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0032] In this specification, unless otherwise specified, "parts" refers to "parts by weight".

[0033] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0034] Bisphenol A type epoxy resin: epoxy value 0.5 mol / 100g; Reactive diluent: 1,4-Butanediol diglycidyl ether; Polyester fiber: PET polyester staple fiber, length 6±1mm; Polyetheramine: Amino-terminated polyether, polyetheramine D-400, number average molecular weight 400; γ-aminopropyltriethoxysilane: KH-550; Accelerator: DMP-30; Polypropylene glycol diglycidyl ether: number average molecular weight 500; Natural crushed stone: continuously graded crushed stone less than 9.5mm; Steel fiber: Short-cut steel fiber, 3-6 mm in length.

[0035] Preparation Example 1 Preparation of modified toughening agents: 100 parts of polypropylene glycol diglycidyl ether were added to a reaction vessel and heated to 65°C. 7 parts of N,N-dimethylethanolamine were added under stirring and the reaction was maintained at this temperature for 3 hours. This allowed the hydroxyl groups in N,N-dimethylethanolamine to undergo a ring-opening reaction with some of the epoxy groups in polypropylene glycol diglycidyl ether, resulting in a polyether intermediate containing tertiary amine groups and residual epoxy groups. Nine parts of sodium chloroacetate were dissolved in 30 parts of deionized water and mixed with 55 parts of ethanol. The mixture was then added to the above polyether intermediate and reacted at 75°C for 5 hours to allow the tertiary amine group to undergo a quaternization reaction with sodium chloroacetate and form a carboxybetaine group. After the reaction was completed, ethanol and water were removed under reduced pressure, and inorganic salts and unreacted small molecules were removed to obtain the modified toughening agent.

[0036] like Figure 1 As shown, the infrared spectrum of the modified toughening agent exhibits typical structural characteristics of polyether betaine. At 3380 cm⁻¹... -1 A broad and strong absorption peak appears nearby, corresponding to the stretching vibration of the hydroxyl group (-OH) formed after the ring opening of the epoxide; 2968, 2920 and 2865 cm⁻¹ -1 The nearby absorption peaks are attributed to the stretching vibrations of CH2 and CH3 in the polyether chain, respectively. (1620 cm⁻¹) -1 The absorption peaks that appear nearby can be attributed to carboxylates (COO). - The antisymmetric stretching vibration of approximately 1400 cm -1 The absorption peak at that location corresponds to COO - The symmetric stretching vibrations of the polyether exhibit a relatively broad absorption band or shoulder peak due to some overlap with the CH2 / CH3 bending vibrations in the polyether backbone. This collectively indicates that the carboxybetaine structure has been successfully introduced into the polyether molecule. (1095 cm⁻¹) -1 The strong absorption peak at 915 cm⁻¹ is attributed to the stretching vibration of the COC bonds in the polyether backbone, and is a characteristic absorption of this polyether skeleton. Furthermore, at 915 cm⁻¹... -1 and 840cm -1 The characteristic absorption peaks of the epoxy ring can still be observed nearby, indicating that some epoxy groups underwent ring-opening in the first step of the reaction, while others were retained, providing active sites for subsequent chemical reactions with the epoxy resin matrix. The above characteristic peaks collectively demonstrate that the polyether backbone, carboxybetaine groups, and residual epoxy groups are all successfully present in the product, indicating that the target modified toughening agent has been successfully prepared.

[0037] Preparation Example 2 Preparation of composite amine curing agent: Add 50 parts of polyetheramine D-400, 30 parts of cashew phenolamine epoxy curing agent and 1 part of KH-550 to a mixing tank and stir at room temperature for 30 minutes to mix them evenly to obtain a composite amine curing agent.

[0038] Preparation Example 3 Preparation of composite amine curing agent: Add 50 parts of polyetheramine D-400, 20 parts of cashew phenolamine epoxy curing agent and 1 part of KH-550 to a mixing tank and stir at room temperature for 30 minutes to mix them evenly to obtain a composite amine curing agent.

[0039] Preparation Example 4 Preparation of composite amine curing agent: Add 50 parts of polyetheramine D-400, 40 parts of cashew phenolamine epoxy curing agent and 1 part of KH-550 to a mixing tank and stir for 30 minutes at room temperature to make them evenly mixed, so as to obtain a composite amine curing agent.

