A bio-based dynamic vinyl polyurethane wood adhesive, and a preparation method and use thereof

By preparing a bio-based dynamic vinyl polyurethane wood adhesive, utilizing biomass resources such as epoxidized soybean oil, furan-2,5-dicarboxyhydrazide, and decanediamine, a thermally reversible crosslinking network and intrinsic fluorescence properties were constructed. This solved the environmental pollution and single-function problems of petroleum-based adhesives, and enabled multifunctional applications with high cohesive strength, reversible recyclability, and non-destructive testing.

CN123131973APending Publication Date: 2026-11-20INST OF CHEM IND OF FOREST PROD CHINESE ACAD OF FORESTRY +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611435256.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing petroleum-based wood adhesives suffer from dependence on fossil resources, environmental pollution caused by irreversible cross-linking networks, and difficulty in recycling the adhesive layer. Furthermore, traditional fluorescent adhesives have poor fluorescence stability, making it difficult to achieve multifunctional bonding, recyclability, and non-destructive testing.

Method used

Bio-based dynamic vinyl polyurethane wood adhesives were prepared using biomass resources such as epoxidized soybean oil, furan-2,5-dicarboxyhydrazide, and decanediamine. A thermally reversible crosslinking network was constructed through dynamic covalent bonds, and combined with intrinsic fluorescence properties, high cohesive strength, reversible recyclability, and non-destructive testing were achieved.

Benefits of technology

This adhesive achieves high interfacial toughness and bonding performance, can be recycled at high temperatures, and can be non-destructively tested using fluorescence properties, thus solving the problems of environmental pollution and limited functionality of traditional adhesives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123131973A_ABST
    Figure CN123131973A_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of wood adhesive, and particularly relates to a bio-based dynamic vinyl polyurethane wood adhesive, a preparation method and application thereof. The adhesive provided by the present application is prepared by the reaction of soybean oil-based acetoacetic ester, furan-2,5-diformyl hydrazine and sunflower diamine, and presents a micro-phase separation structure under an atomic force microscope. The adhesive provided by the present application has high cohesive strength, thermal reversibility, recyclability and intrinsic fluorescence characteristics, and can promote the green and low-carbon transformation of the wood processing industry and expand the application of the adhesive in the field of non-destructive testing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of wood adhesive technology, specifically relating to a bio-based dynamic vinyl polyurethane wood adhesive, its preparation method, and its uses. Background Technology

[0002] Wood adhesives are key raw and auxiliary materials in the engineered wood products and wood processing industries. Currently, petroleum-based aldehyde adhesives such as urea-formaldehyde resin, phenolic resin, and melamine-formaldehyde resin are widely used in industry. These adhesives rely on permanent covalent cross-linking networks to achieve high bonding strength, but they have inherent defects: on the one hand, the raw materials are highly dependent on fossil resources, which is contrary to the development concept of low-carbon manufacturing and circular economy; on the other hand, the cross-linking network is irreversible after curing, and the adhesive layer is difficult to degrade and recycle. At the same time, there is a formaldehyde release problem, which will cause environmental pollution and harm human health.

[0003] Epoxidized soybean oil, as a renewable green resource, can be chemically modified through ring-opening alcoholysis and transesterification to introduce active functional groups such as hydroxyl groups and acetoacetate esters, making it an ideal matrix raw material for preparing bio-based adhesives. Furan-2,5-dicarboxyhydrazide, derived from furanyl dicarboxylic acid, is a typical biomass platform compound. Its molecule possesses a rigid furan aromatic ring structure, providing multiple amino reaction sites for dynamic covalent bond construction and introducing rigid structural units. Through intermolecular hydrogen bonding, it promotes hard segment aggregation and enhances the cohesive strength of the adhesive. Decanediamine, a long-chain aliphatic bio-based diamine, can introduce flexible segments into the polymer network, effectively regulating the toughness of the adhesive and alleviating the brittleness problem caused by the rigid structure. Modifying and reacting epoxidized soybean oil, furan-2,5-dicarboxyhydrazide, and decanediamine can synergistically achieve the regulation of soft and hard segments; however, current technologies have not yet fully realized the efficient synergistic utilization of these three types of biomass raw materials.

