High-adhesion anti-aging silicone adhesive and preparation process thereof

By using a process to prepare highly adhesive and anti-aging silicone sealant, a combination of polysiloxane coupling agents and hindered amine-based p-aminodiphenylamine compounds was employed to solve the problems of poor adhesion and aging of silicone sealant on low surface energy substrates, achieving stable adhesion and long-lasting sealing under extreme environments.

CN123131978APending Publication Date: 2026-11-20LIANZHOU KAIRUN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611198195.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-07
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing silicone sealants have poor adhesion on low surface energy or inert substrates and are prone to aging in extreme environments, leading to adhesion failure and mortar powdering, making it difficult to meet the requirements for long-term sealing.

Method used

A combination of hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil, nano-calcium carbonate, fumed silica, No. 5 white oil, stannous octoate, polysiloxane coupling agent, and hindered aminodiphenylamine compound was used to prepare a highly adhesive and anti-aging silicone adhesive by stirring and mixing. The polysiloxane coupling agent was used to improve the bonding performance, and the hindered aminodiphenylamine compound was used to improve the anti-aging performance.

Benefits of technology

The prepared silicone adhesive exhibits excellent adhesion on a variety of substrates and remains stable under long-term erosion from heat, oxygen, and ultraviolet radiation, thus extending its service life and preventing adhesive failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present application relates to the field of silicone glue, in particular to a high-adhesion anti-aging silicone glue and a preparation process thereof, which is used to solve the problem of poor adhesion and anti-aging performance of the existing silicone glue; the silicone glue comprises the following components: hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil, nano calcium carbonate, fumed white carbon black, 5# white oil, stannous octoate, polysiloxane coupling agent and hindered amine-based p-aminodiphenylamine compound; the preparation process improves the adhesion and mechanical properties of the silicone glue by adding the polysiloxane coupling agent, and the anti-aging performance of the silicone glue is improved after adding the hindered amine-based p-aminodiphenylamine compound, so that the prepared silicone glue has a wide range of applications and exhibits excellent adhesion to various substrates, and the adhesion state does not significantly decay under long-term erosion of heat, oxygen, ultraviolet and the like, which can effectively prevent adhesion failure and prolong the service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of silicone sealants, specifically to a high-adhesion, anti-aging silicone sealant and its preparation process. Background Technology

[0002] Silicone sealant is a key adhesive and sealant material in building curtain walls, photovoltaic modules, and electronic packaging, and its performance directly determines the reliability and lifespan of the end products. However, as application scenarios become more extreme and diversified, the technical shortcomings of traditional silicone sealants are becoming increasingly apparent.

[0003] Existing silicone sealants have poor bonding performance. When facing low surface energy or inert substrates such as glass, stainless steel, and engineering plastics, they are difficult to form strong chemical bonds. Furthermore, they are prone to aging under long-term light exposure, oxidation, and high temperature environments, leading to bonding failure and mortar powdering, making it difficult to meet the long-term sealing requirements under harsh working conditions.

[0004] Therefore, developing a highly adhesive and anti-aging silicone sealant and its preparation process is of great practical significance. Summary of the Invention

[0005] In order to overcome the above-mentioned technical problems, the purpose of this invention is to provide a silicone sealant with high adhesion and anti-aging properties and its preparation process, which solves the problem of poor adhesion and anti-aging properties of existing silicone sealants.

[0006] The objective of this invention can be achieved through the following technical solutions: In a first aspect, this application provides a highly adhesive and anti-aging silicone adhesive, comprising the following components in parts by weight: Hydroxyl-terminated polydimethylsiloxane 30-35 parts, dimethyl silicone oil 5-9 parts, nano-calcium carbonate 55-60 parts, fumed silica 3-7 parts, No. 5 white oil 4.5-6.5 parts, stannous octoate 0.08-0.12 parts, polysiloxane coupling agent 1.2-2.6 parts, and hindered amino group p-aminodiphenylamine compound 0.8-1.6 parts; The polysiloxane coupling agent is prepared by the following steps: Step a1: Add octamethylcyclotetrasiloxane and tetramethylammonium hydroxide to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir the reaction at 20-25℃ and 300-400 r / min for 30-50 min. Then raise the temperature to 110-120℃ and continue stirring for 4-6 h. After the reaction is completed, cool the reaction product to room temperature to obtain tetramethylammonium hydroxide silanolate. Step a2: Add octamethylcyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir for 20-30 min at 20-25℃ and 300-400 r / min. Then add tetramethylammonium hydroxide silanolate and tetramethyldivinyldisiloxane and continue stirring for 20-30 min. Then raise the temperature to 100-105℃ and continue stirring for 4-5 h. Then raise the temperature to 140-150℃ and continue stirring for 1-2 h. Then raise the temperature to 180-200℃ and continue stirring for 20-30 min. After the reaction is complete, cool the reaction product to room temperature to obtain polyene silicone oil. Step a3: Add polyene silicone oil, triethoxysilane, platinum (O)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane solution and n-hexane to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection. Stir the reaction at 20-25℃ and 300-400 r / min for 20-30 min. Then raise the temperature to 70-75℃ and continue stirring for 8-10 h. Then raise the temperature to 90-95℃ and continue stirring for 1-2 h. After the reaction is completed, cool the reaction product to room temperature and then remove the solvent by rotary evaporation to obtain the polysiloxane coupling agent.

