High-strength and high-toughness epoxy adhesive and preparation method thereof
By combining polyetheramine prepolymer modified E-54 epoxy resin, epoxy functionalized hyperbranched polyester, and phenolic epoxy resin, a high-strength and high-toughness epoxy adhesive is formed, which solves the problems of poor adhesion, high brittleness, and narrow processing of spirocyclic polyether resin, and realizes the application of high-strength, high-toughness, and high-transparency adhesives in PBX explosive casting systems.
Patent Information
- Application Number
- CN202611517554.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-20
AI Technical Summary
Spirocyclic polyether resins, after curing, suffer from poor adhesion to metal shells, high brittleness, easy aging, and narrow process windows, making it difficult to meet the high strength, high toughness, and transparency requirements of PBX explosive casting systems.
Using polyetheramine prepolymer modified E-54 epoxy resin, epoxy functionalized hyperbranched polyester and phenolic epoxy resin as the main agents, and hexafunctional polythiol as the curing agent, a high-strength and high-toughness epoxy adhesive is formed through a three-level synergistic effect, including flexible segment embedding, rigid-flexible gradient structure and high cross-linking density network.
It achieves tensile strength ≥35 MPa, elongation at break ≥60%, impact strength ≥90 J/m, and viscosity ≤0.2 Pa·s at 60℃, making it suitable for precision electronic packaging and metal-composite bonding. It solves the problems of poor adhesion, high brittleness, and narrow process window of spirocyclic polyether resin.
Smart Images

Figure CN123131983A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a high-strength and high-toughness epoxy adhesive and its preparation method, belonging to the field of epoxy adhesive preparation technology. Background Technology
[0002] Spirocyclic polyether resin (known in the industry as "123 resin", the main component of which is 3,9-divinyl-2,4,8,10-tetraoxaspiro[5,5]undecane condensate) is widely used in PBX explosive casting systems due to its high hardness and good dimensional stability after curing. However, it has three inherent defects: (1) low polarity, poor adhesion to metal shells, and easy debonding and cracking during hot and cold cycles; (2) high brittleness, elongation at break <5%, and low impact strength; (3) containing spirocyclic structure, it is afraid of moisture, light and heat, and has harsh storage and transportation requirements. In addition, cationic curing is prone to chain termination, resulting in a narrow process window.
[0003] The industry has attempted to replace 123 resin with epoxy resin, but faces a "strength-toughness-processability" dilemma. 1) Although hyperbranched epoxy toughening routes (such as CN102190858A and CN109897175A) can improve toughness, the introduction of hyperbranching is often accompanied by a decrease in heat resistance and poor compatibility with multifunctional epoxy. 2) The low-temperature curing route of polythiol (such as CN105238316B, CN113999637B) can achieve rapid curing at medium and low temperatures, but it often uses polyetheramine / fatty amine as a curing agent blend component, which does not solve the problem of bulk toughening of "long-chain flexible pre-embedded epoxy skeleton", and the transparency and density index are difficult to match 123 resin. 3) Core-shell / inorganic particle toughening (such as CN119060664A) has high shear strength, but it affects the transparency and casting fluidity of the system and is not suitable for scenarios such as PBX where purity is sensitive.
[0004] Therefore, there is still a need for a two-component epoxy adhesive with tensile strength ≥25 MPa, elongation at break ≥35%, impact strength ≥60 J / m, viscosity ≤0.7 Pa·s@60℃, which can be cured at medium temperature and can replace 123 resin. Summary of the Invention
[0005] To address the problems of poor adhesion between spirocyclic polyether resin and metal, high brittleness, easy aging, and narrow process window, this invention proposes a high-strength and high-toughness epoxy adhesive and its preparation method.
[0006] The technical solution adopted by the present invention to solve the above problems is: a high-strength and high-toughness epoxy adhesive proposed in the present invention, comprising: The main components include polyetheramine prepolymerized modified E-54 epoxy resin, epoxy-functionalized hyperbranched polyester, and phenolic epoxy resin. Curing agents include multifunctional polythiols, accelerators, and polymerization inhibitors; The mass ratio of the main agent to the curing agent is (1.0-1.5):1.
[0007] Furthermore, the polyetheramine prepolymer modified E-54 epoxy resin is prepared by prepolymerizing E-54 epoxy resin and polyetheramine at a mass ratio of 90:10 and in the presence of 0.5 parts of accelerator at 80°C for 120-150 min. The polyetheramine has a number average molecular weight of 1000-3000 and the accelerator is DMP-30.