[0040] Comparative Preparation Example 1 Preparation of polyether toughening agents without carboxyl betaine groups: 100 parts of polypropylene glycol diglycidyl ether were added to a reaction vessel and heated to 65°C. Under stirring, 7 parts of N,N-dimethylethanolamine were added, and the reaction was maintained at this temperature for 3 hours. This allowed the hydroxyl groups in N,N-dimethylethanolamine to undergo a ring-opening reaction with some of the epoxy groups in the polypropylene glycol diglycidyl ether, yielding a polyether reaction product containing tertiary amine groups and exhibiting residual epoxy reactivity. After the reaction was completed, unreacted N,N-dimethylethanolamine and other small molecules were removed under reduced pressure to obtain a polyether toughening agent without carboxyl betaine groups. The difference between this comparative preparation example and Preparation Example 1 is that sodium chloroacetate was not added, and no quaternization reaction was performed.

[0041] Comparative Preparation Example 2 Preparation of composite amine curing agents without γ-aminopropyltriethoxysilane Add 50 parts of polyetheramine and 30 parts of cashew phenolamine epoxy curing agent to a mixing tank and stir for 30 minutes at room temperature to mix them evenly, so as to obtain a composite amine curing agent without γ-aminopropyltriethoxysilane.

[0042] Comparative preparation example 3 Preparation of composite amine curing agent without cashew phenol amine epoxy curing agent Add 50 parts of polyetheramine and 1 part of γ-aminopropyltriethoxysilane to a stirred tank and stir at room temperature for 30 minutes to mix them evenly, so as to obtain a composite amine curing agent without cashew phenol amine epoxy curing agent.

[0043] Example 1 Preparation of high-toughness epoxy resin binder for steel bridge deck paving Component A includes: 100 parts of bisphenol A type epoxy resin, 10 parts of reactive diluent, 15 parts of modified toughening agent prepared in Preparation Example 1, and 2 parts of polyester fiber. Component B includes: 35 parts of the composite amine curing agent prepared in Preparation Example 2 and 2 parts of the accelerator; The filler is made by mixing steel fibers and natural crushed stone at a mass ratio of 1:400.

[0044] During preparation, the raw materials of component A are mixed and stirred evenly to obtain component A; the raw materials of component B are mixed and stirred evenly to obtain component B; then components A and B are mixed and stirred for 3 minutes at an equivalent ratio of epoxy groups to amine active hydrogens of 1:1 to obtain a mixed adhesive; the mixed adhesive is mixed with 1000 parts of filler and forcibly stirred until the natural crushed stone and steel fibers are fully coated by the adhesive to obtain a high-toughness epoxy resin binder for steel bridge deck paving.

[0045] Example 2 Preparation of high-toughness epoxy resin binder for steel bridge deck paving It is basically the same as Example 1, except that 35 parts of the composite amine curing agent prepared in Preparation Example 3 are used instead of 35 parts of the composite amine curing agent prepared in Preparation Example 2 in Component B.

[0046] Example 3 Preparation of high-toughness epoxy resin binder for steel bridge deck paving It is basically the same as Example 1, except that 35 parts of the composite amine curing agent prepared in Preparation Example 4 are used instead of 35 parts of the composite amine curing agent prepared in Preparation Example 2 in Component B.

[0047] Comparative Example 1 Preparation of high-toughness epoxy resin binder for steel bridge deck paving The process is basically the same as in Example 1, except that 35 parts of the composite amine curing agent without γ-aminopropyltriethoxysilane prepared in Comparative Preparation Example 2 are used in component B instead of 35 parts of the composite amine curing agent prepared in Preparation Example 2.

[0048] Comparative Example 2 Preparation of high-toughness epoxy resin binder for steel bridge deck paving The preparation is basically the same as in Example 1, except that 35 parts of the composite amine curing agent without cashew phenol amine epoxy curing agent prepared in Comparative Preparation Example 3 are used in component B instead of 35 parts of the composite amine curing agent prepared in Preparation Example 2.

[0049] Comparative Example 3 Preparation of high-toughness epoxy resin binder for steel bridge deck paving The preparation is basically the same as in Example 1, except that the composite amine curing agent prepared in Example 2 is not added to component B, but is replaced by 35 parts of polyetheramine.

[0050] This comparative example was used to investigate the microwetting effect and water and salt stability of the carboxybetaine-type modified toughening agent when used alone.