[0007] In a preferred embodiment of the present invention, the ratio of octamethylcyclotetrasiloxane to tetramethylammonium hydroxide in step a1 is 20g:0.4g.

[0008] In a preferred embodiment of the present invention, the ratio of the amounts of octamethylcyclotetrasiloxane, tetramethyltetravinylcyclotetrasiloxane, tetramethylammonium hydroxide silanolate, and tetramethyldivinyldisiloxane in step a2 is 40-45g: 35-45g: 0.02-0.04g: 0.1-0.2g.

[0009] In a preferred embodiment of the present invention, the ratio of polyene silicone oil, triethoxysilane, platinum(O)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane solution and n-hexane in step a3 is 20-25g: 1-5g: 0.1-0.2mL: 60-70mL.

[0010] In a preferred embodiment of the present invention, the hindered amino group p-aminodiphenylamine compound is prepared by the following steps: Step b1: 3,4-epoxycyclohexyl methacrylate, p-aminodiphenylamine, and hexafluoroisopropanol were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Nitrogen gas was introduced for protection. The mixture was stirred and reacted for 20-30 min at a temperature of 20-25℃ and a stirring rate of 300-400 r / min. Then, the temperature was raised to 120-125℃ and the reaction was continued for 20-30 h. After the reaction was completed, the reaction product was cooled to room temperature and then washed 2-3 times with n-heptane and chloroform in sequence. The solvent was then removed by rotary evaporation to obtain diene-p-aminodiphenylamine compound. Step b2: Add diene-p-aminodiphenylamine compound, 4-amino-2,2,6,6-tetramethylpiperidine and dioxane to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir for 20-30 min at 20-25℃ and 300-400 r / min. Then add 1,8-diazabicyclo[5.4.0]undec-7-ene and continue stirring for 8-10 h at 80-85℃. After the reaction is complete, cool the reaction product to room temperature, then remove the solvent by rotary evaporation. Pour the product into dichloromethane and wash 2-3 times with hydrochloric acid solution and saturated brine solution. Dry with anhydrous magnesium sulfate and then filter under vacuum. Remove the solvent by rotary evaporation of the filtrate to obtain hindered amino-p-aminodiphenylamine compound.

[0011] In a preferred embodiment of the present invention, the ratio of 3,4-epoxycyclohexyl methacrylate, p-aminodiphenylamine and hexafluoroisopropanol in step b1 is 23-25 ​​mmol: 10 mmol: 40-45 mL.

[0012] In a preferred embodiment of the present invention, the ratio of the diene-p-aminodiphenylamine compound, 4-amino-2,2,6,6-tetramethylpiperidine, dioxane, and 1,8-diazabicyclo[5.4.0]undec-7-ene in step b2 is 10 mmol: 23-25 ​​mmol: 70-80 mL: 5-7 mmol.

[0013] In a preferred embodiment of the present invention, the molar concentration of the hydrochloric acid solution in step b2 is 1-1.2 mol / L.

[0014] Secondly, this application provides a process for preparing a highly adhesive and anti-aging silicone sealant, comprising the following steps: Step 1: Weigh out 30-35 parts of hydroxyl-terminated polydimethylsiloxane, 5-9 parts of dimethyl silicone oil, 55-60 parts of nano-calcium carbonate, 3-7 parts of fumed silica, 4.5-6.5 parts of No. 5 white oil, 0.08-0.12 parts of stannous octoate, 1.2-2.6 parts of polysiloxane coupling agent, and 0.8-1.6 parts of hindered amino diphenylamine compound according to the following weight proportions, and set aside for later use; Step 2: Add hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil, nano-calcium carbonate, fumed silica, and No. 5 white oil to a mixer and stir for 3-4 hours at a temperature of 110-120℃ and a stirring speed of 800-1000 r / min. Then, cool down to 40-50℃ and add stannous octoate, polysiloxane coupling agent, and hindered amine p-aminodiphenylamine compound and continue stirring for 3-5 hours to obtain a highly adhesive and anti-aging silicone sealant.

[0015] In a preferred embodiment of the present invention, the hydroxyl-terminated polydimethylsiloxane is a 107 adhesive with a viscosity of 40000 mPa·s.

[0016] In a preferred embodiment of the present invention, the viscosity of the dimethyl silicone oil is 100 mPa·s.

[0017] In a preferred embodiment of the present invention, the average particle size of the nano-calcium carbonate is 80 nm.

[0018] In a preferred embodiment of the present invention, the average particle size of the fumed silica is 500 nm.