[0008] Furthermore, epoxy-functionalized hyperbranched polyester is prepared by hydroxyl-terminated hyperbranched polyester via epoxy ring closure; Hydroxyl-terminated hyperbranched polyester is prepared by esterification and polycondensation of pentaerythritol as the core and 2,2-dimethylolpropionic acid as the AB2-type branching monomer, with a molar ratio of pentaerythritol to 2,2-dimethylolpropionic acid of 1:(8-10). The number average molecular weight of the hydroxyl-terminated hyperbranched polyester is 1700-2300 g / mol, and the degree of branching is 0.48-0.53. The epoxy value of epoxy-functionalized hyperbranched polyester is 0.35-0.50 mol / 100g.
[0009] Furthermore, the epoxy ring-closure process involves mixing hydroxyl-terminated hyperbranched polyester with epichlorohydrin at a molar ratio of hydroxyl to epichlorohydrin of 1:(15-22). After mixing, the mixture is subjected to ring-opening esterification at 100℃ for 3 h under tetrabutylammonium bromide catalysis. The temperature is then lowered to 45-55℃, and 40wt% NaOH aqueous solution is added dropwise until the molar ratio of NaOH to hydroxyl is (1.05)-(1.25:1). After the addition is complete, the mixture is kept at this temperature for ring closure for 3 h. After post-treatment, the epoxy-functionalized hyperbranched polyester is obtained. The dropwise addition time of the NaOH aqueous solution is 30-60 min, and the epoxy value of the epoxy-functionalized hyperbranched polyester is 0.35-0.50 mol / 100g.
[0010] Furthermore, the weight parts of the main agent are as follows: 30-40 parts of flexible segment prepolymer modified epoxy resin, 5-30 parts of epoxy functionalized hyperbranched polyester, 20-40 parts of phenolic epoxy resin F-51, and 0-20 parts of organosilicon modified epoxy diluent. The curing agent comprises, by weight: 60-90 parts of hexafunctional polythiol, 1-5 parts of 2,4,6-tris(dimethylaminomethyl)phenol accelerator, and 2-5 parts of polymerization inhibitor; The hexafunctional polythiol is one of Capcure 3-800, Capcure 3830-81, Capcure 40secHV, EpomateQX-10, and EH-316; The polymerization inhibitor is one or more combinations of MTBHQ, hydroquinone, and mercaptoacetic acid; Organosilicon-modified epoxy diluent is one of mono- or di-epoxy organosilicon epoxy diluents. Organosilicon-modified epoxy diluent is used to reduce the viscosity of the system to ≤0.7 Pa·s (60℃).
[0011] Furthermore, high-strength and high-toughness epoxy adhesives serve as alternatives to spirocyclic polyether 123 resin in precision electronic packaging and metal-composite bonding.
[0012] Furthermore, this invention also proposes a method for preparing a high-strength, high-toughness epoxy adhesive, comprising: Step 1: Ring-opening prepolymerization of E-54 epoxy resin and polyetheramine is carried out to obtain polyetheramine prepolymer modified E-54 epoxy resin. Step 2: Prepare epoxy-functionalized hyperbranched polyester using a two-step method; Step 3: Mix phenolic epoxy resin, polyetheramine prepolymer modified E-54 epoxy resin and epoxy functionalized hyperbranched polyester to obtain the main agent; Step 4: Mix the multifunctional polythiol, accelerator and inhibitor to obtain the curing agent; Step 5: Mix the main agent and the curing agent according to the set ratio to obtain a high-strength and high-toughness epoxy adhesive.
[0013] Furthermore, the two-step method in step 2 includes the sequential synthesis of hydroxyl-terminated hyperbranched polyester and epoxy ring closure. The synthesis of hydroxyl-terminated hyperbranched polyesters includes: Using pentaerythritol as the core and 2,2-dimethylolpropionic acid as the AB2-type branched monomer, the reaction was carried out at 140-150℃ and atmospheric pressure for 2 h under the catalysis of p-toluenesulfonic acid, wherein the molar ratio of pentaerythritol to 2,2-dimethylolpropionic acid was 1:(8-10). After the reaction at atmospheric pressure, the reaction was carried out under reduced pressure of 0.02-0.04 MPa for 2 h until the acid value endpoint was ≤5 mg KOH / g, to obtain hydroxyl-terminated hyperbranched polyester; Closed-ring epoxy includes: Hydroxyl-terminated hyperbranched polyester was mixed with epichlorohydrin at a molar ratio of 1:(15-22). After mixing, the mixture was ring-opened and esterified at 100℃ for 3 h under the catalysis of tetrabutylammonium bromide. The temperature was then lowered to 45-55℃, and 40 wt% NaOH aqueous solution was added dropwise until the molar ratio of NaOH to hydroxyl was 1.05-1.25:1. After the addition was complete, the mixture was kept at the temperature for ring closure for 3 h. After the temperature was maintained, the epoxy-functionalized hyperbranched polyester was obtained through post-treatment.
