Low-stress flame-retardant silicone potting adhesive material and preparation method thereof
Through the synergistic effect of triazine-based double-terminated siloxane chain extender and nano-aluminum hydroxide, an organosilicon potting compound with high flame retardancy, low stress, excellent toughness and interfacial adhesion is formed, which solves the problem of difficulty in achieving both flame retardancy and toughness in the existing technology, and improves the service life and reliability of electronic devices.
Patent Information
- Application Number
- CN202611400903.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-20
AI Technical Summary
Existing addition-type silicone potting compounds are difficult to balance low stress and high flame retardancy, and their interfacial adhesion and humid heat stability are insufficient, which makes electronic devices prone to interfacial peeling, cracking and corrosion under complex working conditions.
A two-component system consisting of a triazine-based double-ended hydrogen siloxane chain extender and a nano-synergistic flame-retardant filler is adopted. Through hydrosilylation reaction, a cross-linked network centered on triazine heterocycles is formed. Combined with the flame-retardant mechanism of nano-aluminum hydroxide, the interfacial adhesion and thermal stability are enhanced.
It achieves a high flame retardant rating with low filler content, reduces internal stress, improves interfacial bonding strength and hygrothermal stability, and is suitable for long-term reliability protection of high-precision electronic devices.
Smart Images

Figure SMS_9 
Figure SMS_10
Abstract
Description
Technical Field
[0001] This invention relates to the field of electronic packaging materials technology, specifically to a low-stress flame-retardant silicone potting compound and its preparation method. Background Technology
[0002] Silicone potting compounds, with their excellent high and low temperature resistance, electrical insulation, weather resistance, and elastic cushioning capabilities, are widely used in the potting and protection of high-end electronic fields such as new energy vehicle electronic control modules, power inverters, precision sensors, and 5G communication devices. As electronic devices develop towards higher power density and higher integration, potting compounds simultaneously face stringent flame retardant safety requirements and stress reliability challenges under complex operating conditions.
[0003] The main technical bottlenecks of existing addition-type silicone potting compounds are as follows: First, it is difficult to achieve both low stress and high flame retardancy. To meet the UL94V-0 flame retardancy standard, existing technologies typically use large amounts of inorganic flame retardant fillers such as aluminum hydroxide and magnesium hydroxide, often exceeding 50wt%. This significantly increases the viscosity of the system, reduces fluidity, and leads to increased modulus and internal stress after curing. Under thermal cycling conditions of -40℃ to 85℃, interface peeling and cracking of the colloid are easily caused by the mismatch of thermal expansion coefficients, resulting in insulation failure of electronic devices. On the other hand, low-modulus, low-stress soft potting compound formulations usually have low crosslinking density and weak charring ability, and the flame retardancy rating can only reach V-1 or even HB, which cannot meet the safety requirements of high-power electronic devices. Second, conventional chain extenders have limited functionality. Existing hydrogen-based silicone oil chain extenders can only adjust the crosslinking density and cannot impart additional flame retardant and toughening effects to the system. Introducing phenyl silicone resin to improve heat resistance increases the system's brittleness and reduces its impact resistance and stress absorption capacity, leading to the technical problem of "increasing rigidity results in brittleness, and increasing toughness results in softness." Third, there is insufficient interfacial adhesion and humid heat stability. Ordinary silicone potting compounds have limited adhesion strength to metals, PCB substrates, and plastic housings, and are prone to interfacial debonding in high-temperature and high-humidity environments. Moisture intrusion accelerates device corrosion and shortens service life.
[0004] Therefore, developing an organosilicon potting compound that simultaneously possesses ultra-low curing internal stress, high flame retardancy, excellent mechanical toughness, and interfacial adhesion is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0005] To address the problems existing in the prior art, the purpose of this invention is to provide a low-stress flame-retardant silicone potting compound material and its preparation method.