[0019] The beneficial effects of this invention are: This invention discloses a high-adhesion, anti-aging silicone sealant and its preparation process. The process involves adding hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil, nano-calcium carbonate, fumed silica, and No. 5 white oil to a mixer for stirring and mixing. After cooling, stannous octoate, a polysiloxane coupling agent, and a hindered aminodiphenylamine compound are added, and stirring continues to produce the high-adhesion, anti-aging silicone sealant. This preparation process enhances the adhesive and mechanical properties of the silicone sealant by adding a polysiloxane coupling agent, and improves its anti-aging properties by adding a hindered aminodiphenylamine compound. This results in a silicone sealant with a wide range of applications, exhibiting excellent adhesion to various substrates. Furthermore, this adhesive bond does not significantly degrade under long-term exposure to heat, oxygen, and ultraviolet radiation, effectively preventing adhesion failure and extending its service life.

[0020] In the preparation of silicone sealant, a polysiloxane coupling agent was first prepared. Octamethylcyclotetrasiloxane, tetramethyltetravinylcyclotetrasiloxane, and tetramethyldivinyldisiloxane were used as monomers to polymerize and form a polyalkenyl silicone oil containing a large number of alkenyl groups. The alkenyl groups on the polyalkenyl silicone oil underwent a hydrosilylation reaction with the Si-H groups on triethoxysilane, introducing a large amount of siloxane to obtain the polysiloxane coupling agent. This polysiloxane coupling agent, with its molecular structure containing a large number of siloxanes, can not only undergo dehydration condensation polymerization with the hydroxyl groups in the silicone sealant to form covalent bonds, improving the mechanical properties of the silicone sealant and increasing its density to enhance its stability, but also react with the hydroxyl groups on the substrate surface to form covalent bonds, thus improving the overall adhesive performance of the silicone sealant.

[0021] In the process of preparing silicone sealant, a hindered amine-based p-aminodiphenylamine compound was also prepared. This was achieved by reacting 3,4-epoxycyclohexyl methacrylate with p-aminodiphenylamine. The epoxy group on 3,4-epoxycyclohexyl methacrylate reacts with the amino group on p-aminodiphenylamine to form a tertiary amine group and simultaneously introduce an alkenyl group, yielding a dienyl p-aminodiphenylamine compound. This dienyl p-aminodiphenylamine compound was then reacted with 4-amino-2,2,6,6-tetramethylpiperidine. The alkenyl group on the dienyl p-aminodiphenylamine compound reacts with the 4-amino-2,2,6,6-tetramethylpiperidine... The amino group on -amino-2,2,6,6-tetramethylpiperidine undergoes a Michael addition reaction, introducing a hindered amine structure to obtain a hindered amine-based p-aminodiphenylamine compound. This hindered amine-based p-aminodiphenylamine compound contains a p-aminodiphenylamine structure in its molecular structure. The active hydrogen atom of the -NH- group inhibits free radical chain growth and chain transfer reactions during the aging process. The hindered amine structure can efficiently capture and remove free radicals generated during photo-oxidative aging, thereby blocking the chain degradation reaction and endowing it with excellent anti-aging properties. Detailed Implementation

[0022] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention. Example

[0023] This embodiment describes a preparation process for a highly adhesive and anti-aging silicone sealant, including the following steps: Step S1: Add 20g of octamethylcyclotetrasiloxane and 0.4g of tetramethylammonium hydroxide to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 20℃ and 300r / min for 30min. Then raise the temperature to 110℃ and continue stirring for 4h. After the reaction is completed, cool the reaction product to room temperature to obtain tetramethylammonium hydroxide silanolate. Step S2: Add 40g of octamethylcyclotetrasiloxane and 35g of tetramethyltetravinylcyclotetrasiloxane to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 20℃ and 300r / min for 20min. Then add 0.02g of tetramethylammonium hydroxide silanolate and 0.1g of tetramethyldivinyldisiloxane and continue stirring for 20min. Then raise the temperature to 100℃ and continue stirring for 4h. Then raise the temperature to 140℃ and continue stirring for 1h. Then raise the temperature to 180℃ and continue stirring for 20min. After the reaction is completed, cool the reaction product to room temperature to obtain polyene silicone oil. Step S3: Add 20g of polyene silicone oil, 1g of triethoxysilane, 0.1mL of platinum(O)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane solution and 60mL of n-hexane to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 20℃ and 300r / min for 20min. Then raise the temperature to 70℃ and continue stirring for 8h. Then raise the temperature to 90℃ and continue stirring for 1h. After the reaction is completed, cool the reaction product to room temperature and then remove the solvent by rotary evaporation to obtain the polysiloxane coupling agent. Step S4: 23 mmol of 3,4-epoxycyclohexyl methacrylate, 10 mmol of p-aminodiphenylamine, and 40 mL of hexafluoroisopropanol were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred at 20 °C and a stirring rate of 300 r / min for 20 min. Then, the temperature was raised to 120 °C and the mixture was stirred for another 20 h. After the reaction was completed, the reaction product was cooled to room temperature and then washed twice with n-heptane and chloroform, respectively. The solvent was then removed by rotary evaporation to obtain diene-p-aminodiphenylamine compound. Step S5: 10 mmol dienyl-p-aminodiphenylamine compound, 23 mmol 4-amino-2,2,6,6-tetramethylpiperidine and 70 mL dioxane were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred for 20 min at 20 °C and a stirring rate of 300 r / min. Then 5 mmol 1,8-diazabicyclo[5.4.0]undec-7-ene was added and the mixture was heated to 80 °C and stirred for another 8 h. After the reaction was completed, the reaction product was cooled to room temperature, and the solvent was removed by rotary evaporation. The product was then poured into dichloromethane and washed twice with 1 mol / L hydrochloric acid solution and saturated brine solution. The product was then dried with anhydrous magnesium sulfate and vacuum filtered. The filtrate was then evaporated by rotary evaporation to remove the solvent, yielding the hindered amino-p-aminodiphenylamine compound. Step S6: Weigh out 30 parts by weight of hydroxyl-terminated polydimethylsiloxane, 5 parts by weight of dimethyl silicone oil, 55 parts by weight of nano-calcium carbonate, 3 parts by weight of fumed silica, 4.5 parts by weight of No. 5 white oil, 0.08 parts by weight of stannous octoate, 1.2 parts by weight of polysiloxane coupling agent, and 0.8 parts by weight of hindered amino-p-aminodiphenylamine compound, and set aside for later use; the hydroxyl-terminated polydimethylsiloxane is 107 glue with a viscosity of 40000 mPa·s; the dimethyl silicone oil has a viscosity of 100 mPa·s; the nano-calcium carbonate has an average particle size of 80 nm; and the fumed silica has an average particle size of 500 nm. Step S7: Add hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil, nano-calcium carbonate, fumed silica, and No. 5 white oil to a mixer and stir for 3 hours at a temperature of 110℃ and a stirring speed of 800r / min. Then, cool down to 40℃ and add stannous octoate, polysiloxane coupling agent, and hindered amine-p-aminodiphenylamine compound and continue stirring for 3 hours to obtain a highly adhesive and anti-aging silicone sealant. Example