[0014] Furthermore, step 3 specifically includes: The reactor is heated to 80°C. Phenolic epoxy resin F-51 is added to the reactor and dried for 2-3 hours to remove water. After water removal, epoxy functionalized hyperbranched polyester, polyetheramine prepolymer modified E-54 epoxy resin and organosilicon modified epoxy diluent are added to the reactor in sequence. After stirring for 1 hour, the temperature is lowered to 30°C to obtain the main agent.
[0015] Furthermore, in step 4, hexafunctional polythiol is added to the reactor as a base material, and an accelerator and a polymerization inhibitor are added to the reactor. The mixture is stirred for 0.5 hours to obtain a curing agent, wherein the accelerator is DMP-30.
[0016] In step 5, the main agent and curing agent are weighed at a mass ratio of (1.0-1.5):1, and stirred at low speed for 30 minutes to mix evenly to obtain a high-strength and high-toughness epoxy adhesive.
[0017] The beneficial effects of this invention are: (1) In this invention, polyetheramine and E-54 epoxy resin are pre-ring-opened and prepolymerized, so that the flexible long chain is covalently embedded in the epoxy skeleton. The resulting polyetheramine prepolymerized modified E-54 epoxy resin has both the entropy elasticity of the flexible chain segment and the reactivity of the epoxy matrix, which improves the polarity of the system and the adhesion performance to the metal shell.
[0018] (2) The present invention uses epoxy-functionalized hyperbranched polyester and phenolic epoxy resin F-51 to induce crack deflection and absorb impact energy by utilizing the topological cavity and branched chain segments of hyperbranched polyester. At the same time, the high-functionality aromatic ring skeleton of F-51 provides rigidity and compensates for heat resistance, forming a rigid-flexible gradient structure, which simultaneously improves the tensile strength and elongation at break of the adhesive.
[0019] (3) The present invention uses hexafunctional polythiol as curing agent. Its multi-thiol and epoxy groups open the ring to form a high cross-linking density network. The sulfur-containing chain segments also give the cross-linking network flexibility, so that the system achieves a balance between high cross-linking and high strength and high flexibility and high toughness of sulfide. With the addition of accelerator, medium temperature curing can be achieved. The room temperature open time can be adjusted in the range of 1-240 min, avoiding the problems of easy chain termination and narrow process window of 123 resin cationic curing.
[0020] (4) Through the above three-level synergistic effect, the two-component epoxy adhesive obtained by the present invention has a tensile strength of up to 35MPa, an elongation at break of ≥60%, an impact strength of ≥90J / m", and a viscosity as low as 0.2Pa·s at 60℃. It has excellent molding processability and comprehensive mechanical properties, and can completely replace spirocyclic polyether 123 resin. It is suitable for precision electronic packaging and metal-composite bonding and other scenarios with comprehensive requirements for density, toughness and adhesion. Attached Figure Description
[0021] Figure 1This is a flowchart of a method for preparing a high-strength, high-toughness epoxy adhesive. Detailed Implementation
[0022] The high-strength, high-toughness epoxy adhesive described in this embodiment consists of a main agent and a curing agent: The main component, by weight, consists of: 30-40 parts of polyetheramine prepolymer modified E-54 epoxy resin, 5-30 parts of epoxy functionalized hyperbranched polyester HBEP, 20-40 parts of phenolic epoxy resin F-51, and 0-20 parts of silicone-modified epoxy diluent; the curing agent, by weight, consists of: 60-90 parts of hexafunctional polythiol, 1-5 parts of 2,4,6-tris(dimethylaminomethyl)phenol accelerator, and 2-5 parts of polymerization inhibitor; the mass ratio of the main component to the curing agent is 1.0-1.5:1. The polyetheramine prepolymer modified E-54 epoxy resin was prepared by prepolymerizing E-54 and polyetheramine (Mn=1000-3000) at a mass ratio of 90:10 in the presence of 0.5 parts of DMP-30 at 80°C for 120-150 min.