[0004] Dynamic covalent chemistry offers a new approach to developing recyclable adhesives. Vinyl polyurethane dynamic bonds can be constructed without a catalyst through the condensation reaction of β-acetoacetate and primary amines. Under thermal stimulation, amine exchange reactions occur, achieving topological rearrangement of the cross-linked network and endowing the material with thermally reversible and reprocessable properties. Simultaneously, this structure contains numerous hydrogen bond donors and acceptors, which can induce hard segment aggregation, construct a microphase-separated structure, and enhance the material's cohesive properties. However, current bio-based wood adhesives based on vinyl dynamic bonds still face many unresolved issues: most systems struggle to balance excellent interfacial adhesion and intrinsic cohesive strength, exhibiting a trade-off between adhesive strength and reversible recyclability. An imbalance in the ratio of hard to soft segments can easily lead to an overly brittle adhesive layer or insufficient cohesion, failing to meet national standards for engineered wood products. Furthermore, traditional adhesives only perform bonding functions, offering limited functionality. During wood processing, defects in the adhesive layer, internal cracks in the substrate, and hidden damage at the bonding interface are difficult to identify visually, and non-destructive testing methods are costly and complex. Most existing fluorescent adhesives rely on the addition of exogenous fluorescent small-molecule dyes to achieve luminescence. However, the exogenous fluorescent groups have poor compatibility with the polymer matrix, are prone to migration and precipitation, and exhibit poor fluorescence stability, limiting their practical application. Intrinsically luminescent polymers, on the other hand, generate fluorescence through cluster aggregation-induced fluorescence, without the need for additional fluorescent dye doping. Introducing intrinsic fluorescence properties into dynamic bio-based adhesives can achieve multiple functions, including bonding, recyclability, and defect visualization detection. However, the molecular design and preparation technology for such multifunctional bio-based wood adhesives remains relatively scarce.

[0005] For example, Chinese patent CN107474785A discloses an environmentally friendly soybean oil-based polyurethane adhesive for wood. This adhesive can be cured at room temperature and humidity and has good bonding performance in the field of wood adhesives. However, this invention still has the aforementioned problems.

[0006] Therefore, there is an urgent need to develop a bio-based dynamic vinyl polyurethane wood adhesive that uses soybean oil, furan-2,5-dicarboxyhydrazide, decanediamine, and other biomass resources as raw materials, and that combines high cohesive strength, thermal reversibility and recyclability, and intrinsic fluorescence properties, in order to promote the green and low-carbon transformation of the wood processing industry and expand the application of adhesives in the field of non-destructive testing. Summary of the Invention

[0007] In view of the shortcomings of the prior art, the purpose of this invention is to provide a bio-based dynamic vinyl polyurethane wood adhesive, its preparation method and uses.

[0008] Terminology Explanation:

[0009] Unless otherwise defined, all technical terms in this document have the same meanings as commonly understood by one of ordinary skill in the art to which the subject matter of the claims pertains. Unless otherwise stated, all patents, patent inventions, and publications cited in this document are incorporated herein by reference in their entirety. If multiple definitions exist for terms in this document, the definitions in this chapter shall prevail.

[0010] It should be understood that the above brief description and the following detailed description are exemplary and for illustrative purposes only, and do not limit the subject matter of the invention in any way. In this invention, the singular is used in conjunction with the plural unless otherwise specifically stated. It should also be noted that, unless otherwise stated, the use of “or” or “or” means “and / or”. Furthermore, the use of the term “comprising” and other forms such as “including,” “containing,” and “contains” are not limiting.

[0011] Unless specifically defined herein, the use of all commercially available products herein employs standard techniques. For example, it may be carried out using the manufacturer's instructions for use with the kit, or in accordance with methods known in the art or the description of this invention. The techniques and methods described herein can generally be implemented according to conventional methods well known in the art, based on the descriptions in the various summary and more specific documents cited and discussed in this specification.