[0051] Comparative Example 4 Preparation of high-toughness epoxy resin binder for steel bridge deck paving The process is basically the same as in Example 1, except that the modified toughening agent prepared in Preparation Example 1 is not added to component A, but is replaced by 15 parts of the polyether toughening agent without carboxyl betaine groups prepared in Comparative Preparation Example 1.

[0052] Comparative Example 5 Preparation of high-toughness epoxy resin binder for steel bridge deck paving The preparation is basically the same as in Example 1, except that the modified toughening agent prepared in Example 1 is not added to component A, but is replaced by 15 parts of polypropylene glycol diglycidyl ether.

[0053] Comparative Example 6 Preparation of high-toughness epoxy resin binder for steel bridge deck paving The preparation is basically the same as in Example 1, except that the modified toughening agent prepared in Example 1 is not added to component A, but is replaced by 15 parts of polypropylene glycol diglycidyl ether; and the composite amine curing agent prepared in Example 2 is not added to component B, but is replaced by 35 parts of polyether amine.

[0054] Test section Dry bond strength test According to the method described in the national standard GB / T 7124-2008 "Determination of Tensile Shear Strength of Adhesives (Rigid Material to Rigid Material)", Q235 steel plate was used as the substrate. The steel plate dimensions were 100mm long × 25mm wide × 2.0mm thick. The surface of the steel plate was sandblasted until a metallic luster was exposed, and after removing dust and oil, it was dried for later use. The mixed adhesives obtained in the examples and comparative examples were uniformly applied to the surface of the steel plate, with the adhesive layer thickness controlled at 1.0-2.0mm. It was then overlapped or bonded to another steel plate that had undergone the same treatment, forming a bonding area of ​​12.5mm × 25mm. After curing at 25±2℃ for 7 days, tensile shear or pull-out tests were performed using a universal testing machine with a loading speed of 5 mm / min. The maximum load at failure was recorded, and the dry bond strength was calculated based on the bonded area. The results are shown in Table 1.

[0055] Micro-wet interface bond strength test After sandblasting and cleaning, the steel plate surface is not completely dried. Instead, a small amount of deionized water is evenly sprayed onto the surface, with the spraying amount controlled at 0.02–0.05 g / cm³. 2The steel plate surface was gently wiped with a lint-free cloth until it was slightly damp but without obvious water. The epoxy adhesives obtained in the examples and comparative examples were then immediately applied, and bonding samples were prepared according to the dry bond strength test method. The bonding strength of the samples was tested after curing at 25±2℃ for 7 days, and this strength was used as the bonding strength at the slightly damp interface. The results are shown in Table 1.

[0056] Test of bond strength retention after salt water immersion Steel plate bonding samples were prepared according to the dry bond strength test method. After curing the samples at 25±2℃ for 7 days, they were immersed in a 3.5% sodium chloride aqueous solution at 25℃ for 7 days. After immersion, the samples were removed, surface moisture was wiped off, and the bond strength was tested and recorded as the bond strength after salt water immersion. The bond strength retention rate after salt water immersion was calculated according to the following formula: The percentage of bond strength retention after salt water immersion is calculated as: (Bond strength after salt water immersion / Dry bond strength) × 100%. The results are shown in Table 1.

[0057] Elongation at break test The epoxy adhesives obtained in the examples and comparative examples were cast into polytetrafluoroethylene molds or flat molds that had undergone demolding treatment to prepare adhesive film samples with a length of 25 mm and a thickness of 2.0 ± 0.2 mm. After curing at 25 ± 2 °C for 7 days, the samples were cut into dumbbell-shaped tensile specimens. The elongation at break was tested using a universal testing machine, and the elongation at break was recorded. The elongation at break was calculated, and the test results are shown in Table 2.

[0058] Low temperature bending strain test The epoxy resin binders obtained in the examples and comparative examples were molded into beam-shaped specimens with a length of 200 mm, a width of 30 mm, and a height of 35 mm. After curing at 25 ± 2 °C for 7 days, the specimens were placed in an environment at -10 °C for at least 4 hours. Subsequently, a three-point bending test was conducted at -10 °C with a loading rate of 50 mm / min. The maximum load and mid-span deflection at the point of specimen failure were recorded, and the tensile strain at failure was calculated as the low-temperature bending strain. The results are shown in Table 2.