[0023] Epoxy-functionalized hyperbranched polyester HBEP was prepared by a two-step method: (a) Synthesis of hydroxyl-terminated hyperbranched polyester: Using pentaerythritol as the core and 2,2-dimethylolpropionic acid as the AB2-type branching monomer, the molar ratio of pentaerythritol to 2,2-dimethylolpropionic acid is 1:(8-10). The reaction is carried out at 140-150℃ and atmospheric pressure for 2 h under the catalysis of p-toluenesulfonic acid, and then the reaction is carried out under reduced pressure of 0.02-0.04 MPa for 2 h. The acid value endpoint is ≤5 mg KOH / g to obtain hydroxyl-terminated hyperbranched polyester with a number average molecular weight of 1700-2300 g / mol and a branching degree of 0.48-0.53. (b) Epoxy ring closure: The product of step (a) is mixed with epichlorohydrin at a hydroxyl:epoxychlorohydrin molar ratio of 1:(15-22), and esterified at 100℃ for 3 h under tetrabutylammonium bromide catalysis. The temperature is then lowered to 45-55℃, and 40 wt% NaOH aqueous solution is added dropwise to make the NaOH:hydroxyl molar ratio 1.05-1.25:1. After the addition is complete, the temperature is maintained for 3 h to close the ring. The post-treatment yields an epoxy-functionalized hyperbranched polyester with an epoxy value of 0.35-0.50 mol / 100g. The NaOH aqueous solution is added dropwise for 30-60 min.
[0024] The hexafunctional polythiol is selected from one of Capcure 3-800, Capcure 3830-81, Capcure 40secHV, Epomate QX-10, and EH-316. The polymerization inhibitor is one or a combination of MTBHQ, hydroquinone, and mercaptoacetic acid. The silicone-modified epoxy diluent is a mono- or di-epoxy silicone epoxy diluent used to reduce the system viscosity to ≤0.7 Pa·s@(60℃).
[0025] This implementation method achieves its goals through the following three-level coordination: Synergistic ① Pre-ring-opening modification of E-54 with polyetheramine to form a flexible long-chain prepolymer; Polyetheramine (Mn=1000-3000, preferably 2000) and E-54 are prepolymerized at 80°C with a ratio of 90:10 under DMP-30 catalysis, resulting in long-chain flexible blocks with epoxy groups at both ends. Unlike CN105238316B, which uses polyetheramine D-400 as a curing agent component in the blend, this invention covalently integrates polyetheramine into the epoxy backbone, preserving the entropy elasticity of the flexible segments while avoiding the introduction of excessive amino groups on the curing agent side, which could lead to yellowing and embrittlement of the system.
[0026] Synergistic ② Constructing a "topology toughening-rigid skeleton" gradient using epoxy functionalized HBEP + phenolic F-51; A self-made HBEP (Mn=1700-2300, branching degree 0.5) terminal epoxy and F-51 high-functionality aromatic ring backbone form a rigid-flexible gradient of "soft topological cavity + hard aromatic ring crosslinking": the nanocavity of HBEP induces crack deflection and the branched segments absorb impact energy; F-51 provides high-density benzene ring rigidity to compensate for the heat loss caused by the introduction of HBEP. When the mass ratio of the two is controlled at HBEP:F-51=0.125-1.5:1 (i.e. HBEP 5-30 / F-51 20-40), the tensile strength and elongation at break are improved simultaneously (see Examples 1 vs 4).
[0027] Synergistic effect ③: High cross-linking of hexafunctional polythiol + sulfur-containing flexible segments achieve rapid curing at medium temperature; Hexafunctional polythiols (such as Capcure 3-800) have 6 -SH bonds per molecule, which form a highly cross-linked network after ring-opening with epoxy. At the same time, the -S-C- bonds themselves are flexible, allowing the system to achieve a balance between "high cross-linking → high strength" and "thioether flexibility → high toughness". With the addition of DMP-30 accelerator, it is possible to achieve an adjustable room temperature operating time of 1-240 min and a medium temperature (60-80℃) curing time of several hours, avoiding the chain termination risk of cationic curing of 123 resin.