[0024] This embodiment describes a preparation process for a highly adhesive and anti-aging silicone sealant, including the following steps: Step S1: Add 20g of octamethylcyclotetrasiloxane and 0.4g of tetramethylammonium hydroxide to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 22℃ and 350r / min for 40min. Then raise the temperature to 115℃ and continue stirring for 5h. After the reaction is completed, cool the reaction product to room temperature to obtain tetramethylammonium hydroxide silanolate. Step S2: Add 42g of octamethylcyclotetrasiloxane and 40g of tetramethyltetravinylcyclotetrasiloxane to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 22℃ and 350r / min for 25min. Then add 0.03g of tetramethylammonium hydroxide silanolate and 0.15g of tetramethyldivinyldisiloxane and continue stirring for 25min. Then raise the temperature to 102℃ and continue stirring for 4.5h. Then raise the temperature to 145℃ and continue stirring for 1.5h. Then raise the temperature to 190℃ and continue stirring for 25min. After the reaction is complete, cool the reaction product to room temperature to obtain polyene silicone oil. Step S3: 22g of polyene silicone oil, 3g of triethoxysilane, 0.15mL of platinum(O)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane solution and 65mL of n-hexane were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Nitrogen gas was introduced for protection. The reaction was stirred at 22℃ and 350r / min for 25min. Then the temperature was raised to 72℃ and the reaction was stirred for 9h. Then the temperature was raised to 92℃ and the reaction was stirred for 1.5h. After the reaction was completed, the reaction product was cooled to room temperature and the solvent was removed by rotary evaporation to obtain the polysiloxane coupling agent. Step S4: 24 mmol of 3,4-epoxycyclohexyl methacrylate, 10 mmol of p-aminodiphenylamine, and 42 mL of hexafluoroisopropanol were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred at 22 °C and a stirring rate of 350 r / min for 25 min. Then, the temperature was raised to 122 °C and the mixture was stirred for another 25 h. After the reaction was completed, the reaction product was cooled to room temperature and then washed twice with n-heptane and chloroform, respectively. The solvent was then removed by rotary evaporation to obtain diene-p-aminodiphenylamine compound. Step S5: 10 mmol dienyl-p-aminodiphenylamine compound, 24 mmol 4-amino-2,2,6,6-tetramethylpiperidine and 75 mL dioxane were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred for 25 min at 22 °C and 350 r / min. Then 6 mmol 1,8-diazabicyclo[5.4.0]undec-7-ene was added and the mixture was heated to 82 °C and stirred for another 9 h. After the reaction was completed, the product was cooled to room temperature, and the solvent was removed by rotary evaporation. The product was then poured into dichloromethane and washed twice with 1.1 mol / L hydrochloric acid solution and saturated brine solution. The product was then dried with anhydrous magnesium sulfate and vacuum filtered. The filtrate was then evaporated by rotary evaporation to remove the solvent, yielding the hindered amino-p-aminodiphenylamine compound. Step S6: Weigh out 32 parts by weight of hydroxyl-terminated polydimethylsiloxane, 7 parts by weight of dimethyl silicone oil, 58 parts by weight of nano-calcium carbonate, 5 parts by weight of fumed silica, 5.5 parts by weight of No. 5 white oil, 0.10 parts by weight of stannous octoate, 1.9 parts by weight of polysiloxane coupling agent, and 1.2 parts by weight of hindered amino-p-aminodiphenylamine compound, and set aside for later use; the hydroxyl-terminated polydimethylsiloxane is 107 glue with a viscosity of 40000 mPa·s; the dimethyl silicone oil has a viscosity of 100 mPa·s; the nano-calcium carbonate has an average particle size of 80 nm; and the fumed silica has an average particle size of 500 nm. Step S7: Add hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil, nano-calcium carbonate, fumed silica, and No. 5 white oil to a mixer and mix for 3.5 h at a temperature of 115℃ and a stirring speed of 900 r / min. Then, cool down to 45℃ and add stannous octoate, polysiloxane coupling agent, and hindered amine-p-aminodiphenylamine compound and continue mixing for 4 h to obtain a highly adhesive and anti-aging silicone sealant. Example