[0006] The objective of this invention is achieved through the following technical solution: In a first aspect, the present invention provides a low-stress flame-retardant silicone potting compound material, which is a two-component system, consisting of component A and component B mixed and cured in a mass ratio of 1:1 by mass parts; Component A comprises: 80-100 parts of vinyl-terminated polydimethylsiloxane, 0.5-2 parts of platinum catalyst, and 5-15 parts of nano-synergistic flame retardant filler. Component B comprises: 60-80 parts of vinyl-terminated polydimethylsiloxane, 15-25 parts of triazine-based bihydrosiloxane chain extender, 0.5-5 parts of crosslinking agent, 0.05-0.2 parts of inhibitor, 2-6 parts of adhesion promoter, and 5-15 parts of nano-synergistic flame retardant filler. The triazine-based bihydrosiloxane chain extender has a triazine heterocycle as the central rigid node, with polydimethylsiloxane segments connected to both sides by propylene groups formed by hydrosilylation. The two ends of the molecule are active Si-H bonds. It is prepared by hydrosilylation reaction of hydrogen-terminated polydimethylsiloxane and diallyl isocyanurate.
[0007] Furthermore, the viscosity of the end-vinyl polydimethylsiloxane is 500-5000. The vinyl content is 0.1%-0.5% by mass.
[0008] Furthermore, the preparation method of the triazine-based dihydrosiloxane chain extender includes: S1. Under nitrogen protection, hydrogen-terminated polydimethylsiloxane and diallyl isocyanurate are added to toluene at a molar ratio of 2.05-2.30:1, with the solid content controlled at 20-40 wt%. After stirring and dissolving, Karstedt platinum catalyst is added, with the amount of platinum being 2-8 ppm of the total reactant mass, and stirred until homogeneous.
[0009] The hydrogen-terminated polydimethylsiloxane has a number-average molecular weight of 800-1500, a Si-H content of 1.2-2.5 mmol / g, and contains 2 terminal Si-H atoms per molecule.
[0010] S2. Under nitrogen protection at 60-80℃, a toluene solution of diallyl isocyanurate is slowly added dropwise to the above reaction solution over 1-2 hours. After the addition is complete, the reaction continues for 2-4 hours, then heating is stopped, and the mixture is cooled to room temperature. After the reaction is complete, toluene is recovered by vacuum distillation. The residue is separated by molecular distillation or column chromatography to remove unreacted di-terminated PDMS and di-terminated addition byproducts. The di-terminated Si-H triazine chain extender fraction is collected. The fraction is then decolorized with activated carbon and dried under vacuum to obtain the target product.
[0011] Furthermore, the crosslinking agent is a hydrogen-containing silicone oil with a hydrogen mass fraction of 0.5%-1.0% and a viscosity of 50-200. .
[0012] Furthermore, the nano-synergistic flame retardant filler is surface-modified silane-modified nano-aluminum hydroxide with a particle size of 20-50 nm, and the total addition amount accounts for 8%-12% of the total mass of the system; its surface modification uses vinyltriethoxysilane with a grafting rate of 1.5%-2.5%.
[0013] Furthermore, the platinum catalyst is a platinum-vinylsiloxane complex (Karstedt catalyst) with a platinum metal mass fraction of 3000-5000 ppm; the inhibitor is ethynylcyclohexanol.
[0014] Furthermore, the adhesion promoter is a mixture of γ-glycidoxypropyltrimethoxysilane and γ-methacryloyloxypropyltrimethoxysilane in a mass ratio of 1:1.
[0015] Secondly, the present invention provides a method for preparing the above-mentioned low-stress flame-retardant silicone potting compound material, comprising the following steps: Step 1: Add vinyl-terminated polydimethylsiloxane to a planetary mixer according to the formula. Add nano-synergistic flame retardant filler in batches under low-speed stirring. After stirring and dispersing for 20-30 minutes, add platinum catalyst and continue vacuum stirring for 15-20 minutes. The vacuum degree is ≤-0.09MPa. Filter the material to obtain component A. Step 2: Add vinyl-terminated polydimethylsiloxane to a planetary mixer according to the formula, add nano-synergistic flame retardant filler in batches, and after even dispersion, add triazine-based double-terminated hydrogen siloxane chain extender, crosslinking agent, inhibitor and adhesion promoter in sequence. Stir under vacuum for 25-35 minutes, with a vacuum degree ≤-0.09MPa, and filter to obtain component B. Step 3: Prepare components A and B according to their respective formula proportions. When using, mix components A and B at a mass ratio of 1:1, degas, fill and seal, let stand at room temperature for 4-8 hours for initial curing, and heat at 80℃ for 2 hours for complete curing.