[0028] Example 1 1) Hydroxyl-terminated hyperbranched polyester (HBPE) synthesis stage; A three-necked flask was equipped with a mechanical stirrer, an N2 inlet, and a condenser with a drying tube. 1.36 g (10 mmol) of pentaerythritol and 16.34 g (90 mmol) of DMPA were weighed, i.e., a molar ratio of pentaerythritol:DMPA = 1:9. 0.082 g of p-toluenesulfonic acid catalyst (0.5% of the DMPA feed mass) was added. Under N2 protection and mechanical stirring, the temperature was raised to 145±5℃ and reacted at atmospheric pressure for 2 h (this stage involves esterification and dehydration; the acid value was monitored every 30 min by KOH-EtOH titration; when the acid value dropped to ≤20 mg KOH / g, the next step was initiated). Then, the N2 was turned off, the three-necked flask was sealed, and the pressure was reduced to 1.2 kPa, and the reaction continued for another 2 h. Ten minutes before the end of the reaction, a sample was taken to check the acid value, which was ≤5 mg KOH / g. Heating was stopped, N2 was introduced to release the pressure, and the temperature was lowered to below 80℃ before discharging. A colorless, transparent, viscous liquid, HBPE-2, was obtained, with a yield >92%. Characterization: GPC (THF, PS standard) analysis showed Mn ≈ 1950 g / mol. ≈1.38; FT-IR: 1728 cm -1 (Ester C=O), 3470 cm -1 (-OH); ¹H NMR (DMSO-d6) calculated by Fréchet method: DB = (D+T) / (D+T+L) ≈ 0.51; hydroxyl value was determined to be 0.48-0.52 mol / 100g according to GB / T 12008.3.
[0029] 2) Epoxy closed-loop segment; The three-necked flask is equipped with a mechanical stirrer, a constant-pressure dropping funnel, a condenser, and an N2 inlet. Weigh the above-mentioned HBPE-2 (hydroxyl value 0.50 mol / 100g, equivalent to approximately 0.32 mol of hydroxyl molar amount) into the three-necked flask, add 180 g (approximately 1.95 mol) of epichlorohydrin (ECH), i.e., ECH:hydroxyl molar ratio ≈ 18:1, and then add 0.64 g of tetrabutylammonium bromide (TBAB) (2% of the HBPE mass) as a phase transfer catalyst. Pour N2 through the flask, heat to 100℃, and perform a ring-opening esterification reaction at atmospheric pressure for 3 h (during this stage, the terminal -OH group of HBPE ring-opens with ECH to form a chlorohydrin intermediate).
[0030] The temperature was then lowered to 50°C, and 40 wt% NaOH aqueous solution (NaOH to hydroxyl molar ratio 1.15:1, approximately 14.7 g of 40% NaOH solution) was added dropwise using a constant pressure dropping funnel. The dropping rate was controlled at 1-2 drops / second, and the temperature was maintained at 48-52°C during the dropping process. After the dropping was completed, the reaction was kept at this temperature for 3 hours (closed-loop stage).
[0031] After the reaction was completed, a post-treatment step was performed, which included: cooling to room temperature, adding 150 mL of deionized water to stop the reaction, transferring to a separatory funnel, allowing the layers to separate, discarding the lower brine phase; washing the organic phase twice with saturated NaCl solution, and then washing with deionized water until pH≈7; drying with anhydrous Na2SO4 for 12 h; and removing excess ECH by vacuum distillation to obtain a pale yellow viscous liquid HBEP-EPOX, i.e., epoxy binder, with a yield of ≈78%. The temperature during distillation was 60℃ and the pressure was 0.02 MPa.
[0032] Characterization: FT-IR: 910 cm⁻¹ -1 850 cm -1 Characteristic absorption of epoxy three-membered rings is observed at 3470 cm⁻¹. -1 (-OH) significantly reduced; epoxy value measured according to GB / T 1677-2008 Method B (hydrochloric acid-pyridine) was 0.41-0.43 mol / 100g; GPC Mn≈2100g / mol, ≈1.42;¹H NMR confirmed that the terminal epoxy group content was >85%.
[0033] Comparative Example 1 Pentaerythritol:DMPA = 1:6 (low branching degree DB≈0.38), the rest is the same as in Example 1, and the results are as follows: epoxy value 0.38mol / 100g, Mn 1450g / mol, which proves the necessity of feeding 1:8-10.
[0034] Comparative Example 2 The closed-loop reaction was performed by adding NaOH solid in batches instead of dropwise, with the rest following the same procedure as in Example 1. The results are as follows: epoxy value only 0.28 mol / 100g, FT-IR 550 cm⁻¹ -1 The appearance of a secondary peak (polyether chain) demonstrates the importance of "droplet addition".