[0025] This embodiment describes a preparation process for a highly adhesive and anti-aging silicone sealant, including the following steps: Step S1: Add 20g of octamethylcyclotetrasiloxane and 0.4g of tetramethylammonium hydroxide to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 25℃ and 400r / min for 50min. Then raise the temperature to 120℃ and continue stirring for 6h. After the reaction is completed, cool the reaction product to room temperature to obtain tetramethylammonium hydroxide silanolate. Step S2: Add 45g of octamethylcyclotetrasiloxane and 45g of tetramethyltetravinylcyclotetrasiloxane to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 25°C and 400r / min for 30min. Then add 0.04g of tetramethylammonium hydroxide silanolate and 0.2g of tetramethyldivinyldisiloxane and continue stirring for 30min. Then raise the temperature to 105°C and continue stirring for 5h. Then raise the temperature to 150°C and continue stirring for 2h. Then raise the temperature to 200°C and continue stirring for 30min. After the reaction is complete, cool the reaction product to room temperature to obtain polyene silicone oil. Step S3: Add 25g of polyene silicone oil, 5g of triethoxysilane, 0.2mL of platinum(O)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane solution and 70mL of n-hexane to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 25℃ and 400r / min for 30min. Then raise the temperature to 75℃ and continue stirring for 10h. Then raise the temperature to 95℃ and continue stirring for 2h. After the reaction is completed, cool the reaction product to room temperature and then remove the solvent by rotary evaporation to obtain the polysiloxane coupling agent. Step S4: 25 mmol of 3,4-epoxycyclohexyl methacrylate, 10 mmol of p-aminodiphenylamine, and 45 mL of hexafluoroisopropanol were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred at 25 °C and 400 r / min for 30 min. Then, the temperature was raised to 125 °C and the mixture was stirred for another 30 h. After the reaction was completed, the product was cooled to room temperature and then washed three times with n-heptane and chloroform. The solvent was then removed by rotary evaporation to obtain diene-p-aminodiphenylamine compound. Step S5: 10 mmol dienyl-p-aminodiphenylamine compound, 25 mmol 4-amino-2,2,6,6-tetramethylpiperidine and 80 mL dioxane were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred at 25 °C and 400 r / min for 30 min. Then 7 mmol 1,8-diazabicyclo[5.4.0]undec-7-ene was added and the mixture was heated to 85 °C and stirred for 10 h. After the reaction was completed, the reaction product was cooled to room temperature, and the solvent was removed by rotary evaporation. The product was then poured into dichloromethane and washed three times with 1.2 mol / L hydrochloric acid solution and saturated brine solution. The product was then dried with anhydrous magnesium sulfate and vacuum filtered. The filtrate was then evaporated by rotary evaporation to remove the solvent, yielding the hindered amino-p-aminodiphenylamine compound. Step S6: Weigh out 35 parts by weight of hydroxyl-terminated polydimethylsiloxane, 9 parts by weight of dimethyl silicone oil, 60 parts by weight of nano-calcium carbonate, 7 parts by weight of fumed silica, 6.5 parts by weight of No. 5 white oil, 0.12 parts by weight of stannous octoate, 2.6 parts by weight of polysiloxane coupling agent, and 1.6 parts by weight of hindered amino-p-aminodiphenylamine compound, and set aside for later use; the hydroxyl-terminated polydimethylsiloxane is 107 glue with a viscosity of 40000 mPa·s; the dimethyl silicone oil has a viscosity of 100 mPa·s; the nano-calcium carbonate has an average particle size of 80 nm; and the fumed silica has an average particle size of 500 nm. Step S7: Add hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil, nano-calcium carbonate, fumed silica, and No. 5 white oil to a mixer and stir for 4 hours at a temperature of 120°C and a stirring speed of 1000 r / min. Then, cool down to 50°C and add stannous octoate, polysiloxane coupling agent, and hindered amine-p-aminodiphenylamine compound and continue stirring for 5 hours to obtain a highly adhesive and anti-aging silicone sealant.

