A two-stage curing polyurethane composite binder for water permeable pavement and a preparation method and application thereof

By using the interfacial directional reaction of the two-stage curing polyurethane composite binder and the water-triggered secondary densification components, the adhesion and structural stability of the aggregate-binder interface in permeable pavement are improved, solving the problem of easy interface deterioration in the prior art, and making it suitable for heavy-duty permeable pavement.

CN123131972APending Publication Date: 2026-11-20TONGJI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611644913.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-23
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing polyurethane binders for permeable pavements have insufficient adhesion at the aggregate-binder interface, making them susceptible to deterioration under water exposure and difficult to balance permeability and long-term service performance.

Method used

A two-stage curing polyurethane composite binder is adopted, which improves interfacial adhesion and provides local reinforcement during service life by combining interfacial directional reactive components and water-triggered secondary densification components. This includes the use of interfacial directional reactive components containing hydrolyzable silanes and microencapsulated polyurea shell water-triggered components.

Benefits of technology

It improves the bonding stability of the aggregate-binder interface and the structural stability of permeable pavement, maintains the permeability function, and slows down the deterioration of weak areas at the interface during long-term service. It is suitable for heavy-duty permeable pavement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123131972A_ABST
    Figure CN123131972A_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of road engineering maintenance and repair, and particularly relates to a two-stage curing polyurethane composite binder for a water-permeable pavement as well as a preparation method and application thereof. The two-stage curing polyurethane composite binder comprises the following components in mass fractions: 100 parts of polyurethane prepolymer; 1-5 parts of an interface directional reaction component; 0.5-6 parts of a water-triggered secondary densification component; 0.02-0.8 parts of a catalyst; 1-10 parts of a chain extender; 5-60 parts of a filler; 0.1-3 parts of a rheological modifier; and 0.1-2 parts of an auxiliary agent. Compared with the prior art, the two-stage curing polyurethane composite binder has both initial forming and binding functions and subsequent service period local reinforcement functions, and is conducive to taking into account the water-permeable pavement construction forming adaptability and long-term service interface stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of road engineering maintenance and repair technology, and relates to a two-stage curing polyurethane composite binder for permeable pavements, its preparation method and application. Background Technology

[0002] Permeable pavement is an important component of sponge cities, green transportation infrastructure, and functional paving. Compared to traditional dense pavements, permeable pavements need to maintain the structural stability and service durability of the aggregate skeleton while ensuring interconnected pores and drainage channels. In recent years, in addition to permeable cement concrete and permeable asphalt, polyurethane-based binders have been increasingly used in permeable pavements and related road functional layers due to their high initial bonding strength, good construction environmental friendliness, and low temperature sensitivity, demonstrating great application potential.

[0003] Existing polyurethane binders for permeable pavements typically employ single-component or two-component polyurethane systems. These systems utilize the reaction of polyols and polyisocyanates to form a polyurethane curing network, which binds the open-graded aggregate skeleton and creates a permeable structural layer. This technology enables the basic shaping and initial bonding of permeable pavements and has been used in general permeable roads, landscape paving, and pedestrian systems. However, the following shortcomings still exist: (1) The interface interaction between aggregates and polyurethane is still mainly based on conventional coating and bonding. The aggregate-binder interface is still prone to becoming a weak part in the large pore structure, and the adhesion is insufficient under the coupling effect of environment and traffic; (2) In the existing technology, moisture is often regarded as an environmental factor for polyurethane curing or an unfavorable factor for service durability. It is easy to enter the interior of the structural layer along the interconnected pores, thereby causing structural loosening and other defects during long-term service; (3) The existing polyurethane permeable pavement technology is mainly aimed at general permeable pavement scenarios. There is still room for improvement in terms of higher traffic loads, long-term effects of moisture in interconnected pores, and continuous stability of the aggregate-binder interface. In particular, it is difficult to take into account the composite requirements of interface stability, interconnected pore maintenance, and long-term structural durability of permeable pavement, including heavy loads.

[0004] Therefore, how to improve the bonding performance of the mineral aggregate-polyurethane interface and maintain the permeability and service durability of permeable pavements remains a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0005] The purpose of this invention is to overcome the problems of insufficient adhesion between aggregate and binder interface, easy interface deterioration under water action, and difficulty in balancing the maintenance of permeable skeleton structure and long-term service performance of existing polyurethane binder materials for permeable pavements. This invention provides a two-stage curing polyurethane composite binder for permeable pavements, its preparation method, and its application.