[0012] To achieve the above objectives, the present invention adopts the following technical solution:

[0013] In a first aspect, the present invention provides a bio-based dynamic vinyl polyurethane wood adhesive, said wood adhesive comprising the structure shown in formula (I):

[0014] (I)

[0015] In equation (Ⅰ), R1 is: or ;

[0016] In equation (Ⅰ), R2 is: .

[0017] Preferably, the adhesive exhibits a microphase separation structure under an atomic force microscope.

[0018] Secondly, the present invention provides a method for preparing a bio-based dynamic vinyl polyurethane wood adhesive, the method comprising the following steps:

[0019] S1. Preparation of soybean oil-based polyols: Epoxidized soybean oil and methanol undergo a ring-opening addition reaction under Lewis acid catalysis to obtain soybean oil-based polyols;

[0020] S2. Preparation of soybean oil-based polyether polyol: Soybean oil-based polyether polyol and propylene oxide undergo a ring-opening grafting reaction under Lewis base catalysis to obtain soybean oil-based polyether polyol.

[0021] S3. Preparation of soybean oil-based acetoacetate: Soybean oil-based polyether polyol is condensed with tert-butyl acetoacetate to obtain soybean oil-based acetoacetate;

[0022] S4. Preparation of bio-based dynamic vinyl polyurethane adhesive: Soybean oil-based acetoacetate, furan-2,5-dicarboxyhydrazide and decanediamine are reacted to prepare bio-based dynamic vinyl polyurethane wood adhesive.

[0023] Preferably, the reaction temperature in step S1 is 75~110℃, the reaction time is 30~60 min, the mass ratio of epoxidized soybean oil to methanol is 1:(0.1~0.5), and the Lewis acid is selected from any one of fluoroboric acid, boron trifluoride, aluminum trichloride, zinc chloride, and trimethylaluminum.

[0024] More preferably, the reaction temperature in step S1 is 75°C, the reaction time is 30 min, the mass ratio of epoxidized soybean oil to methanol is 1:0.36, and the Lewis acid is fluoroboric acid.

[0025] Preferably, the reaction temperature in step S2 is 120~140℃, the pressure is 0.5~1.3MPa, the reaction time is 4~6h, the mass ratio of soybean oil-based polyol to propylene oxide is 1:(0.6~0.8), and the Lewis base is selected from at least one of potassium hydroxide, tetrabutylammonium bromide, triethylamine, and dimethyl sulfide.

[0026] More preferably, the reaction temperature in step S2 is 130°C, the pressure is 0.8 MPa, the reaction time is 6 h, the mass ratio of soybean oil-based polyol to propylene oxide is 1:0.69, and the Lewis base is potassium hydroxide and triethylamine, with a mass ratio of 3:1.

[0027] Preferably, the reaction temperature in step S3 is 130~160℃, the reaction time is 4~6h, and the mass ratio of soybean oil-based polyether polyol to tert-butyl acetoacetate is 1:(1.2~1.4).

[0028] More preferably, the reaction temperature in step S3 is 150°C, the reaction time is 5 hours, and the mass ratio of soybean oil-based polyether polyol to tert-butyl acetoacetate is 1:1.26.

[0029] Preferably, the reaction described in step S4 is stirred and mixed at room temperature, and then heated to polymerize at a temperature of 40-60°C; the mass ratio of soybean oil-based acetoacetate to decanediamine is 2:(0.3~0.6).

[0030] More preferably, the mass ratio of soybean oil-based acetoacetate to decanediamine in step S4 is 2:0.5, and the heating temperature is 50°C.

[0031] Preferably, the amount of furan-2,5-dicarboxyhydrazide added in step S4 is 0-28% of the adhesive system.

[0032] More preferably, the amount of furan-2,5-dicarboxyhydrazide added in step S4 is 7-21% of the adhesive system.

[0033] More preferably, the amount of furan-2,5-dicarboxyhydrazide added in step S4 is 21% of the adhesive system.

[0034] Thirdly, the present invention also provides the application of the above-mentioned bio-based dynamic vinyl polyurethane wood adhesive as a wood adhesive.

[0035] The present invention provides a method for disassembling and recycling adhesives based on vinyl dynamic bonds at high temperatures, enabling the reuse of wood adhesives.