[0026] Comparative Example 1: This comparative example illustrates the preparation process of a highly adhesive and anti-aging silicone sealant, including the following steps: Step S1: Weigh out 35 parts by weight of hydroxyl-terminated polydimethylsiloxane, 9 parts by weight of dimethyl silicone oil, 60 parts by weight of nano-calcium carbonate, 7 parts by weight of fumed silica, 6.5 parts by weight of No. 5 white oil, 0.12 parts by weight of stannous octoate, 2.6 parts by weight of γ-aminopropyltriethoxysilane, and 1.6 parts by weight of hindered amino-p-aminodiphenylamine compound, and set aside. The hydroxyl-terminated polydimethylsiloxane is a 107 adhesive with a viscosity of 40000 mPa·s; the dimethyl silicone oil has a viscosity of 100 mPa·s; the nano-calcium carbonate has an average particle size of 80 nm; and the fumed silica has an average particle size of 500 nm. Step S2: Add hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil, nano calcium carbonate, fumed silica, and No. 5 white oil to a mixer and stir for 4 hours at 120°C and 1000 r / min. Then, cool the mixture to 50°C, add stannous octoate and γ-aminopropyltriethoxysilane, and continue stirring for 5 hours to obtain a highly adhesive and anti-aging silicone sealant.

[0027] Comparative Example 2: This comparative example illustrates the preparation process of a highly adhesive and anti-aging silicone sealant, including the following steps: Step S1: 25 mmol of 3,4-epoxycyclohexyl methacrylate, 10 mmol of p-aminodiphenylamine, and 45 mL of hexafluoroisopropanol were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred at 25 °C and 400 r / min for 30 min. Then, the temperature was raised to 125 °C and the mixture was stirred for another 30 h. After the reaction was completed, the product was cooled to room temperature and then washed three times with n-heptane and chloroform. The solvent was then removed by rotary evaporation to obtain diene-p-aminodiphenylamine compound. Step S2: 10 mmol dienyl-p-aminodiphenylamine compound, 25 mmol 4-amino-2,2,6,6-tetramethylpiperidine and 80 mL dioxane were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred for 30 min at 25 °C and 400 r / min. Then 7 mmol 1,8-diazabicyclo[5.4.0]undec-7-ene was added and the mixture was heated to 85 °C and stirred for 10 h. After the reaction was completed, the reaction product was cooled to room temperature, and the solvent was removed by rotary evaporation. The product was then poured into dichloromethane and washed three times with 1.2 mol / L hydrochloric acid solution and saturated brine solution. The product was then dried with anhydrous magnesium sulfate and vacuum filtered. The filtrate was then evaporated by rotary evaporation to remove the solvent, yielding the hindered amino-p-aminodiphenylamine compound. Step S3: Weigh out 35 parts by weight of hydroxyl-terminated polydimethylsiloxane, 9 parts by weight of dimethyl silicone oil, 60 parts by weight of nano-calcium carbonate, 7 parts by weight of fumed silica, 6.5 parts by weight of No. 5 white oil, 0.12 parts by weight of stannous octoate, 2.6 parts by weight of γ-aminopropyltriethoxysilane, and 1.6 parts by weight of hindered amino-p-aminodiphenylamine compound, and set aside for later use; the hydroxyl-terminated polydimethylsiloxane is a 107 adhesive with a viscosity of 40000 mPa·s; the dimethyl silicone oil has a viscosity of 100 mPa·s; the nano-calcium carbonate has an average particle size of 80 nm; and the fumed silica has an average particle size of 500 nm. Step S7: Add hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil, nano-calcium carbonate, fumed silica, and No. 5 white oil to a mixer and stir for 4 hours at a temperature of 120°C and a stirring rate of 1000 r / min. Then, cool the mixture to 50°C and add stannous octoate, γ-aminopropyltriethoxysilane, and hindered amino diphenylamine compound and continue stirring for 5 hours to obtain a highly adhesive and anti-aging silicone sealant.

[0028] Comparative Example 3: This comparative example illustrates the preparation process of a highly adhesive and anti-aging silicone sealant, including the following steps: Step S1: Add 20g of octamethylcyclotetrasiloxane and 0.4g of tetramethylammonium hydroxide to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 25℃ and 400r / min for 50min. Then raise the temperature to 120℃ and continue stirring for 6h. After the reaction is completed, cool the reaction product to room temperature to obtain tetramethylammonium hydroxide silanolate. Step S2: Add 45g of octamethylcyclotetrasiloxane and 45g of tetramethyltetravinylcyclotetrasiloxane to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 25°C and 400r / min for 30min. Then add 0.04g of tetramethylammonium hydroxide silanolate and 0.2g of tetramethyldivinyldisiloxane and continue stirring for 30min. Then raise the temperature to 105°C and continue stirring for 5h. Then raise the temperature to 150°C and continue stirring for 2h. Then raise the temperature to 200°C and continue stirring for 30min. After the reaction is complete, cool the reaction product to room temperature to obtain polyene silicone oil. Step S3: Add 25g of polyene silicone oil, 5g of triethoxysilane, 0.2mL of platinum(O)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane solution and 70mL of n-hexane to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 25℃ and 400r / min for 30min. Then raise the temperature to 75℃ and continue stirring for 10h. Then raise the temperature to 95℃ and continue stirring for 2h. After the reaction is completed, cool the reaction product to room temperature and then remove the solvent by rotary evaporation to obtain the polysiloxane coupling agent. Step S4: Weigh out 35 parts by weight of hydroxyl-terminated polydimethylsiloxane, 9 parts by weight of dimethyl silicone oil, 60 parts by weight of nano-calcium carbonate, 7 parts by weight of fumed silica, 6.5 parts by weight of No. 5 white oil, 0.12 parts by weight of stannous octoate, and 2.6 parts by weight of polysiloxane coupling agent, and set aside. The hydroxyl-terminated polydimethylsiloxane is a 107 adhesive with a viscosity of 40000 mPa·s; the dimethyl silicone oil has a viscosity of 100 mPa·s; the nano-calcium carbonate has an average particle size of 80 nm; and the fumed silica has an average particle size of 500 nm. Step S5: Add hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil, nano calcium carbonate, fumed silica, and No. 5 white oil to a mixer and stir for 4 hours at a temperature of 120°C and a stirring speed of 1000 r / min. Then, cool the mixture to 50°C, add stannous octoate and polysiloxane coupling agent, and continue stirring for 5 hours to obtain a highly adhesive and anti-aging silicone sealant.