[0059] Table 1 Table 2 As shown in Examples 1 and 2-3, there is an optimal range for the addition ratio of cashew phenol amine epoxy curing agent in the composite amine curing agent. Its dosage directly affects the overall balance between toughness, water and salt resistance, and interfacial adhesion retention. In Example 2, when the amount of cashew phenol amine epoxy curing agent is relatively low, although the proportion of flexible polyether segments in the cured network is relatively high, which is beneficial for improving the material's elongation at break and low-temperature deformation ability, the insufficient hydrophobic long-chain units in the system weaken the shielding effect against water absorption and salt ion penetration that may be caused by highly polar carboxylic betaine groups, resulting in a significant decrease in the interfacial adhesion retention rate after salt water immersion. Conversely, in Example 3, when the amount of cashew phenol amine epoxy curing agent is too high, although it enhances the hydrophobicity of the cured network and the interfacial resistance to salt water erosion and debonding, the excessive rigid hydrophobic segments and phenolic structure restrict the movement of the flexible polyether segments, adversely affecting the elongation and low-temperature crack resistance of the cured product. It is evident that only with appropriate proportions can the material maintain high bonding strength in both dry and slightly wet environments, while also ensuring good toughness, low-temperature crack resistance, and long-term resistance to salt water erosion.

[0060] As shown in Example 1 and Comparative Example 1, the lack of KH-550 in the composite amine curing agent in Comparative Example 1 significantly reduced the retention rate of adhesive strength after salt water immersion. This is because the alkoxysilane structure of KH-550, after hydrolysis, can form chemical bonds with the hydroxyl groups on the surface of the steel bridge deck oxide layer. This interfacial covalent bond is much more stable in salt water media than physical adsorption. Without this interfacial coupling effect, moisture and salt ions can more easily penetrate along the adhesive / steel plate interface, weakening the interfacial bond. Therefore, KH-550 is a key component to ensure long-term water and salt resistance interfacial stability.

[0061] As shown in Example 1 and Comparative Example 2, the adhesion strength retention rate after brine immersion in Comparative Example 2 was significantly reduced after the composite amine curing agent was not composed of cashew phenol amine epoxy curing agent. This may be because the long-chain alkyl hydrophobic segments in the cashew phenol amine molecule can form localized hydrophobic microregions in the cured network, effectively inhibiting the diffusion of water and salt ions to the highly polar carboxybetaine region. Without this hydrophobic shielding effect, the strong water absorption tendency of the zwitterionic groups will cause brine to penetrate more easily to the interface, weakening the adhesion layer's resistance to brine erosion and debonding.

[0062] As can be seen from Example 1 and Comparative Example 3, in Comparative Example 3, only polyetheramine was used as a curing agent, and cashew phenolamine and KH-550 were completely absent. The strength retention rate of the latter decreased the most significantly after soaking in salt water. This is because polyetheramine can only provide flexible segments to participate in curing. It cannot form hydrophobic shielding micro-regions to inhibit water penetration, nor can it enhance the interfacial bonding through chemical bonding. Under these conditions, the strong hydration ability of the carboxybetaine group becomes a water absorption channel, which makes it easy for salt water and water to accumulate in the interfacial region, causing interfacial debonding and corrosion.

[0063] As shown in Example 1 and Comparative Example 4, the modified toughening agent in Comparative Example 4, lacking the carboxybetaine group, exhibits a significant decrease in the bonding strength at the micro-wet interface. The principle behind this is that carboxybetaine, as an amphoteric structure, possesses strong polarity and hydration capabilities. It can displace and bind trace amounts of moisture on the surface of the oxide layer of the micro-wet steel bridge deck, transforming the weak boundary layer of free water, which is detrimental to bonding, into a hydrated bonding layer. This improves the wetting and adsorption of the resin on the micro-wet substrate. Without this group, the resin system cannot effectively displace the water film and maintain close contact with the substrate at the micro-wet interface, resulting in a significant weak boundary layer effect. Therefore, this group is the core functional unit for achieving reliable bonding at the micro-wet interface.

[0064] As can be seen from Examples 1 and 5, in Comparative Example 5, the micro-wet bond strength and elongation at break were significantly lower when only ordinary polypropylene glycol diglycidyl ether was used instead of the modified toughening agent of this application. This is because the ordinary polyether diluent does not contain carboxyl betaine groups on its molecular chain, and therefore does not have the ability to replace water and wetting at the micro-wet interface; at the same time, it exists in the system only in a physical blending manner, lacking the reactivity to covalently connect with the cured network, and thus has limited effect on the flexible control of the network structure of the cured product.