[0036] The bio-based dynamic vinyl polyurethane wood adhesive provided by this invention can be excited to produce yellow fluorescence under a 365nm ultraviolet lamp, and can be used for the detection of wood defects.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] (1) This invention provides a bio-based dynamic vinyl polyurethane wood adhesive with high cohesive strength and high interfacial toughness. By adjusting the content of the rigid furan segment and the flexible decanediamine segment, the microphase separation structure is precisely controlled. The rigid furan ring increases the stiffness of the polymer, while the flexible polyether chain and aliphatic chain release mechanical stress through hydrogen bond breaking and flexible chain elongation, thereby improving the overall cohesive strength of the adhesive. At the same time, the urethane group forms strong hydrogen bonds with the hydroxyl group on the substrate, thereby enhancing the interfacial adhesion. Meanwhile, the adhesive can effectively penetrate into the porous channels of the substrate to form a mechanically locked structure, further improving the interfacial toughness of the adhesive, and ultimately achieving strong bonding performance of the adhesive.

[0039] (2) Dynamic vinyl polyurethane bonds are activated at high temperatures, resulting in the breaking of dynamic bonds and the generation of free carbonyl and amino functional groups. The polymer transforms from a solid state to a fluid state. Upon cooling to room temperature, hydrogen bonds and dynamic bonds are rebuilt, and the adhesive returns to a solid state. The newly formed hydrogen bonds synergistically enhance the interfacial bonding strength with the dynamic covalent bonds of vinyl urea, thereby restoring the original excellent adhesive properties. This dynamic change process enables the recycling of the adhesive.

[0040] (3) The vinyl polyurethane group contains abundant electron donors and unsaturated bonds. Among them, the NH bond is combined with the adjacent carbonyl group through intramolecular hydrogen bonding, which restricts the rotation and vibration of the molecule, thereby forming a stable six-membered heterocyclic structure. Therefore, the adhesive relies on the cluster aggregation-induced emission effect to generate fluorescence without the need for additional doping with fluorescent dyes. The fluorescence properties of the adhesive can enable non-destructive testing of the bonded materials. Attached Figure Description

[0041] Figure 1 The NMR spectrum of the synthesis of soybean oil-based polyols;

[0042] Figure 2 The NMR spectrum of the synthesis of soybean oil-based polyether polyol;

[0043] Figure 3 The NMR spectrum of the synthesis of soybean oil acetyl acetate;

[0044] Figure 4 Infrared spectrum of the synthesis of bio-based dynamic vinyl polyurethane wood adhesive;

[0045] Figure 5 Images are shown in the scanning electron microscope (SEM) and atomic force microscope (AFM) images. Figure 5 Scanning electron microscope image of bio-based dynamic vinyl polyurethane wood adhesive in Example 4. Figure 5 Atomic force microscopy image of bio-based dynamic vinyl polyurethane wood adhesive;

[0046] Figure 6 Shear strength of plywood prepared with bio-based dynamic vinyl polyurethane wood adhesives with different furan-2,5-dicarboxyhydrazide contents;

[0047] Figure 7 The image shows the shear strength of the wood board bonded with the adhesive prepared in Example 4 after 4 cycles of heating, debonding, and rebonding.

[0048] Figure 8 Fluorescence intensity diagrams of bio-based dynamic vinyl polyurethane wood adhesives with different furan-2,5-dicarboxyhydrazide contents;

[0049] Figure 9 The adhesive prepared in Example 4 was tested for bonding defects in plywood under sunlight and UV light irradiation.

[0050] Figure 10 Shear strength of plywood prepared with different proportions of adhesives. Detailed Implementation

[0051] To make the above-mentioned objects, embodiments, features and advantages of the present invention more apparent and understandable, the present invention will be described in detail below with reference to embodiments.

[0052] The following detailed embodiments provide numerous specific technical details to facilitate a thorough understanding and implementation of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Those skilled in the art can make similar extensions, substitutions, or transformations without departing from the essence and basic principles of the present invention, such as equivalent substitutions of similar catalysts, solvents, etc. Therefore, the present invention is not limited to the following specific embodiments.