[0029] Comparative Example 4: This comparative example illustrates the preparation process of a highly adhesive and anti-aging silicone sealant, including the following steps: Step S1: Add 20g of octamethylcyclotetrasiloxane and 0.4g of tetramethylammonium hydroxide to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 25℃ and 400r / min for 50min. Then raise the temperature to 120℃ and continue stirring for 6h. After the reaction is completed, cool the reaction product to room temperature to obtain tetramethylammonium hydroxide silanolate. Step S2: Add 45g of octamethylcyclotetrasiloxane and 45g of tetramethyltetravinylcyclotetrasiloxane to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 25°C and 400r / min for 30min. Then add 0.04g of tetramethylammonium hydroxide silanolate and 0.2g of tetramethyldivinyldisiloxane and continue stirring for 30min. Then raise the temperature to 105°C and continue stirring for 5h. Then raise the temperature to 150°C and continue stirring for 2h. Then raise the temperature to 200°C and continue stirring for 30min. After the reaction is complete, cool the reaction product to room temperature to obtain polyene silicone oil. Step S3: Add 25g of polyene silicone oil, 5g of triethoxysilane, 0.2mL of platinum(O)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane solution and 70mL of n-hexane to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 25℃ and 400r / min for 30min. Then raise the temperature to 75℃ and continue stirring for 10h. Then raise the temperature to 95℃ and continue stirring for 2h. After the reaction is completed, cool the reaction product to room temperature and then remove the solvent by rotary evaporation to obtain the polysiloxane coupling agent. Step S4: Weigh out 35 parts by weight of hydroxyl-terminated polydimethylsiloxane, 9 parts by weight of dimethyl silicone oil, 60 parts by weight of nano-calcium carbonate, 7 parts by weight of fumed silica, 6.5 parts by weight of No. 5 white oil, 0.12 parts by weight of stannous octoate, 2.6 parts by weight of polysiloxane coupling agent, and 1.6 parts by weight of p-aminodiphenylamine, and set aside for later use; the hydroxyl-terminated polydimethylsiloxane is 107 adhesive with a viscosity of 40000 mPa·s; the dimethyl silicone oil has a viscosity of 100 mPa·s; the nano-calcium carbonate has an average particle size of 80 nm; and the fumed silica has an average particle size of 500 nm. Step S5: Add hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil, nano calcium carbonate, fumed silica, and No. 5 white oil to a mixer and stir for 4 hours at a temperature of 120°C and a stirring speed of 1000 r / min. Then, cool down to 50°C and add stannous octoate, polysiloxane coupling agent, and p-aminodiphenylamine and continue stirring for 5 hours to obtain a highly adhesive and anti-aging silicone sealant.

[0030] Performance testing The high-adhesion, anti-aging silicone adhesives of Examples 1-3 and Comparative Examples 1-4 were tested for peel strength according to GB / T13477.18-2002, and for tensile strength and tensile strength retention according to JG / T 465-2014.

[0031] The test results are shown in the table below:

[0032] Referring to the data in the table above, and based on the comparison between Examples 1-3 and Comparative Examples 1-4, it can be seen that using polysiloxane coupling agents and adding p-aminodiphenylamine can significantly improve the peel strength, tensile strength, and tensile strength retention rate of silicone sealant, indicating that the silicone sealant of this application has excellent adhesive properties and anti-aging properties.

[0033] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0034] The above description is merely an example and illustration of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described or use similar methods to replace them, as long as they do not deviate from the invention or exceed the scope defined in this application, they should all fall within the protection scope of the present invention.