[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.

Claims

1. A high-toughness epoxy resin binder for steel bridge deck paving, characterized in that, Includes the following quantities of raw materials: 100 parts bisphenol A type epoxy resin, 8-12 parts reactive diluent, 10-20 parts modified toughening agent, 1-2.5 parts polyester fiber, 25-45 parts composite amine curing agent, 1-3 parts accelerator, 800-1200 parts filler. The modified toughening agent includes a polyether compound containing carboxyl betaine groups and epoxy groups; The composite amine curing agent is obtained by mixing polyether amine, cashew phenol amine epoxy curing agent, and γ-aminopropyltriethoxysilane in a mass ratio of 50:(20-40):(0.5-1.5). The filler is obtained by mixing steel fibers and natural crushed stone at a mass ratio of 1:300-500.

2. The high-toughness epoxy resin binder for steel bridge deck paving according to claim 1, characterized in that, The preparation method of the modified toughening agent includes the following steps: Polypropylene glycol diglycidyl ether is mixed and reacted with N,N-dimethylethanolamine, so that the hydroxyl groups in N,N-dimethylethanolamine react with some of the epoxy groups in polypropylene glycol diglycidyl ether to undergo a ring-opening reaction, thereby obtaining a polyether intermediate containing tertiary amine groups and having residual epoxy groups. Sodium chloroacetate is added to the polyether intermediate to cause the tertiary amine group to undergo a quaternization reaction with sodium chloroacetate, forming a carboxybetaine group, and obtaining a polyether compound containing carboxybetaine group and epoxy group as a modified toughening agent.

3. The high-toughness epoxy resin binder for steel bridge deck paving according to claim 2, characterized in that, The preparation method of the modified toughening agent includes the following steps: 100 parts of polypropylene glycol diglycidyl ether were added to a reaction vessel and heated to 55-75°C. 4-10 parts of N,N-dimethylethanolamine were added under stirring and the reaction was maintained at this temperature for 2-4 hours to obtain a polyether intermediate containing tertiary amine groups and having residual epoxy groups. Dissolve 6-12 parts of sodium chloroacetate in 20-40 parts of deionized water, mix with 40-70 parts of ethanol, and add to the polyether intermediate. React at 65-85°C for 3-6 hours to form carboxybetaine groups. After the reaction is complete, remove ethanol and water under reduced pressure, and remove inorganic salts and unreacted small molecules to obtain the modified toughening agent.

4. The high-toughness epoxy resin binder for steel bridge deck paving according to claim 1, characterized in that, The polyetheramine is an amino-terminated polyether.

5. The high-toughness epoxy resin binder for steel bridge deck paving according to claim 4, characterized in that, The polyetheramine is a polyoxypropylene ether diamine with primary amine-terminated ends and a number average molecular weight of 300-500.

6. The high-toughness epoxy resin binder for steel bridge deck paving according to claim 1, characterized in that, The bisphenol A type epoxy resin is a liquid bisphenol A type epoxy resin with an epoxy value of 0.45 to 0.55 mol / 100g.

7. The high-toughness epoxy resin binder for steel bridge deck paving according to claim 1, characterized in that, The reactive diluent is a reactive glycidyl ether, including one or more of 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, and polypropylene glycol diglycidyl ether.

8. The high-toughness epoxy resin binder for steel bridge deck paving according to claim 1, characterized in that, The polyester fibers include chopped polyester fibers.

9. A high-toughness epoxy resin binder for steel bridge deck paving according to claim 1, characterized in that, The accelerator is a tertiary amine accelerator.

10. A method for preparing a high-toughness epoxy resin binder for steel bridge deck paving, characterized in that, Includes the following steps: Provide the raw materials as described in claims 1 to 9; Component A is obtained by mixing bisphenol A type epoxy resin, reactive diluent, modified toughening agent and polyester fiber, and component B is obtained by mixing composite amine curing agent and accelerator. Component A and component B are mixed at an equivalent ratio of epoxy groups to active hydrogen in amines of 1:0.8 to 1.2 to obtain a mixed adhesive. The mixed adhesive is mixed with filler to obtain a high-toughness epoxy resin binder for steel bridge deck paving.