[0016] The beneficial effects of this invention are as follows: 1. This invention prepares a triazine-based double-terminated hydrogen siloxane chain extender via a hydrosilylation reaction, forming a molecular structure with a triazine heterocycle at the center and polydimethylsiloxane segments symmetrically connected on both sides. After this chain extender is integrated into the organosilicon crosslinking network, the central triazine heterocycle acts as a rigid structural unit, improving the system's thermal stability and char-forming ability. During combustion, it catalyzes the formation of a dense, continuous char barrier layer, effectively blocking the transfer of heat and oxygen. The polydimethylsiloxane segments on both sides impart good segmental flexibility and stress relaxation properties to the crosslinking network, effectively dissipating the internal stress generated during thermal cycling. This achieves a synergistic improvement in flame retardancy and low-stress characteristics at the molecular level, solving the problem of the difficulty in simultaneously achieving flame retardancy, toughness, and low stress in traditional organosilicon potting compounds.
[0017] 2. This invention employs a flame-retardant system that combines molecular chemical bonding flame retardancy with synergistic effects of nanofillers. The triazine flame-retardant structure is introduced into the cross-linked network backbone through chain extension reactions, avoiding the problems of easy migration and precipitation of small molecule flame retardants, resulting in a long-lasting and stable flame-retardant effect. Its combination with the endothermic decomposition and solid-phase barrier effect of nano-aluminum hydroxide forms a multiple flame-retardant mechanism, enabling the system to achieve a high flame-retardant rating even with a low filler content. The low filler content also maintains excellent flow processing properties, minimal volume shrinkage during curing, low internal stress in the cured product, and good dimensional stability, meeting the potting requirements of high-precision electronic components.
[0018] 3. The chain extender of this invention forms a stable carbon-silicon bond structure through hydrosilylation. Compared with conventional heteroatom-linked chain extenders, it exhibits superior resistance to hydrolysis, oxidation, and heat aging, thus improving the structural integrity of the crosslinked network under high temperature and humidity conditions. Simultaneously, the triazine polar group and the compounded adhesion promoter work synergistically to form multiple interfacial interactions of chemical bonding and physical adsorption on various substrates such as metals, ceramics, and PCB substrates. This significantly improves the interfacial adhesion strength of the potting compound, reduces the risk of interfacial debonding during long-term service, and enhances the protective reliability and service life of electronic devices.
[0019] 4. This invention adopts a two-component system with good viscosity matching between the two components, simple mixing ratio, and flexible operation period that can be adjusted by the amount of inhibitor. It is suitable for various construction methods such as manual potting and automated online potting. The preparation process is mild, the product is easy to separate and purify, and it is suitable for large-scale industrial production. Detailed Implementation
[0020] The technical solution of the present invention is illustrated below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not preclude the existence of other method steps before or after the combined steps, or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the present invention. Furthermore, unless otherwise stated, the numbering of each method step is merely a convenient tool for identifying each method step, and not for limiting the order of the method steps or defining the scope of the present invention. Changes or adjustments to their relative relationships, without substantially altering the technical content, should also be considered within the scope of the present invention.
[0021] To better understand the above technical solutions, exemplary embodiments of the present invention are described in more detail below. While exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided to enable a more thorough understanding of the present invention and to fully convey the scope of the invention to those skilled in the art.
[0022] The present invention will be further described below with reference to the following embodiments.
[0023] Example 1 A low-stress flame-retardant silicone potting compound material, composed of components A and B in a mass ratio of 1:1.
[0024] Component A, by mass parts: 90 parts vinyl-terminated polydimethylsiloxane (viscosity 2000) The catalyst contained 0.25% vinyl content, 1 part Karstedt platinum catalyst (platinum content 3000ppm), and 10 parts modified nano aluminum hydroxide (particle size 30nm).