[0035] Example 2 like Figure 1 As shown, the preparation method of a high-strength and high-toughness epoxy adhesive described in this embodiment includes the following steps: (1) Preparation of the main agent: At room temperature, the reaction vessel is first heated to 80°C, and 40g of phenolic epoxy resin F-51 is added into the reaction vessel and dried for 2-3 hours. Then, 30g of HBEP-EPOX prepared according to Example 1, 40g of self-made polyetheramine modified E-54 epoxy resin and 20g of organosilicon modified epoxy diluent are added into the reaction vessel in proportion. After stirring for 1 hour, the temperature is lowered to 30°C and the material is discharged to obtain the main agent. (2) Preparation of curing agent: 90g of hexafunctional thiol was added into the reactor in proportion, and 5g of accelerator DMP-30 and 5g of polymerization inhibitor MTBHQ were added in proportion. The mixture was stirred for 0.5h to make it uniform, and then discharged to obtain the curing agent. (3) Preparation of epoxy adhesive: According to the mixing ratio (by weight) main agent: curing agent = 1.3:1, accurately weigh the main agent and curing agent, stir for 30 minutes under low speed mixer to make the main agent and curing agent evenly mixed, and obtain the adhesive.
[0036] Example 3 (1) Preparation of the main agent: At room temperature, the reaction vessel is first heated to 80°C, and 40g of phenolic epoxy resin F-51 is added into the reaction vessel and dried for 2-3 hours. Then, 30g of HBEP-EPOX prepared according to Example 1 and 40g of self-made polyetheramine modified E-54 epoxy resin are added into the reaction vessel in proportion. After stirring for 1 hour, the temperature is lowered to 30°C and the material is discharged to obtain the main agent. (2) Preparation of curing agent: 90g of hexafunctional thiol was added into reactor No. 2 according to the proportion, and 5g of accelerator DMP-30 and 5g of polymerization inhibitor MTBHQ were added according to the proportion. The mixture was stirred for 0.5h to make it uniform, and then discharged to obtain the curing agent. (3) Preparation of epoxy adhesive: According to the mixing ratio (by weight) main agent: curing agent = 1.1:1, accurately weigh the main agent and curing agent, stir in a low speed mixer for 30 minutes to make the main agent and curing agent evenly mixed, and obtain the adhesive.
[0037] Example 4 (1) Preparation of the main agent: At room temperature, the No. 1 reactor was first heated to 80°C, and 30g of phenolic epoxy resin F-51 was added into the reactor and dried for 2-3 hours. Then, 20g of HBEP-EPOX prepared according to Example 1, 30g of self-made polyetheramine modified E-54 epoxy resin and 10g of organosilicon modified epoxy diluent were added into the reactor in proportion. After stirring for 1 hour, the temperature was lowered to 30°C and the material was discharged to obtain the main agent. (2) Preparation of curing agent: 70g of hexafunctional thiol was added into reactor No. 2 according to the proportion, and 2g of accelerator DMP-30 and 3g of mercaptoacetic acid were added according to the proportion. The mixture was stirred for 0.5h to make it uniform, and then discharged to obtain the curing agent. (3) Preparation of epoxy adhesive: According to the mixing ratio (by weight) main agent: curing agent = 1.2:1, accurately weigh the main agent and curing agent, and stir them in a low-speed mixer for 30 minutes to make the main agent and curing agent evenly mixed to obtain the adhesive. Example 5 (1) Preparation of the main agent: At room temperature, the reaction vessel is first heated to 80°C, and 40g of phenolic epoxy resin F-51 is added into the reaction vessel and dried for 2-3 hours. Then, 40g of self-made polyetheramine modified E-54 epoxy resin and 10g of organosilicon modified epoxy diluent are added into the reaction vessel in proportion. After stirring for 1 hour, the temperature is lowered to 30°C and the material is discharged to obtain the main agent. (2) Preparation of curing agent: 70g of hexafunctional thiol was added into reactor No. 2 according to the proportion, and 2g of accelerator DMP-30 and 3g of mercaptoacetic acid were added according to the proportion. The mixture was stirred for 0.5h to make it uniform, and then discharged to obtain the curing agent. (3) Preparation of epoxy adhesive: According to the mixing ratio (by weight) main agent: curing agent = 1.2:1, accurately weigh the main agent and curing agent, and stir them in a low-speed mixer for 30 minutes to make the main agent and curing agent evenly mixed to obtain the adhesive. Comparison Example 1: (No polyetheramine prepolymer, replaced with E-54 + polyetheramine D-400 blended into the main agent): The formulation was the same as in Example 2, but E-54 was not prepolymerized, and 4 parts of polyetheramine D-400 were blended into the main agent as a diluent. Results: tensile strength 28 MPa (↓20%), elongation at break 42% (↓30%), impact strength 65 J / m (↓28%) – demonstrating the essential difference between "pre-ring-opening prepolymerization" and blending.