[0006] The objective of this invention can be achieved through the following technical solutions: One of the technical solutions of the present invention is to provide a two-stage curing polyurethane composite binder for permeable pavements, comprising the following components in parts by weight: 100 parts of polyurethane prepolymer; 1-5 parts of interfacial directional reaction component; 0.5–6 parts of water-triggered secondary densification component; Catalyst: 0.02–0.8 parts; Chain extender 1-10 parts; 5-60 parts of filler; Rheology modifier 0.1–3 parts; 0.1 to 2 parts of auxiliary agent; The polyurethane prepolymer is an isocyanate-containing prepolymer, and the isocyanate content in the polyurethane prepolymer is 10wt% to 18wt%. The interface-directed reaction component is a silane coupling agent containing both hydrolyzable silane groups and organic functional groups, wherein the organic functional groups are selected from at least one of amino and epoxy groups; The water-triggered secondary densification component is a microcapsule with a polyurea shell and a reactive isocyanate active component as the core material.

[0007] In some specific embodiments, the interface-oriented reaction component is selected from any one or both of γ-aminopropyltriethoxysilane (KH-550) and γ-(2,3-epoxypropoxy)propyltrimethoxysilane (KH-560); When the interface-directed reaction component is composed of γ-aminopropyltriethoxysilane and γ-(2,3-epoxypropoxy)propyltrimethoxysilane, the mass ratio of γ-aminopropyltriethoxysilane to γ-(2,3-epoxypropoxy)propyltrimethoxysilane is 1:1 to 4:1.

[0008] More preferably, the mass ratio of γ-aminopropyltriethoxysilane to γ-(2,3-epoxypropoxy)propyltrimethoxysilane is 3:2.

[0009] In some specific embodiments, the polyurethane prepolymer is obtained by the following preparation method: The polyether diol was dehydrated to a moisture content of less than 0.05%. Diphenylmethane diisocyanate (MDI) was added under nitrogen protection and mechanical stirring, and the equivalent ratio of isocyanate groups to hydroxyl groups (NCO / OH) was controlled to be 3.8~4.2:1. The reaction was continued at 75~85℃ for 2~3 h. During the reaction, the isocyanate group content of the system was measured periodically. The reaction was stopped when the isocyanate group content was basically stable. The mixture was cooled and sealed for storage to obtain an isocyanate-terminated polyether polyurethane prepolymer.

[0010] In some specific embodiments, the water-triggered secondary densification component is obtained by the following preparation method: Isophorone diisocyanate (IPDI) and polymethylene polyphenyl polyisocyanate (PAPI) containing 30%–32% isocyanate groups by mass were mixed at a mass ratio of 2.6–4.9:1 to obtain the oil phase; A composite emulsifier is obtained by mixing polyvinyl alcohol (PVA-1795) and gum arabic at a mass ratio of 0.9–3.5:1. The composite emulsifier is then mixed with water to obtain an aqueous phase, wherein the total amount of the composite emulsifier is 2–5 wt% of the mass of the aqueous phase. The oil phase is slowly added to the water phase, and the mass ratio of the oil phase to the water phase is 12~20:60. The mixture is emulsified at 5000~7000 rpm for 4~6 min at 0~5℃ to form an oil-in-water emulsion. A 2-3 wt% aqueous solution of diethylenetriamine (DETA) is added dropwise to the oil-in-water emulsion, such that the mass ratio of the oil phase, aqueous phase, and DETA aqueous solution is 12-20:60:60. The dropwise addition time is 15-20 min, allowing the amino groups in the diethylenetriamine aqueous solution to react with the isocyanate groups in the polymethylene polyphenyl polyisocyanate at the oil-water interface, forming a polyurea shell in situ. After the dropwise addition is completed, stirring is continued for 20-40 min, and then the temperature is increased to 60-65°C at a rate of 9-11°C / min, and the reaction is maintained at this temperature for 1.5-2.5 h. After the reaction was completed and cooled to room temperature, the microcapsules were obtained by centrifugation or filtration. They were then washed with deionized water and petroleum ether in sequence, and vacuum dried at 30–40 °C for 12–24 h to obtain the microencapsulated water-triggered secondary densification component.

[0011] In some specific embodiments, the median particle size D50 of the microcapsules is 5–30 μm; The shell thickness of the microcapsule is 0.2–3 μm and does not exceed 1 / 4 of the median particle size D50 of the microcapsule volume. The core-to-wall mass ratio of the microcapsule is 1:1 to 50:1.

[0012] More preferably, the core-to-wall mass ratio of the microcapsule is 2:1 to 8:1.

[0013] More preferably, the core-to-wall mass ratio of the microcapsule is 3:1 to 5:1.

[0014] In some specific embodiments, the catalyst is an organobismuth catalyst.

[0015] In some specific embodiments, the chain extender is 1,4-butanediol.

[0016] In some specific embodiments, the filler is a composite filler made by mixing mineral powder and silica fume in a mass ratio of 3:1 to 5:1.

[0017] More preferably, the mass ratio of the mineral powder to silica fume is 4:1.

[0018] In some specific embodiments, the rheology modifier is fumed silica.

[0019] In some specific embodiments, the additive is selected from at least one of stabilizers, antioxidants, ultraviolet absorbers, and defoamers.