[0025] Component B, by mass parts: 70 parts vinyl-terminated polydimethylsiloxane (viscosity 2000) The product contains 0.25% vinyl content, 20 parts triazine-based double-terminated hydrosiloxane chain extender, 1.0 part hydrogen-containing silicone oil crosslinking agent (0.8% hydrogen content), 0.1 part ethynylcyclohexanol inhibitor, 4 parts adhesion promoter, and 10 parts modified nano aluminum hydroxide (30nm particle size).
[0026] The preparation of triazine-based double-terminated hydrosiloxane chain extenders includes: S1. Under nitrogen protection, weigh 102.8 g of hydrogen-terminated polydimethylsiloxane (number average molecular weight 1000, Si-H content 2.0 mmol / g) and add it to a reaction flask. Add toluene and stir to dilute. Separately weigh 10 g of diallyl isocyanurate (molar ratio of hydrogen-terminated polydimethylsiloxane to diallyl isocyanurate 2.15:1, i.e., molar ratio of Si-H to allyl double bond 2.15:1) and dissolve it in toluene to prepare a solution. The total solid content of the system is controlled to be 30 wt%. After stirring evenly, add Karstedt platinum catalyst at 5 ppm of the total reactant mass based on platinum atoms, and stir to mix evenly.
[0027] S2. Under nitrogen protection, the temperature was raised to 70℃, and a toluene solution of diallyl isocyanurate was slowly added dropwise to the reaction flask over 1.5 hours. After the addition was complete, the reaction was continued at this temperature for 3 hours. A sample was taken and the conversion rate of the allyl double bond was 96.2%, and the residual Si-H content was 55.3% of the initial value. Heating was then stopped, and the mixture was cooled to room temperature. After the reaction was complete, toluene was recovered by vacuum distillation at 45℃. The residue was purified by molecular distillation to remove unreacted dihydrogen-terminated PDMS and dihydrogen-terminated byproducts. The target fraction was collected, decolorized with activated carbon, and vacuum dried at 40℃ for 12 hours to obtain a transparent, viscous triazine-based dihydrogen-terminated siloxane chain extender with a Si-H content of 0.91 mmol / g.
[0028] The adhesion promoter is a mixture of γ-glycidoxypropyltrimethoxysilane and γ-methacryloyloxypropyltrimethoxysilane in a mass ratio of 1:1; the nano-aluminum hydroxide is surface-modified with vinyltriethoxysilane with a grafting rate of 2.0%.
[0029] The preparation method of the above-mentioned silicone potting compound material: Step 1, Preparation of Component A: Add vinyl-terminated polydimethylsiloxane to a planetary mixer, add nano-aluminum hydroxide in 3 batches under low speed stirring, stir at 300 r / min for 25 min; add platinum catalyst, stir under vacuum for 15 min at a vacuum degree of -0.095 MPa, and filter out through a 200 mesh filter.
[0030] Step 2, Preparation of Component B: Add vinyl-terminated polydimethylsiloxane to a planetary mixer, add nano-aluminum hydroxide in 3 batches and disperse evenly; add chain extender, crosslinking agent, inhibitor, and adhesion promoter in sequence, stir under vacuum for 30 min, and filter out through a 200 mesh filter.
[0031] Step 3: Prepare components A and B according to their respective formula proportions. When using, mix components A and B at a mass ratio of 1:1, degas under vacuum for 5 minutes, fill and seal, let stand at room temperature for 6 hours for initial curing, and then cure at 80°C for 2 hours.
[0032] Example 2 A low-stress flame-retardant silicone potting compound material differs from Example 1 in that the formulation ratio and chain extender preparation parameters are different.
[0033] Component A, by mass parts: 80 parts vinyl-terminated polydimethylsiloxane (viscosity 500... The mixture contains 0.4% vinyl content, 0.5 parts platinum catalyst, and 5 parts modified nano-aluminum hydroxide (particle size 20nm).