Claims

1. A highly adhesive and anti-aging silicone sealant, characterized in that, Includes the following components by weight: Hydroxyl-terminated polydimethylsiloxane 30-35 parts, dimethyl silicone oil 5-9 parts, nano-calcium carbonate 55-60 parts, fumed silica 3-7 parts, No. 5 white oil 4.5-6.5 parts, stannous octoate 0.08-0.12 parts, polysiloxane coupling agent 1.2-2.6 parts, and hindered amino group p-aminodiphenylamine compound 0.8-1.6 parts; The polysiloxane coupling agent is prepared by the following steps: Step a1: Octamethylcyclotetrasiloxane and tetramethylammonium hydroxide are stirred and reacted. After the reaction is completed, the reaction product is cooled to obtain tetramethylammonium hydroxide silanolate. Step a2: Octamethylcyclotetrasiloxane and tetramethyltetravinylcyclotetrasiloxane are stirred and reacted, then tetramethylammonium hydroxide silanolate and tetramethyldivinyldisiloxane are added and the reaction is continued. After the reaction is completed, the reaction product is cooled to obtain polyene silicone oil. Step a3: Polyolefin silicone oil, triethoxysilane, platinum (0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane solution and n-hexane are stirred and reacted. After the reaction is completed, the reaction product is cooled and then rotary evaporated to obtain polysiloxane coupling agent.

2. The high-adhesion, anti-aging silicone sealant according to claim 1, characterized in that, The ratio of octamethylcyclotetrasiloxane to tetramethylammonium hydroxide in step a1 is 20g:0.4g.

3. The high-adhesion, anti-aging silicone sealant according to claim 1, characterized in that, The ratio of octamethylcyclotetrasiloxane, tetramethyltetravinylcyclotetrasiloxane, tetramethylammonium hydroxide silanolate, and tetramethyldivinyldisiloxane in step a2 is 40-45g: 35-45g: 0.02-0.04g: 0.1-0.2g.

4. The high-adhesion, anti-aging silicone sealant according to claim 1, characterized in that, The ratio of polyene silicone oil, triethoxysilane, platinum (O)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane solution and n-hexane in step a3 is 20-25g: 1-5g: 0.1-0.2mL: 60-70mL.

5. The high-adhesion, anti-aging silicone sealant according to claim 1, characterized in that, The hindered amino group p-aminodiphenylamine compound was prepared by the following steps: Step b1: 3,4-epoxycyclohexyl methacrylate, p-aminodiphenylamine and hexafluoroisopropanol were stirred and reacted. After the reaction was completed, the reaction product was cooled, washed and rotary evaporated to obtain diene-p-aminodiphenylamine compound. Step b2: The dienyl-p-aminodiphenylamine compound, 4-amino-2,2,6,6-tetramethylpiperidine and dioxane were stirred and reacted. Then, 1,8-diazabicyclo[5.4.0]undec-7-ene was added and the reaction was stirred and reacted. After the reaction was completed, the reaction product was cooled, then evaporated by rotary evaporation, and then poured into dichloromethane. After washing and drying, the product was filtered under vacuum and the filtrate was evaporated by rotary evaporation to obtain the hindered amino-p-aminodiphenylamine compound.

6. The high-adhesion, anti-aging silicone sealant according to claim 5, characterized in that, In step b1, the ratio of 3,4-epoxycyclohexyl methacrylate, p-aminodiphenylamine, and hexafluoroisopropanol is 23-25 ​​mmol: 10 mmol: 40-45 mL.

7. The high-adhesion, anti-aging silicone sealant according to claim 5, characterized in that, The ratio of diene-p-aminodiphenylamine compound, 4-amino-2,2,6,6-tetramethylpiperidine, dioxane, and 1,8-diazabicyclo[5.4.0]undec-7-ene in step b2 is 10 mmol: 23-25 ​​mmol: 70-80 mL: 5-7 mmol.

8. A preparation process for a high-adhesion, anti-aging silicone sealant as described in any one of claims 1-7, characterized in that, Includes the following steps: Step 1: Weigh out 30-35 parts of hydroxyl-terminated polydimethylsiloxane, 5-9 parts of dimethyl silicone oil, 55-60 parts of nano-calcium carbonate, 3-7 parts of fumed silica, 4.5-6.5 parts of No. 5 white oil, 0.08-0.12 parts of stannous octoate, 1.2-2.6 parts of polysiloxane coupling agent, and 0.8-1.6 parts of hindered amino group p-aminodiphenylamine compound according to the following weight proportions, and set aside for later use; Step 2: Add hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil, nano-calcium carbonate, fumed silica, and No. 5 white oil to a mixer and stir for 3-4 hours at a temperature of 110-120℃ and a stirring speed of 800-1000 r / min. Then, cool down to 40-50℃ and add stannous octoate, polysiloxane coupling agent, and hindered amine p-aminodiphenylamine compound and continue stirring for 3-5 hours to obtain a highly adhesive and anti-aging silicone sealant.

9. The preparation process of a high-adhesion, anti-aging silicone sealant according to claim 8, characterized in that, The hydroxyl-terminated polydimethylsiloxane is a 107 adhesive with a viscosity of 40000 mPa·s; The viscosity of the dimethyl silicone oil is 100 mPa·s; The average particle size of the nano-calcium carbonate is 80 nm. The average particle size of the fumed silica is 500 nm.