[0020] The second technical solution of the present invention provides a method for preparing a two-stage curing polyurethane composite binder for permeable pavements as described in one of the above technical solutions, comprising the following steps: A1. Add interfacial directional reaction components, catalysts, chain extenders, fillers, rheology modifiers, and additives to polyurethane prepolymer and mix to obtain a premixed binder; A2. Add water to the premixed binder obtained in step A1 to trigger the secondary densification component, stir under low shear conditions to make it uniformly dispersed, and obtain a two-stage curing polyurethane composite binder. or, B1. Add an interfacial directional reaction component to the polyurethane prepolymer and mix to obtain a pre-reactive modified polyurethane prepolymer; B2. Add water-triggered secondary densification components, catalysts, chain extenders, fillers, rheology modifiers, and additives to the pre-reactive modified polyurethane prepolymer obtained in step B1, and mix to obtain a two-stage curing polyurethane composite binder.

[0021] In some specific embodiments, step A1 involves mixing under the following conditions: dispersion at 300–1200 rpm for 5–40 minutes at 20–60°C. Step A2: When the temperature of the premixed binder is 15-40°C, water is added to trigger a secondary densification component. The mixing conditions were to disperse the microcapsules at a speed of 50–300 rpm for 2–15 min and at a temperature of 25 ± 2 °C, in order to reduce the risk of unintended damage to the microcapsules during the mixing process.

[0022] In some specific embodiments, step B1 involves mixing under the following conditions: dispersion at a speed of 300–1200 rpm for 5–40 min and a temperature of 20–60°C. In step B2, when the temperature of the pre-reactive modified polyurethane prepolymer is 15-40°C, water-triggered secondary densification components, catalysts, chain extenders, fillers, rheology modifiers, and additives are added. The mixing conditions were to disperse the microcapsules at a speed of 50–300 rpm for 2–15 min and at a temperature of 25 ± 2 °C, in order to reduce the risk of unintended damage to the microcapsules during the mixing process.

[0023] The second technical solution of the present invention is to provide an application of the two-stage curing polyurethane composite binder as described in one of the above technical solutions in the preparation of permeable pavement structural layers.

[0024] In some specific embodiments, the permeable pavement structure layer is formed by an open-graded aggregate skeleton.

[0025] In some specific embodiments, the permeable pavement is a heavy-duty permeable pavement.

[0026] In this invention, the water-triggered secondary densification component is introduced in the form of microcapsules. Its polyurea shell forms a diffusion barrier on the core material during the preparation and initial curing stages. Unintended shell breakage of the microcapsules is reduced through post-addition and low-shear dispersion processes, keeping the component latent during the initial curing stage. The initial molding and interface construction are mainly completed by the polyurethane prepolymer and the interface-oriented reactive component. The interface-oriented reactive component can be introduced into the polyurethane system through direct incorporation, pre-reaction, or a combination of partial pre-reaction and partial free incorporation. During service, ambient moisture enters the structural layer through interconnected pores and gradually acts on the polyurea shell, causing the reactive isocyanate component within the microcapsules to gradually participate in the reaction. This facilitates the formation of supplementary reaction products or localized filling reinforcement in the aggregate-binder interface region, thereby improving wet interface retention and anti-scattering performance. Thus, this invention forms a two-stage curing mechanism combining initial curing and service-stage water-triggered densification.

[0027] Compared with the prior art, the present invention has the following advantages: (1) The present invention designs an interface-oriented reaction component containing hydrolyzable silane, which can participate in the formation of polyurethane curing network and form an interface chemical bond on the surface of mineral aggregates, which is beneficial to improve the bonding state of the aggregate-binder interface and improve the interface stability.

[0028] (2) The present invention designs a microencapsulated water-triggered secondary densification component for a polyurea shell-coated reactive isocyanate core material, so that the binder can undergo further local densification in the interface area under the action of subsequent moisture after initial curing, thereby helping to slow down the deterioration of the weak interface area in the permeable structure under the action of water.

[0029] (3) The present invention does not achieve structural reinforcement by significantly increasing the amount of binder or by completely closing the pores. Instead, it improves the state of the interface area by combining interface directional construction with local secondary densification. Therefore, it is beneficial to improve the structural stability while maintaining the interconnected pore structure of the permeable skeleton. In the embodiments of the present invention, the permeability retention rate only changes slightly and remains above 90%, indicating that the improvement of the above-mentioned structural stability is not at the expense of significantly sacrificing the permeability function.

[0030] (4) The dual-stage curing polyurethane composite binder of the present invention has both initial molding and bonding functions and subsequent service period local reinforcement functions, which is beneficial to balance the adaptability of permeable pavement construction and the stability of interface during long-term service.

[0031] (5) The composition of the two-stage curing polyurethane composite binder of the present invention is clear and the preparation steps are clear, which is suitable for the preparation and application of permeable pavement structural layers, especially for heavy-duty permeable pavement structural layers. Attached Figure Description

[0032] Figure 1 This is a schematic diagram of the preparation method of the two-stage curing polyurethane composite binder of the present invention.