[0034] Component B, by weight parts: 60 parts of vinyl-terminated polydimethylsiloxane (viscosity 500... The product contains 0.4% vinyl content, 15 parts triazine-based double-terminated hydrosiloxane chain extender, 2.15 parts hydrogen-containing silicone oil crosslinking agent (hydrogen content 1.0%), 0.05 parts inhibitor, 2 parts adhesion promoter, and 5 parts modified nano aluminum hydroxide.
[0035] The preparation of triazine-based double-terminated hydrosiloxane chain extenders includes: S1. Under nitrogen protection, 82g of hydrogen-terminated polydimethylsiloxane (number average molecular weight 800, Si-H content 2.5mmol / g) was weighed and placed into a reaction flask, and toluene was added and stirred to dilute. Separately, 10g of diallyl isocyanurate (molar ratio 2.14:1) was weighed and dissolved in toluene to prepare a solution. The total solid content of the system was controlled to be 20wt%. After stirring evenly, Karstedt platinum catalyst was added, with the amount of platinum being 2ppm of the total reactant mass, and the mixture was stirred evenly.
[0036] S2. Under nitrogen protection, heat to 60°C and slowly add a toluene solution of diallyl isocyanurate dropwise into the reaction flask over 1 hour. After the addition is complete, keep the temperature constant and continue the reaction for 2 hours. Take a sample and test the conversion rate of allyl double bonds to 95.4%. Stop heating and cool down.
[0037] After the reaction was completed, toluene was recovered by vacuum distillation at 40 °C; the residue was purified by column chromatography with hexane / ethyl acetate, and the target component was collected, decolorized by activated carbon, and dried under vacuum at 35 °C for 15 h to obtain a triazine-based dihydrosiloxane chain extender with a Si-H content of 1.11 mmol / g.
[0038] The remaining raw materials and preparation methods are the same as in Example 1.
[0039] Example 3
[0040] A low-stress flame-retardant silicone potting compound material differs from Example 1 in that the formulation ratio and chain extender preparation parameters are different.
[0041] Component A, by weight: 100 parts vinyl-terminated polydimethylsiloxane (viscosity 5000) (Vinyl content 0.15%), 2 parts platinum catalyst, and 15 parts modified nano-aluminum hydroxide (particle size 50nm).
[0042] Component B, by mass parts: 80 parts of vinyl-terminated polydimethylsiloxane (viscosity 5000) The product contains 0.15% vinyl content, 25 parts triazine-based double-terminated hydrosiloxane chain extender, 0.57 parts hydrogen-containing silicone oil crosslinking agent (0.5% hydrogen content), 0.2 parts inhibitor, 6 parts adhesion promoter, and 15 parts modified nano aluminum hydroxide.
[0043] The preparation of triazine-based double-terminated hydrosiloxane chain extenders includes: S1. Under nitrogen protection, 164.3 g of hydrogen-terminated polydimethylsiloxane (number average molecular weight 1500, Si-H content 1.33 mmol / g) was weighed and placed into a reaction flask, and toluene was added and stirred to dilute. Separately, 10 g of diallyl isocyanurate (molar ratio 2.30:1) was weighed and dissolved in toluene to prepare a solution. The total solid content of the system was controlled to be 40 wt%. After stirring evenly, Karstedt platinum catalyst was added, with the amount of platinum being 8 ppm of the total reactant mass, and the mixture was stirred evenly.
[0044] S2. Under nitrogen protection, the temperature is raised to 80℃, and the toluene solution of diallyl isocyanurate is slowly added dropwise to the reaction flask over a period of 2 hours. After the addition is complete, the temperature is maintained and the reaction continues for another 4 hours. The allyl double bond conversion rate is 98.5%, and the Si-H content is reduced to 57.2% of the initial value. Heating is then stopped and the mixture is cooled.
[0045] After the reaction was completed, toluene was recovered by vacuum distillation at 50℃; the residue was purified by molecular distillation, and the target fraction was collected, decolorized by activated carbon, and dried under vacuum at 40℃ for 10 h to obtain a triazine-based dihydrosiloxane chain extender with a Si-H content of 0.62 mmol / g.