[0053] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.

[0054] The epoxidized soybean oil (analytical grade, epoxy value = 0.52~0.63), fluoroboric acid (analytical grade, >50%), potassium hydroxide (analytical grade, >99%), and triethylamine (analytical grade, >90%) mentioned in the following specific embodiments are from Shanghai Maclean's Co., Ltd. Furan-2,5-dicarboxyhydrazide (analytical grade, >99%), decanediamine (analytical grade, >99%), tert-butyl acetoacetate, 1,5-pentanediamine, and adipate dihydrazide are from Shanghai Aladdin Co., Ltd. Propylene oxide is from Nanjing Jinling Petrochemical Co., Ltd., and methanol is from Nanjing Chemical Reagent Co., Ltd.

[0055] Example 1: A bio-based dynamic vinyl polyurethane wood adhesive and its preparation method

[0056] The preparation method of this bio-based dynamic vinyl polyurethane wood adhesive is as follows:

[0057] (1) 100g of epoxidized soybean oil was dissolved in 36 mL of methanol, and then 0.98g of fluoroboric acid solution was slowly added as a catalyst. The mixture was stirred and heated to 75℃ for 30 min. After the reaction, the mixture was neutralized with potassium hydroxide, and then extracted with ethyl acetate. The organic phase was washed three times with water, and then the ethyl acetate was removed by vacuum distillation to obtain a dark brown viscous soybean oil-based polyol. Figure 1 The 1H-NMR of soybean oil-based polyols showed that the epoxy groups at 3.0~3.5 ppm disappeared, and a hydroxyl peak appeared at 2.0~2.5 ppm.

[0058] (2) 150g of soybean oil-based polyol, 0.63g of potassium hydroxide, and 0.21g of triethylamine were added to a 250mL high-pressure reactor. After mixing and stirring evenly, the reactor was brought to negative pressure, and propylene oxide was added dropwise to 104.54g. The reaction was carried out at 130°C for 6 hours at a pressure of 0.8MPa until the pressure inside the reactor no longer changed. The reaction was stopped, and excess propylene oxide was removed by vacuum filtration. The mixture was then extracted with ethyl acetate, and the organic phase was washed three times with water to remove the catalyst. Ethyl acetate was removed by vacuum filtration to obtain a golden-yellow viscous soybean oil-based polyether polyol. Figure 2 The 1H-NMR of soybean oil-based polyether polyols showed primary hydroxyl groups at 4.5–5.2 ppm and methyl groups from propylene oxide ring-opening grafting at 0–1.5 ppm.

[0059] (3) 253.12 g of soybean oil-based polyether polyol was dissolved in 320 g of tert-butyl acetoacetate. The reaction temperature was raised to 150°C and refluxed for 5 hours. After the reaction was completed, excess tert-butyl acetoacetate was removed by rotary evaporation under reduced pressure, and the product was dried in a vacuum oven at 100°C to obtain a golden-yellow viscous soybean oil-based acetoacetate. Figure 3 The 1H-NMR of soybean oil-based acetoacetate shows acetoacetate groups at a range of 1 to 1.5 ppm.

[0060] (4) Stir 2g of soybean oil-based acetoacetate and 0.5g of decanediamine at high speed until homogeneous, then pour into an 80×80 mm container. 2 Bio-based dynamic vinyl polyurethane wood adhesive was prepared by high-temperature polymerization at 50°C in a Teflon mold.

[0061] Example 2: A bio-based dynamic vinyl polyurethane wood adhesive and its preparation method

[0062] This embodiment provides a method for preparing a bio-based dynamic vinyl polyurethane wood adhesive, which differs from Example 1 in step (4): 2g of soybean oil-based acetoacetate, 0.5g of decanediamine and 0.19g of furan-2,5-dicarboxyhydrazide are stirred at high speed until homogeneous, and then poured into an 80×80 mm... 2 A bio-based dynamic vinyl polyurethane wood adhesive was prepared by high-temperature polymerization at 50°C in a Teflon mold. The mass of furan-2,5-dicarboxyhydrazide in the adhesive system was 7%. Figure 4 The infrared spectrum of the bio-based dynamic vinyl polyurethane wood adhesive is visible at 1603.03 cm⁻¹. -1 1731.76 cm -1 and 3328.53 cm -1The infrared absorption peaks are attributed to C, C=O, and NH in the urethane bonds, respectively. Therefore, furan-2,5-dicarboxyhydrazide, soybean oil-based acetoacetate, and decanediamine react to form a vinyl polyurethane structure.