[0033] Figure 2 A comparison chart of the interfacial bonding performance test results for each group of specimens.

[0034] Figure 3 This is a comparison chart of the permeability coefficient and permeability retention rate results for each group of specimens.

[0035] Figure 4 This is a comparison chart of the interconnected porosity test results for each group of specimens.

[0036] Figure 5 A comparison chart of the structural stability performance test results for each group of specimens.

[0037] Figure 6 This is a schematic diagram of the structure of the microencapsulated water-triggered secondary densification component of the present invention, wherein 12 is a microcapsule, 13 is a core material, and 14 is a polyurea shell. Detailed Implementation

[0038] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. These embodiments are based on the technical solution of the present invention and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.

[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application.

[0040] Unless otherwise specified, the materials and processes used in the following embodiments or examples are conventional materials and processes employed in the art to achieve the corresponding functions.

[0041] Example 1: This embodiment provides a two-stage curing polyurethane composite binder for permeable pavements, the preparation method of which is as follows: Figure 1 As shown, it includes the following steps: 1. Raw materials (1) Polyurethane prepolymer: Isocyanate-terminated polyether polyurethane prepolymer with an isocyanate group content of 12.5 wt% was selected.

[0042] The method for preparing the isocyanate-terminated polyether polyurethane prepolymer used in this embodiment is as follows: Polyether diol PPG1000 is added to a reaction vessel and dehydrated under vacuum at 110±5℃ for 1–2 h until the moisture content is below 0.05%. Then, the temperature is lowered to 70–80℃, and diphenylmethane diisocyanate (MDI) is added under nitrogen protection and mechanical stirring, controlling the isocyanate group to hydroxyl group equivalent ratio (NCO / OH) to be approximately 4.0:1. The reaction is continued at 75–85℃ for 2–3 h, with the isocyanate group content of the system measured periodically during the reaction. The reaction is terminated after the isocyanate group content has stabilized. The prepolymer is then cooled and sealed for storage to obtain the isocyanate-terminated polyether polyurethane prepolymer. The isocyanate group content of the obtained polyurethane prepolymer is 12.5 wt%.

[0043] (2) Interfacial directional reaction components: a compound system of γ-aminopropyltriethoxysilane (KH-550) and γ-(2,3-epoxypropoxy)propyltrimethoxysilane (KH-560, i.e. glycidyl etheroxypropyltrimethoxysilane) was selected, with a mass ratio of 3:2.

[0044] (3) Water-triggered secondary densification components: Microencapsulated latent reaction components, such as Figure 6 The microcapsule 12 structure shown consists of a polyurea shell 14 and a core material 13, wherein the core material 13 is composed of a reactive isocyanate active component; the median particle size D50 of the microcapsule 12 is 18 μm, the thickness of the polyurea shell 14 is 0.6 μm, and the core-to-wall mass ratio is approximately 4:1.

[0045] The microencapsulated water-triggered secondary densification component can be prepared by interfacial polymerization or by commercially available microcapsules that meet the above requirements for particle size, polyurea shell 14 and core material 13.

[0046] The preparation method of the microencapsulated water-triggered secondary densification component includes the following preparation steps: using isophorone diisocyanate (IPDI) as the main reactive core material, and polymethylene polyphenyl polyisocyanate (PAPI, isocyanate group mass fraction of 30% to 32%, WANNATE® PM-200 produced by Wanhua Chemical Group Co., Ltd.) as the interface shell-forming isocyanate component, with a mass ratio of IPDI to PAPI of 3:1; adding 5% to 10% of cyclohexanone as an inert diluent to adjust the viscosity of the oil phase, in this embodiment the amount of cyclohexanone used is 5% of the total mass of the oil phase.

[0047] Polyvinyl alcohol (PVA-1795) and gum arabic were used as a composite emulsifier, with a PVA-1795 to gum arabic mass ratio of 2:1. The total amount of the composite emulsifier was 3 wt% of the aqueous phase, and deionized water was used as the continuous phase. The oil phase was slowly added to the aqueous phase at a mass ratio of 16:60. Emulsification was carried out at 6000 rpm for 5 min using a high-speed homogenizing disperser at 0–5 °C to form a stable oil-in-water emulsion.

[0048] Subsequently, 60 g of a 2.8 wt% diethylenetriamine (DETA) aqueous solution was added dropwise to the above oil-in-water emulsion, with the mass ratio of oil phase, aqueous phase, and DETA aqueous solution being 16:60:60. The addition time was controlled at 15–20 min, allowing the amino groups in DETA to react primarily with the isocyanate groups in PAPI at the oil-water interface, forming a polyurea shell in situ. After the addition was complete, stirring was continued for 30 min, and then the temperature was increased to 60–65 °C at a rate of approximately 10 °C / min, and the reaction was maintained at this temperature for 2 h.