[0046] The remaining raw materials and preparation methods are the same as in Example 1.
[0047] Comparative Example 1 An organosilicon potting compound differs from Example 1 in that it uses a common linear dihydrogen-terminated polydimethylsiloxane with an equivalent hydrogen content instead of a triazine dihydrogen-terminated siloxane chain extender, while the other raw materials, proportions, and preparation methods remain the same.
[0048] Comparative Example 2 An organosilicon potting compound differs from Example 1 in that it does not contain a triazine-based double-terminated siloxane chain extender. Instead, it achieves the same UL94 V-0 flame retardant rating by increasing the amount of nano-aluminum hydroxide. The amount of modified nano-aluminum hydroxide in components A and B is adjusted to 17.5 parts and 17.5 parts respectively, totaling 35 parts. The rest of the preparation method is the same as in Example 1.
[0049] Comparative Example 3 Commercially available ordinary flame-retardant silicone potting compound, labeled UL94V-0 grade, was used as a blank control.
[0050] Performance testing Standard test specimens were prepared using the potting compounds from each embodiment and the comparative embodiment. After complete curing, the performance was tested according to the corresponding standards. The test standards are as follows: (1) Flame retardant rating: UL94-2013, sample thickness 2.0mm; (2) Volume shrinkage rate: calculated by density method before and after curing, and density measured by Archimedes' drainage method; (3) Shore A hardness: GB / T 531.1-2008; (4) Tensile strength / elongation at break: GB / T 528-2009; (5) Adhesion to glass substrate: GB / T 9286-1998 Cross-cut adhesion test; (6) Thermal cycling test: -40℃ to 85℃, 100 cycles, observe whether cracking or delamination occurs; (7) Damp heat aging: Placed at 85℃ / 85% RH for 1000h, the bond strength retention rate was tested; (8) Compression modulus: Characterizes the stress level. The lower the modulus, the stronger the stress buffering capacity.
[0051] The test results are shown in Tables 1 and 2.
[0052]
[0053]
[0054] The test results show that: The potting compounds prepared in Examples 1-3 achieved UL94 V-0 flame retardancy while maintaining extremely low compressive modulus and curing shrinkage, with an elongation at break exceeding 200%, and internal stress levels far lower than the comparative examples. They also exhibited excellent performance under thermal cycling and humid aging. Comparative Example 1 used a common linear hydrogen-containing chain extender, lacking the synergistic flame retardancy and rigidity of the triazine ring, resulting in a decreased flame retardancy rating, increased stress levels, and poorer adhesion and weather resistance. Comparative Example 2 achieved flame retardancy through high filler content, but this significantly increased hardness and modulus, increased shrinkage, and markedly increased internal stress, making it prone to cracking under thermal cycling and exhibiting severe degradation in adhesive performance after humid aging. Comparative Example 3, a commercially available product, showed a significant gap in achieving a comprehensive balance between low stress and flame retardancy.
[0055] In summary, this invention uses triazine-based double-terminated hydrogen siloxane as a chain extender to achieve a synergistic improvement in low stress and high flame retardancy of silicone potting compounds, while also possessing excellent hydrolytic stability and interfacial adhesion, making it suitable for long-term reliable protection of high-power precision electronic devices.
[0056] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. The illustrative expressions of the above terms in this specification should not be construed as necessarily referring to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. In addition, those skilled in the art can combine and integrate the different embodiments or examples described in this specification.
[0057] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.
Claims
1. A low-stress flame-retardant silicone potting compound material, characterized in that, It is formed by mixing and curing component A and component B in a mass ratio of 1:1; component A, by mass parts, includes: 80-100 parts of vinyl-terminated polydimethylsiloxane, 0.5-2 parts of platinum catalyst, and 5-15 parts of nano-synergistic flame retardant filler. The B component, by mass parts, comprises: 60-80 parts vinyl-terminated polydimethylsiloxane, 15-25 parts triazine-based bihydrosiloxane chain extender, 0.5-5 parts crosslinking agent, 0.05-0.2 parts inhibitor, 2-6 parts adhesion promoter, and 5-15 parts nano-synergistic flame retardant filler. The triazine-based double-terminated siloxane chain extender is prepared by hydrosilylation reaction of hydrogen-terminated polydimethylsiloxane and diallyl isocyanurate.