[0063] Example 3: A bio-based dynamic vinyl polyurethane wood adhesive and its preparation method

[0064] This embodiment provides a method for preparing a bio-based dynamic vinyl polyurethane wood adhesive, which differs from Example 1 in step (4): 2g of soybean oil-based acetoacetate, 0.5g of decanediamine and 0.41g of furan-2,5-dicarboxyhydrazide are stirred at high speed until homogeneous, and then poured into an 80×80 mm... 2 Bio-based dynamic vinyl polyurethane wood adhesive was prepared by high-temperature polymerization at 50°C in a Teflon mold. The mass of furan-2,5-dicarboxyhydrazide in the adhesive system was 14%.

[0065] Example 4: A bio-based dynamic vinyl polyurethane wood adhesive and its preparation method

[0066] This embodiment provides a method for preparing a bio-based dynamic vinyl polyurethane wood adhesive, which differs from Example 1 in step (4): 2g of soybean oil-based acetoacetate, 0.5g of decanediamine and 0.66g of furan-2,5-dicarboxyhydrazide are stirred at high speed until homogeneous, and then poured into an 80×80 mm... 2 Bio-based dynamic vinyl polyurethane wood adhesive was prepared by high-temperature polymerization at 50°C in a Teflon mold. The mass of furan-2,5-dicarboxyhydrazide in the adhesive system was 21%.

[0067] like Figure 5 As shown, when furan-2,5-dicarboxyhydrazide is further added to 21%, this embodiment prepares a bio-based dynamic vinyl polyurethane wood adhesive with an island structure. Figure 5 a). Atomic force microscopy revealed that the adhesive possessed a uniform microphase separation structure.

[0068] Example 5: A bio-based dynamic vinyl polyurethane wood adhesive and its preparation method

[0069] This embodiment provides a method for preparing a bio-based dynamic vinyl polyurethane wood adhesive, which differs from Example 1 in step (4): 2g of soybean oil-based acetoacetate, 0.5g of decanediamine and 0.97g of furan-2,5-dicarboxyhydrazide are stirred at high speed until homogeneous, and then poured into an 80×80 mm... 2 Bio-based dynamic vinyl polyurethane wood adhesive was prepared by high-temperature polymerization at 50°C in a Teflon mold. The mass of furan-2,5-dicarboxyhydrazide in the adhesive system was 28%.

[0070] Example 6: Adhesion performance of a bio-based dynamic vinyl polyurethane wood adhesive for eucalyptus veneer

[0071] The bio-based dynamic vinyl polyurethane wood adhesives prepared in Examples 1, 2, 3, 4, and 5 were applied to eucalyptus veneers through a process of "coating → pre-pressing → hot pressing" to obtain three-layer eucalyptus plywood. The preparation process of the three-layer eucalyptus plywood was as follows: the three eucalyptus veneers consisted of an upper layer, a lower layer, and a core layer. The bio-based dynamic vinyl polyurethane wood adhesive was applied to both sides of the core layer, while the upper and lower layers were coated on only one side, with an adhesive application rate of 180 g / m². 2 Then, the coated upper layer, core layer, and lower layer are assembled along the direction perpendicular to the wood grain. The mixture is then subjected to room temperature cold pressing (1.0 MPa, 2 h) on a flat vulcanizing machine; followed by hot pressing at 120 °C (1.0 MPa, 405 s); finally, it is cooled to room temperature to obtain eucalyptus plywood.

[0072] The bonding strength and other mechanical properties of the plywood were tested according to the test methods for Class II plywood in GB / T 9846-2015 "Ordinary Plywood".