[0049] After the reaction was completed and cooled to room temperature, the microcapsules were obtained by centrifugation or filtration. They were then washed with deionized water and petroleum ether in sequence, and vacuum dried at 30–40 °C for 12–24 h to obtain the water-triggered secondary densification component of the microencapsulation.

[0050] (4) Catalyst: an organic bismuth catalyst was selected. In this example, BCAT-E16 organic bismuth catalyst was used.

[0051] (5) Chain extender: 1,4-Butanediol is selected.

[0052] (6) Filler: A composite filler of limestone powder and silica fume is selected with a mass ratio of 4:1. The limestone powder is ordinary limestone powder produced by the road material supplier. The powder is obtained by grinding limestone and is required to be dry, clean, and free of lumps and agglomerates. The passing rate of the 0.60 mm sieve is 100%, the passing rate of the 0.15 mm sieve is 90% to 100%, and the passing rate of the 0.075 mm sieve is 75% to 100%. The silica fume is NR90 silica fume produced by Wuhan Newrich New Materials Co., Ltd.

[0053] (7) Rheology modifier: Fumed silica is selected.

[0054] (8) Additives: The composite additives selected are RIANOX® 1010 hindered phenolic antioxidant (produced by Tianjin Lianlong New Material Co., Ltd.), RIASORB® UV-P ultraviolet absorber (produced by Tianjin Lianlong New Material Co., Ltd.) and Tech-4854 non-silicone polymer defoamer (produced by Shanghai Tiger Polymer Technology Co., Ltd.), with a mass ratio of 1:2:1.

[0055] 2. Preparation of two-stage curing polyurethane composite binder, such as... Figure 1 As shown, it includes the following steps: (1) Weigh each component according to the following proportions: 100 parts of polyurethane prepolymer, 3 parts of interfacial directional reaction component, 2 parts of water-triggered secondary densification component, 0.15 parts of catalyst, 4 parts of chain extender, 20 parts of filler, 0.8 parts of rheology modifier, and 0.6 parts of additive.

[0056] (2) Add the polyurethane prepolymer to a mixing container equipped with a mechanical stirring device and pre-stir at 400 rpm for 10 min at 35°C.

[0057] (3) Add the interfacial directional reaction component, catalyst, chain extender, filler, rheology modifier and additive to the system obtained in step (2), and stir and disperse at 800 rpm for 20 min at 35°C to obtain the premixed binder.

[0058] (4) After the premixed binder obtained in step (3) cools down to 25°C, water is added to trigger the secondary densification component, and the mixture is stirred at 120 rpm with low shear for 5 min to disperse it evenly, thus obtaining a two-stage curing polyurethane composite binder.

[0059] Example 2 The difference between this embodiment and Embodiment 1 is that the interface-oriented reactive component is introduced into the polyurethane prepolymer through a pre-reaction modification method.

[0060] Except for the interface-oriented reaction component, which was introduced through pre-reaction modification, the types, proportions, and preparation conditions of the other raw materials were the same as in Example 1.

[0061] Specifically, polyurethane prepolymer and interfacial directional reaction component were weighed at a mass ratio of 100:3, and stirred at 300 rpm for 30 min at 45℃ to obtain pre-reactive modified polyurethane prepolymer. After cooling to 25℃, 2 parts of water-triggered secondary densification component, 0.15 parts of catalyst, 4 parts of chain extender, 20 parts of filler, 0.8 parts of rheology modifier, and 0.6 parts of additive were added, and stirred at 120 rpm with low shear for 5 min to ensure uniform dispersion, thus obtaining a two-stage curing polyurethane composite binder.

[0062] Example 3 This embodiment is largely the same as Embodiment 1, except that the amount of water-triggered secondary densification component is adjusted from 2 parts to 0.5 parts when preparing the two-stage curing polyurethane composite binder.

[0063] Comparative Example 1 This comparative example provides a polyurethane binder that does not contain interface-oriented reaction components or water-triggered secondary densification components.

[0064] This comparative example is almost identical to Example 1, except that no interface-oriented reaction component and water-triggered secondary densification component are added when preparing the two-stage curing polyurethane composite binder.

[0065] Comparative Example 2 This comparative example provides a polyurethane binder that does not contain water-triggered secondary densification components.

[0066] This comparative example is almost identical to Example 1, except that no water-triggered secondary densification component is added when preparing the two-stage curing polyurethane composite binder.

[0067] Comparative Example 3 This comparative example provides a polyurethane binder that does not contain interfacial directional reactive components.

[0068] This comparative example is almost identical to Example 1, except that no interfacial directional reaction component is added when preparing the two-stage curing polyurethane composite binder.