[0038] Comparative Example 2: (No HBEP, 0 parts hyperbranched epoxy, F-51 increased to 70 parts): The approach is the same as in Example 5, but with the addition of F-51. Results: Tensile strength 31 MPa, elongation at break 18% (↓51%), impact strength 45 J / m (↓34%) – demonstrating the irreplaceable toughness of HBEP.
[0039] Compare with Example 3: (Polythiol replaced with trifunctional Capcure WR-6): Same as Example 2, but with the curing agent replaced by trifunctional polythiol. Results: Tensile strength 24 MPa (↓31%), open time shortened to 45 min—demonstrating the dual contribution of hexafunctional polythiol to strength and operating time.
[0040] The epoxy adhesives and 123 resins prepared in the examples and control examples were subjected to performance comparison tests, and the test results are shown in Table 1.
[0041] Table 1
[0042] As can be seen from the table above, the epoxy adhesives prepared in Examples 1-5, compared with resin 123, exhibit superior molding processability, excellent mechanical strength, and a longer working time, achieving the expected goals. Furthermore, compared with control examples C1-C3, only the complete three-stage synergy (i.e., Example 2) simultaneously achieves "tensile strength ≥35MPa, elongation at break ≥60%, and impact strength ≥90J / m," with any missing component resulting in a significant performance drop.
[0043] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent substitutions, and improvements made to the above embodiments without departing from the scope of the present invention, based on the technical essence of the present invention and within the spirit and principles of the present invention, shall still fall within the protection scope of the present invention.
Claims
1. A high-strength, high-toughness epoxy adhesive, characterized in that, The epoxy adhesive consists of a base agent and a curing agent; The main agent includes polyetheramine prepolymer modified E-54 epoxy resin, epoxy-functionalized hyperbranched polyester and phenolic epoxy resin. The curing agent includes multifunctional polythiols, accelerators, and polymerization inhibitors; The mass ratio of the main agent to the curing agent is (1.0-1.5):
1.
2. The high-strength, high-toughness epoxy adhesive according to claim 1, characterized in that, The polyetheramine prepolymer modified E-54 epoxy resin is prepared by prepolymerizing E-54 epoxy resin and polyetheramine at a mass ratio of 90:10 and in the presence of 0.5 parts of accelerator at 80°C for 120-150 min. The number average molecular weight of the polyetheramine is 1000-3000 and the accelerator is DMP-30.
3. The high-strength, high-toughness epoxy adhesive according to claim 1, characterized in that, The epoxy-functionalized hyperbranched polyester is prepared by hydroxyl-terminated hyperbranched polyester via epoxy ring closure; The hydroxyl-capped hyperbranched polyester is formed by esterification and polycondensation of pentaerythritol as the core and 2,2-dimethylolpropionic acid as the AB2-type branching monomer, with a molar ratio of pentaerythritol to 2,2-dimethylolpropionic acid of 1:(8-10). The number average molecular weight of the hydroxyl-capped hyperbranched polyester is 1700-2300 g / mol, and the degree of branching is 0.48-0.
53. The epoxy value of the epoxy-functionalized hyperbranched polyester is 0.35-0.50 mol / 100g.
4. The high-strength, high-toughness epoxy adhesive according to claim 3, characterized in that, The epoxy ring-closure is achieved by mixing hydroxyl-terminated hyperbranched polyester and epichlorohydrin at a molar ratio of hydroxyl to epichlorohydrin of 1:(15-22). After mixing, the mixture is subjected to ring-opening esterification at 100°C for 3 hours under the catalysis of tetrabutylammonium bromide. The temperature is then lowered to 45-55°C, and 40wt% NaOH aqueous solution is added dropwise until the molar ratio of NaOH to hydroxyl is (1.05)-(1.25:1). After the addition is complete, the mixture is kept at this temperature for 3 hours to close the ring. After post-treatment, epoxy-functionalized hyperbranched polyester is obtained. The dropwise addition time of NaOH aqueous solution is 30-60 minutes, and the epoxy value of the epoxy-functionalized hyperbranched polyester is 0.35-0.50 mol / 100g.
5. The high-strength, high-toughness epoxy adhesive according to claim 1, characterized in that, The main agent is expressed in parts by weight as follows: 30-40 parts of flexible segment prepolymer modified epoxy resin, 5-30 parts of epoxy functionalized hyperbranched polyester, 0-40 parts of phenolic epoxy resin F-512, and 0-20 parts of organosilicon modified epoxy diluent. The curing agent comprises, by weight: 60-90 parts of hexafunctional polythiol, 1-5 parts of 2,4,6-tris(dimethylaminomethyl)phenol accelerator, and 2-5 parts of polymerization inhibitor. The hexafunctional polythiol is one of Capcure 3-800, Capcure 3830-81, Capcure 40secHV, Epomate QX-10, and EH-316; The polymerization inhibitor is one or more of MTBHQ, hydroquinone, and mercaptoacetic acid; The silicone-modified epoxy diluent is one of mono-epoxy or di-epoxy silicone epoxy diluents, and is used to reduce the viscosity of the system to ≤0.7 Pa·s (60℃).