[0073] like Figure 6 It is observed that the shear strength of plywood gradually increases with the increasing content of furan-2,5-dicarboxyhydrazide. This improvement is mainly attributed to the enhanced bonding performance of the hard phase domains (composed of furan rings) within the soft-chain matrix (composed of polyether and aliphatic chains). Furthermore, the hydrogen bonds between the soft and hard phases also act as sacrificial bonds, dissipating energy during tensile deformation and thus improving adhesion. The optimal adhesion performance occurs at a furan-2,5-dicarboxyhydrazide content of 21%. At this composition, the shear strength of the wood reaches 2.41 MPa. When the furan-2,5-dicarboxyhydrazide content further increases to 28%, the adhesion performance significantly decreases. This decrease is attributed to brittle fracture caused by stress concentration due to excessive aggregation of the hard segments.

[0074] Example 7

[0075] A eucalyptus plywood was prepared using the adhesive obtained in Example 4 and the preparation method in Example 6. The plywood was then debonded, and its shear strength was tested, repeated four times. Figure 7 As shown, the shear strength remained above 95% of its initial value. This is mainly attributed to the activation and breakage of dynamic vinyl polyurethane bonds at high temperatures, resulting in the formation of free carbonyl and amino functional groups. After the reconstituted plywood was cooled to room temperature, hydrogen bonds and dynamic bonds were rebuilt, and the adhesive returned to a solid state. The reformed hydrogen bonds synergistically enhanced the interfacial bonding strength with the dynamic covalent bonds of vinyl urea, thereby restoring the original excellent adhesive properties. This dynamic process enabled the recycling of the adhesive.

[0076] Example 8: Testing of Fluorescence Properties of Bio-based Dynamic Vinyl Polyurethane Wood Adhesive

[0077] The adhesives prepared in Examples 1-5 were cured to obtain an adhesive strip, and then the fluorescence intensity of the sample was tested under 365nm ultraviolet light excitation. Figure 8 As shown, with the continuous increase of furan-2,5-dicarboxyhydrazide content, the fluorescence intensity and emission wavelength of the cured bio-based dynamic vinyl polyurethane wood adhesive strips gradually increased, reaching their maximum at a furan-2,5-dicarboxyhydrazide content of 21% (Example 4). Figure 9 As shown, compared with sunlight, the location of bonding defects is easily detected under UV light. Therefore, the fluorescent properties of adhesives provide the possibility for non-destructive testing of wood bonding.

[0078] Comparative Example 1

[0079] The difference from Example 4 is as follows: Step (4): 1g of soybean oil-based acetoacetate, 0.5g of decanediamine and 0.66g of furan-2,5-dicarboxyhydrazide are stirred evenly at high speed, and then poured into an 80×80 mm container. 2 Bio-based dynamic vinyl polyurethane wood adhesive was prepared by high-temperature polymerization at 50°C in a Teflon mold.

[0080] Comparative Example 2

[0081] The difference from Example 4 is as follows: Step (4): 2g of soybean oil-based acetoacetate, 0.2g of decanediamine and 0.66g of furan-2,5-dicarboxyhydrazide are stirred evenly at high speed, and then poured into an 80×80 mm container. 2 Bio-based dynamic vinyl polyurethane wood adhesive was prepared by high-temperature polymerization at 50°C in a Teflon mold.

[0082] Comparative Example 3

[0083] The difference from Example 4 is as follows: Step (4): 2g of soybean oil-based acetoacetate, 0.5g of 1,5-pentanediamine and 0.66g of furan-2,5-dicarboxyhydrazide are stirred evenly at high speed, and then poured into an 80×80 mm container. 2 Bio-based dynamic vinyl polyurethane wood adhesive was prepared by high-temperature polymerization at 50°C in a Teflon mold.

[0084] Comparative Example 4

[0085] The difference from Example 4 is as follows: Step (4): 2g of soybean oil-based acetoacetate, 0.5g of decanediamine and 0.66g of adipic acid dihydrazide are stirred evenly at high speed, and then poured into an 80×80 mm container. 2 Bio-based dynamic vinyl polyurethane wood adhesive was prepared by high-temperature polymerization at 50°C in a Teflon mold.