[0069] The polyurethane binders obtained in Examples 1-3 and Comparative Examples 1-3 were used to prepare permeable pavement structural layer specimens, including the following steps: First, the mineral aggregates were dried to constant weight at 105±5℃ and cooled to 25±2℃. They were then weighed and mixed uniformly according to the open gradation standard. The gradation composition was based on the PA-13 drainage asphalt mixture gradation range in the "Technical Specification for Design and Construction of Drainage Asphalt Pavement" (JTG / T 3350-03-2020). In this embodiment, the arithmetic mean value of the specified passing rate range for each sieve aperture was used. Subsequently, polyurethane binders prepared in Examples 1-3 and Comparative Examples 1-3 were added, with a binder-to-aggregate ratio of 5.2%. The mixtures were mechanically mixed at 25±2℃ for 60-90 seconds to ensure the binder evenly coats the surface of the mineral aggregates. The mixed materials were then placed into Marshall molds with an inner diameter of 101.6 mm and compacted 50 times on both sides at room temperature.

[0070] To verify the application effect of the proposed two-stage curing polyurethane composite binder in permeable pavement, specimens of the two-stage curing polyurethane composite binder and permeable pavement structural layer were prepared using the formulations and processes described in Examples 1-3 and Comparative Examples 1-3, respectively. The interfacial bonding performance, permeable structure retention performance and structural stability were then tested.

[0071] Among them, Comparative Example 1 is a conventional polyurethane bonding system without the interface-oriented reaction component and the water-triggered secondary densification component; Comparative Example 2 is a polyurethane bonding system containing only the interface-oriented reaction component and without the water-triggered secondary densification component; Comparative Example 3 is a polyurethane bonding system containing only the water-triggered secondary densification component and without the interface-oriented reaction component. Examples 1 to 3 all contain both the interface-oriented reaction component and the water-triggered secondary densification component. Example 1 is the basic example, Example 2 is used to illustrate the implementation effect when the interface-oriented reaction component is introduced by a pre-reaction modification method, and Example 3 is used to illustrate the implementation effect when the amount of the water-triggered secondary densification component is varied.

[0072] All specimens in each group were prepared using the same type of mineral aggregate, the same gradation range, the same molding size, and the same curing conditions. Unless otherwise specified, all specimens in each group were cured at 25℃ for 24 hours after molding before relevant performance tests were conducted. At least three specimens were prepared in parallel for each group, and the average value of the test results was taken.

[0073] Indicator 1: Interfacial adhesion performance Interfacial adhesion performance was evaluated using dry pull-out strength, wet pull-out strength, and wet retention rate, which characterize the interfacial adhesion ability of the binder in its initial state and its interfacial retention ability after exposure to water.

[0074] The dry pull-out strength is denoted as . Pull-out strength refers to the tensile strength of the specimen measured under standard curing conditions; wet pull-out strength is denoted as... The tensile strength refers to the tensile strength measured after the specimen has undergone a specified water treatment. The wet retention rate is calculated using the following formula:

[0075] in: The percentage of wetted water retention is %. Dry tensile strength (MPa); The wet pull-out strength (MPa) is given.

[0076] Indicator 2: Permeable structure retention performance The permeable structure retention performance is evaluated using the initial permeability coefficient, permeability retention rate, and interconnected porosity, which characterize the ability of the technical solution of the present invention to maintain the interconnected pore structure of the permeable skeleton while improving the interfacial bonding performance.

[0077] The initial permeability coefficient is denoted as . The permeability coefficient refers to the coefficient of permeability measured after the specimen has been cured; the permeability coefficient after water treatment is denoted as... The permeability coefficient refers to the coefficient of water permeability measured after the specimen has been treated with specified water.

[0078] The water retention rate is calculated using the following formula:

[0079] in: Permeability retention rate (%) The initial permeability coefficient (mm / s); The permeability coefficient (mm / s) after water action.

[0080] The interconnected void ratio was determined according to the vacuum sealing method specified in T0741-2025 of the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" JTG 3410-2025, and calculated using the following formula:

[0081] in: P c The porosity (%) of the specimen; m a The mass (g) of the dried specimen; m b The mass (g) of the sealed bag; m c The mass (g) in water for the sealed specimen and sealed bag; m cv The mass (g) in water for saturated specimens and open sealed bags. γ T This represents the relative density of the sealed bag at 25°C.

[0082] Indicator 3: Structural stability performance Structural stability was evaluated using the Cantabro scattering loss rate and the scattering loss rate after immersion in water, which characterizes the scattering resistance of the permeable skeleton structural layer and its structural stability after water exposure.

[0083] Wherein, the Cantabro scattering loss rate is denoted as The rate of loss due to scattering after immersion in water is recorded as follows: Both are in percentage.

[0084] The test results for indicators 1, 2, and 3 above are as follows: Figures 2-5 As shown. Test results indicate that, compared with conventional polyurethane bonding systems that do not contain interfacial directional reaction components and / or water-triggered secondary densification components, the two-stage curing polyurethane composite binder of the present invention exhibits better overall performance in terms of interfacial bonding properties, water permeability retention properties, and structural stability.