6. A high-strength, high-toughness epoxy adhesive according to any one of claims 1-5, characterized in that, The high-strength and high-toughness epoxy adhesive is a substitute for spirocyclic polyether 123 resin in precision electronic packaging and metal-composite bonding.
7. A method for preparing a high-strength, high-toughness epoxy adhesive, applied to the high-strength, high-toughness epoxy adhesive according to any one of claims 1-6, characterized in that, include: Step 1: Ring-opening prepolymerization of E-54 epoxy resin and polyetheramine is carried out to obtain polyetheramine prepolymer modified E-54 epoxy resin. Step 2: Prepare epoxy-functionalized hyperbranched polyester using a two-step method; Step 3: Mix phenolic epoxy resin, polyetheramine prepolymer modified E-54 epoxy resin and epoxy functionalized hyperbranched polyester to obtain the main agent; Step 4: Mix the multifunctional polythiol, accelerator and inhibitor to obtain the curing agent; Step 5: Mix the main agent and the curing agent according to the set ratio to obtain the high-strength and high-toughness epoxy adhesive.
8. The method for preparing a high-strength, high-toughness epoxy adhesive according to claim 7, characterized in that, Step 2, a two-step process, includes the sequential synthesis of hydroxyl-terminated hyperbranched polyester and epoxy ring closure. The synthesis of the hydroxyl-terminated hyperbranched polyester includes: Using pentaerythritol as the core and 2,2-dimethylolpropionic acid as the AB2-type branched monomer, the reaction was carried out at 140-150℃ and atmospheric pressure for 2 hours under the catalysis of p-toluenesulfonic acid, wherein the molar ratio of pentaerythritol to 2,2-dimethylolpropionic acid was 1:(8-10). After the reaction at atmospheric pressure, the reaction was carried out under reduced pressure of 0.02-0.04 MPa for 2 hours until the acid value endpoint was ≤5 mg KOH / g, to obtain hydroxyl-terminated hyperbranched polyester; The epoxy closed-ring includes: Hydroxyl-terminated hyperbranched polyester and epichlorohydrin were mixed at a hydroxyl:epicochlorohydrin molar ratio of 1:(15-22). After mixing, the mixture was ring-opened and esterified at 100℃ for 3 hours under the catalysis of tetrabutylammonium bromide. The temperature was then lowered to 45-55℃, and 40wt% NaOH aqueous solution was added dropwise until the NaOH:hydroxyl molar ratio was 1.05-1.25:
1. After the addition was complete, the mixture was kept at the temperature for ring closure for 3 hours. After the temperature was maintained, the epoxy-functionalized hyperbranched polyester was obtained through post-treatment.
9. The method for preparing a high-strength, high-toughness epoxy adhesive according to claim 7, characterized in that, Step 3 specifically includes: The reactor is heated to 80°C. Phenolic epoxy resin F-51 is added to the reactor and dried for 2-3 hours to remove water. After water removal, epoxy functionalized hyperbranched polyester, polyetheramine prepolymer modified E-54 epoxy resin and organosilicon modified epoxy diluent are added to the reactor in sequence. After stirring for 1 hour, the temperature is lowered to 30°C to obtain the main agent.
10. The method for preparing a high-strength, high-toughness epoxy adhesive according to claim 7, characterized in that, In step 4, hexafunctional polythiol is added to the reactor as a base material, and an accelerator and a polymerization inhibitor are added to the reactor. The mixture is stirred for 0.5 hours to obtain the curing agent, wherein the accelerator is DMP-30. In step 5, the main agent and curing agent are weighed at a mass ratio of (1.0-1.5):1, and stirred at low speed for 30 minutes to mix evenly to obtain a high-strength and high-toughness epoxy adhesive.
Citation Information
Patent Citations
Epoxy resin material toughened by nanometer silica and preparation method thereof
CN102190858A
Low-temperature curing two-component epoxy stone dry-hanging adhesive and its preparation method
CN105238316B
Castor oil based hyperbranched epoxy resin and preparation method and applications thereof
CN109897175A
A one-component low-temperature epoxy adhesive and its preparation method
CN113999637B
Single-component epoxy-thiol system adhesive and preparation method thereof