[0086] The adhesives prepared in Comparative Examples 1-4 were used to prepare a three-layer eucalyptus plywood according to the method in Example 6. The plywood was then heated to de-adhere and its shear strength was tested. This process was repeated 4 times.

[0087] Depend on Figure 10 It can be seen that the bonding performance of the wood in Comparative Examples 1-4 is lower than that in Example 4, thus proving that Example 4 is the optimal formulation.

[0088] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, and is not intended to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions made by those skilled in the art to the technical solution of the present invention do not depart from the essence and scope of the technical solution of the present invention.

Claims

1. A bio-based dynamic vinyl polyurethane wood adhesive, characterized in that, The wood adhesive contains the structure shown in formula (I): (Ⅰ); In equation (Ⅰ), R1 is: or ; In equation (Ⅰ), R2 is: .

2. The bio-based dynamic vinyl polyurethane wood adhesive according to claim 1, characterized in that, The wood adhesive exhibits a microphase separation structure under an atomic force microscope.

3. The method for preparing the bio-based dynamic vinyl polyurethane wood adhesive according to any one of claims 1-2, characterized in that, The preparation method includes the following steps: S1. Preparation of soybean oil-based polyols: Epoxidized soybean oil and methanol undergo a ring-opening addition reaction under Lewis acid catalysis to obtain soybean oil-based polyols; S2. Preparation of soybean oil-based polyether polyol: Soybean oil-based polyether polyol and propylene oxide undergo a ring-opening grafting reaction under Lewis base catalysis to obtain soybean oil-based polyether polyol. S3. Preparation of soybean oil-based acetoacetate: Soybean oil-based polyether polyol is condensed with tert-butyl acetoacetate to obtain soybean oil-based acetoacetate; S4. Preparation of bio-based dynamic vinyl polyurethane adhesive: Soybean oil-based acetoacetate, furan-2,5-dicarboxyhydrazide and decanediamine are reacted to prepare bio-based dynamic vinyl polyurethane wood adhesive.

4. The preparation method according to claim 3, characterized in that, The reaction temperature in step S1 is 75~110℃, the reaction time is 30~60 min, the mass ratio of epoxidized soybean oil to methanol is 1:(0.1~0.5), and the Lewis acid is selected from any one of fluoroboric acid, boron trifluoride, aluminum trichloride, zinc chloride, and trimethylaluminum.

5. The preparation method according to claim 3, characterized in that, The reaction temperature in step S2 is 120~140℃, the pressure is 0.5~1.3MPa, the reaction time is 4~6 h, the mass ratio of soybean oil-based polyol to propylene oxide is 1:(0.6~0.8), and the Lewis base is selected from at least one of potassium hydroxide, tetrabutylammonium bromide, triethylamine, and dimethyl sulfide.

6. The preparation method according to claim 3, characterized in that, The reaction temperature in step S3 is 130~160℃, the reaction time is 4~6 h, and the mass ratio of soybean oil-based polyether polyol to tert-butyl acetoacetate is 1:(1.2~1.4).

7. The preparation method according to claim 3, characterized in that, The reaction described in step S4 is stirred and mixed at room temperature and then heated for polymerization; the mass ratio of soybean oil-based acetoacetate to decanediamine is 2:(0.3~0.6).

8. The preparation method according to claim 3, characterized in that, The amount of furan-2,5-dicarboxyhydrazide added in step S4 accounts for 0-28% of the adhesive system.

9. The use of the bio-based dynamic vinyl polyurethane wood adhesive according to any one of claims 1-2 or the bio-based dynamic vinyl polyurethane wood adhesive prepared by the preparation method according to any one of claims 3-8 as an adhesive.

10. The application according to claim 9, characterized in that, The bio-based dynamic vinyl polyurethane wood adhesive can be excited to produce yellow fluorescence under a 365nm ultraviolet lamp, and can be used for the detection of wood defects.

Citation Information

Patent Citations

  • Environment-friendly soybean oil-based moisture-cured polyurethane wood adhesive

    CN107474785A