[0085] (1) By Figure 2 As can be seen, compared with Comparative Example 1, the dry pull-out strength, wet pull-out strength, and wet retention rate of Examples 1-3 are all improved, indicating that the technical solution of the present invention can improve the interfacial bonding state between polyurethane binder and mineral aggregate, and improve the interfacial retention capacity after water treatment. The results of Comparative Examples 2 and 3 show that introducing the interfacial directional reaction component alone or introducing the water-triggered secondary densification component alone can improve some interfacial properties; while Example 1, after introducing two functional components simultaneously, shows a better overall effect in interfacial bonding indicators. Although Examples 2 and 3 also achieved good results, they were not entirely superior to Example 1, indicating that Example 1 has a better overall balance in the technical solution of the present invention. It should be noted that, according to the dry pull-out strength σ... d With wet pull-out strength σ w In absolute terms, the improvement of Example 1 compared to Comparative Examples 2 and 3 exceeds the sum of the improvement of Comparative Examples 2 and 3 compared to Comparative Example 1. This means that the interface-oriented reaction component and the water-triggered secondary densification component exhibit synergistic effects on interfacial bonding performance. Furthermore, it is difficult to simultaneously achieve multiple objectives such as interfacial bonding, water permeability retention, and structural anti-scattering by introducing any single functional component alone. Only when both are used together can the above-mentioned comprehensive optimal effect be achieved, indicating that the effects of the two are not simply superimposed.

[0086] (2) By Figure 3 and Figure 4As can be seen, the initial permeability coefficient and interconnected porosity of each group of specimens remained within a relatively stable range, indicating that each group of specimens formed a permeable skeleton structure. Compared with Comparative Example 1, although the permeability coefficient and interconnected porosity of Examples 1-3 changed slightly, the permeability retention rate remained at a high level, indicating that the present invention does not achieve interface reinforcement and structural stability improvement by significantly sacrificing the permeable structure, but rather achieves local reinforcement while maintaining the basic interconnection of the permeable skeleton. Example 1, while maintaining a high permeability retention rate, also took into account improvements in interfacial bonding performance and structural stability.

[0087] (3) By Figure 5 As can be seen, compared with Comparative Example 1, the Cantabro scattering loss rate and the scattering loss rate after immersion in Examples 1-3 are significantly reduced, indicating that the present invention can improve the scattering resistance and structural stability of the open-graded skeleton structure layer after immersion. Although Comparative Examples 2 and 3 show improvements over Comparative Example 1, Example 1 has a better overall performance, indicating that the combined action of the interface-oriented reaction component and the water-triggered secondary densification component is more conducive to improving the overall stability of the permeable pavement structure layer.

[0088] In summary, the two-stage curing polyurethane composite binder of the present invention can improve the interfacial bonding state of the aggregate-binder and the stability of the structural layer after immersion in water, while maintaining the basic connectivity of the permeable skeleton structure. Examples 2 and 3 further demonstrate that the technical solution of the present invention is feasible under different introduction methods and different component dosages, indicating that the present invention has a good parameter applicability range.

[0089] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A two-stage curing polyurethane composite binder for permeable pavements, characterized in that, The components include the following parts by mass: 100 parts of polyurethane prepolymer; 1-5 parts of interfacial directional reaction component; 0.5–6 parts of water-triggered secondary densification component; Catalyst: 0.02–0.8 parts; Chain extender 1-10 parts; 5-60 parts of filler; Rheology modifier 0.1–3 parts; 0.1 to 2 parts of auxiliary agent; The polyurethane prepolymer is an isocyanate-containing prepolymer, and the content of the isocyanate groups is 10wt% to 18wt%. The interface-directed reaction component is a silane coupling agent containing both hydrolyzable silane groups and organic functional groups, wherein the organic functional groups are selected from at least one of amino and epoxy groups; The water-triggered secondary densification component is a microcapsule with a polyurea shell and a reactive isocyanate active component as the core material.

2. The two-stage curing polyurethane composite binder for permeable pavements according to claim 1, characterized in that, The interface-directed reaction component is selected from any one or a combination of two of γ-aminopropyltriethoxysilane and γ-(2,3-epoxypropoxy)propyltrimethoxysilane. When the interface-directed reaction component is composed of γ-aminopropyltriethoxysilane and γ-(2,3-epoxypropoxy)propyltrimethoxysilane, the mass ratio of γ-aminopropyltriethoxysilane to γ-(2,3-epoxypropoxy)propyltrimethoxysilane is 1:1 to 4:

1.