2. The low-stress flame-retardant silicone potting compound material according to claim 1, characterized in that, The viscosity of the vinyl-terminated polydimethylsiloxane is 500-5000. The vinyl content is 0.1%-0.5% by mass.
3. The low-stress flame-retardant silicone potting compound material according to claim 1, characterized in that, The preparation method of the triazine-based double-terminated hydrosiloxane chain extender includes: S1. Under nitrogen protection, hydrogen-terminated polydimethylsiloxane was added to toluene and stirred to dilute it. Karstedt platinum catalyst was added and stirred until homogeneous. The amount of platinum was 2-8 ppm of the total reactant mass. S2. Under nitrogen protection at 60-80℃, a toluene solution of diallyl isocyanurate is slowly added dropwise to the above reaction solution. The molar ratio of hydrogen-terminated polydimethylsiloxane to diallyl isocyanurate is 2.05-2.30:1, the solid content of the system is controlled at 20-40 wt%, and the addition time is 1-2 h. After the addition is complete, the reaction continues for 2-4 h. After the reaction is completed, the toluene is recovered by vacuum distillation, purified, and vacuum dried to obtain a triazine-based double-terminated hydrosiloxane chain extender.
4. The low-stress flame-retardant silicone potting compound material according to claim 3, characterized in that, The hydrogen-terminated polydimethylsiloxane has a number average molecular weight of 800-1500, a Si-H content of 1.2-2.5 mmol / g, and contains 2 terminal Si-H atoms per molecule.
5. The low-stress flame-retardant silicone potting compound material according to claim 1, characterized in that, The crosslinking agent is a hydrogen-containing silicone oil with a hydrogen mass fraction of 0.5%-1.0% and a viscosity of 50-200. .
6. The low-stress flame-retardant silicone potting compound material according to claim 1, characterized in that, The nano-synergistic flame retardant filler is surface-modified silane-modified nano-aluminum hydroxide with a particle size of 20-50 nm, and the total addition amount accounts for 8%-12% of the total mass of the system; the surface modification uses vinyltriethoxysilane with a grafting rate of 1.5%-2.5%.
7. The low-stress flame-retardant silicone potting compound material according to claim 1, characterized in that, The platinum catalyst is a platinum-vinylsiloxane complex with a platinum metal mass fraction of 3000-5000 ppm; the inhibitor is ethynylcyclohexanol.
8. The low-stress flame-retardant silicone potting compound material according to claim 1, characterized in that, The adhesion promoter is a mixture of γ-glycidoxypropyltrimethoxysilane and γ-methacryloyloxypropyltrimethoxysilane in a mass ratio of 1:
1.
9. A method for preparing the low-stress flame-retardant silicone potting compound material according to any one of claims 1-8, characterized in that, Includes the following steps: Step 1: Add vinyl-terminated polydimethylsiloxane to a planetary mixer according to the formula. Add nano-synergistic flame retardant filler in batches under low-speed stirring. After stirring and dispersing for 20-30 minutes, add platinum catalyst and continue vacuum stirring for 15-20 minutes. The vacuum degree is ≤-0.09MPa. Filter the material to obtain component A. Step 2: Add vinyl-terminated polydimethylsiloxane to a planetary mixer according to the formula, add nano-synergistic flame retardant filler in batches, and after even dispersion, add triazine-based double-terminated hydrogen siloxane chain extender, crosslinking agent, inhibitor and adhesion promoter in sequence. Stir under vacuum for 25-35 minutes, with a vacuum degree ≤-0.09MPa, and filter to obtain component B.
10. The preparation method according to claim 9, characterized in that, When using, mix components A and B thoroughly at a mass ratio of 1:1, degas, fill and seal, let stand at room temperature for 4-8 hours for initial curing, and heat at 80℃ for 2 hours for complete curing.