3. The two-stage curing polyurethane composite binder for permeable pavements according to claim 2, characterized in that, The polyurethane prepolymer was obtained using the following preparation method: The polyether diol was dehydrated to a moisture content of less than 0.05%; diphenylmethane diisocyanate was added under nitrogen protection and mechanical stirring, and the equivalent ratio of isocyanate groups to hydroxyl groups was controlled to be 3.8~4.2:1; the reaction was continued at 75~85℃ for 2~3 h, cooled and sealed for storage to obtain polyurethane prepolymer.

4. The two-stage curing polyurethane composite binder for permeable pavements according to claim 1, characterized in that, The water-triggered secondary densification component was obtained using the following preparation method: Isophorone diisocyanate and polymethylene polyphenyl polyisocyanate containing 30%–32% isocyanate groups were mixed at a mass ratio of 2.6–4.9:1 to obtain the oil phase; A composite emulsifier is obtained by mixing polyvinyl alcohol and gum arabic at a mass ratio of 0.9 to 3.5:

1. The composite emulsifier is then mixed with water to obtain an aqueous phase, wherein the total mass of the composite emulsifier is 2 to 5 wt% of the mass of the aqueous phase. The oil phase is slowly added to the water phase, and the mass ratio of the oil phase to the water phase is 12~20:

60. The mixture is emulsified at 5000~7000 rpm for 4~6 min at 0~5℃ to form an oil-in-water emulsion. A 2-3 wt% aqueous solution of diethylenetriamine is added dropwise to the oil-in-water emulsion, such that the mass ratio of the oil phase, aqueous phase, and DETA aqueous solution is 12-20:60:

60. The dropwise addition time is 15-20 min, allowing the amino groups in the diethylenetriamine aqueous solution to react with the isocyanate groups in the polymethylene polyphenyl polyisocyanate at the oil-water interface, forming a polyurea shell in situ. After the dropwise addition is completed, stirring is continued for 20-40 min, and then the temperature is increased to 60-65°C at a rate of 9-11°C / min, and the reaction is maintained at this temperature for 1.5-2.5 h. After the reaction was completed and cooled to room temperature, the microcapsules were obtained by centrifugation or filtration. They were then washed with deionized water and petroleum ether in sequence, and vacuum dried at 30–40 °C for 12–24 h to obtain the microencapsulated water-triggered secondary densification component.

5. The two-stage curing polyurethane composite binder for permeable pavements according to claim 1, characterized in that, The median particle size D50 of the microcapsules is 5–30 μm; The shell thickness of the microcapsule is 0.2–3 μm and does not exceed 1 / 4 of the median particle size D50 of the microcapsule volume. The core-to-wall mass ratio of the microcapsule is 1:1 to 50:

1.

6. The two-stage curing polyurethane composite binder for permeable pavements according to claim 1, characterized in that, The catalyst is an organic bismuth catalyst, the chain extender is 1,4-butanediol, the filler is a composite filler made of mineral powder and silica fume in a mass ratio of 3:1 to 5:1, the rheology modifier is fumed silica, and the additives are selected from at least one of stabilizers, antioxidants, ultraviolet absorbers, and defoamers.

7. A method for preparing a two-stage curing polyurethane composite binder for permeable pavements as described in any one of claims 1 to 6, characterized in that, Includes the following steps: A1. Add interfacial directional reaction components, catalysts, chain extenders, fillers, rheology modifiers, and additives to polyurethane prepolymers and mix to obtain a premixed binder; A2. Add water to the premixed binder obtained in step A1 to trigger the secondary densification component, and mix to obtain a two-stage curing polyurethane composite binder. or, B1. Add an interfacial directional reaction component to the polyurethane prepolymer and mix to obtain a pre-reactive modified polyurethane prepolymer; B2. Add water-triggered secondary densification components, catalysts, chain extenders, fillers, rheology modifiers, and additives to the pre-reactive modified polyurethane prepolymer obtained in step B1, and mix to obtain a two-stage curing polyurethane composite binder.

8. The method for preparing the two-stage curing polyurethane composite binder for permeable pavements according to claim 7, characterized in that, Step A1, the mixing conditions are: dispersion at 300-1200 rpm for 5-40 minutes at 20-60°C; Step A2: When the temperature of the premixed binder is 15-40°C, water is added to trigger a secondary densification component. The mixing conditions are: dispersion at a speed of 50-300 rpm for 2-15 minutes and a temperature of 25±2℃.

9. The method for preparing the two-stage curing polyurethane composite binder for permeable pavements according to claim 7, characterized in that, Step B1, the mixing conditions are: dispersion at a speed of 300-1200 rpm for 5-40 minutes, and a temperature of 20-60℃; Step B2 involves adding water-triggered secondary densification components, catalysts, chain extenders, fillers, rheology modifiers, and additives to the pre-reactive modified polyurethane prepolymer at a temperature of 15–40°C. The mixing conditions are: dispersion at a speed of 50-300 rpm for 2-15 minutes and a temperature of 25±2℃.

10. The application of the two-stage curing polyurethane composite binder as described in claim 1 in the preparation of a permeable pavement structural layer.