Flexible expanded graphite seal material and method of forming same

By combining grafted modified expanded graphite with dual-response microcapsules, a three-layer core-shell structure sealing material is formed, which solves the problems of easy oxidation and weight loss and pore leakage of flexible expanded graphite at high temperatures, realizes dynamic self-repair and long-term sealing, and improves the overall performance of the material.

CN123131985APending Publication Date: 2026-11-20LIAONING GLORY SPECIAL GRAPHITE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611636482.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-22
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing flexible expanded graphite sealing materials are prone to oxidation and weight loss at high temperatures, resulting in pore leakage and an inability to self-heal. Traditional chemical cross-linking modification makes the materials brittle and cannot meet the requirements for long-term dynamic sealing.

Method used

A three-layer core-shell structured sealing material is formed by combining grafted modified expanded graphite with dual-response microcapsules. The inner aqueous phase contains an antioxidant precursor, the middle oil phase contains a low-melting-point phase change material, and the outer layer consists of a dynamic covalent network and a calcium alginate ion network. It is prepared using microfluidic technology to achieve dynamic self-healing and high-temperature antioxidant properties.

Benefits of technology

It achieves dynamic self-healing, oxidation resistance and long-term sealing of sealing materials at high temperatures, overcomes the problems of pore leakage and oxidation weight loss, and improves the mechanical strength and resilience of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The application discloses a kind of flexible expanded graphite sealing material and its forming method, belong to sealing material technical field.The sealing material is made of grafting modification expanded graphite and double response microcapsule composition, wherein grafting modification expanded graphite surface bonding has the covalent network containing dynamic disulfide bond, microcapsule has inner water phase core material, intermediate oil layer containing phenyl silicone oil and double network hydrogel shell layer.Forming time mould pressing pressure makes microcapsule break and release phenyl silicone oil filling graphite pore, realize instant sealing;Service temperature triggers phenyl silicone oil slow-release after double temperature control barrier, while antioxidant precursor in core material generates B2O3-SiO2-AlPO4-based ceramic film in situ, and the material bulk phase self-passivating ability is endowed.The sealing material has self-repair, low leakage rate and excellent high-temperature oxidation resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sealing materials technology, and in particular to a flexible expanded graphite sealing material and its molding method. Background Technology

[0002] Flexible expandable graphite sealing materials are widely used in static sealing applications in the petroleum, chemical, and nuclear power industries due to their excellent compression resilience, corrosion resistance, and radiation resistance. However, these sealing materials suffer from the following three main technical shortcomings in actual service: First, pore leakage is a significant problem, and existing impregnation modifications lack dynamic self-healing capabilities. Expanded graphite, after high-temperature expansion, forms a loose, porous, worm-like structure. While this structure imparts good compressive resilience to the material, it also results in numerous micron-sized pores within it. When the sealing medium is gas, these pores constitute permeation channels for gas leakage. Existing technologies typically use methods such as impregnation with polytetrafluoroethylene (PTFE) emulsions or phenolic resins to fill these pores and prevent leakage. However, PTFE begins to decompose at approximately 380°C, and phenolic resins, after curing, make the material brittle and significantly reduce its resilience. More importantly, these impregnating agents are all static fillers; when new micro-gaps are created due to flange thermal expansion and contraction or mechanical vibration, they cannot actively migrate for secondary sealing, making it difficult to meet the long-term dynamic sealing requirements under complex operating conditions.

[0003] Secondly, it exhibits poor high-temperature oxidation resistance, and existing protective mechanisms are passive surface protection. In high-temperature, oxygen-rich environments, flexible graphite undergoes significant oxidative weight loss when temperatures exceed 450°C, leading to structural damage and seal failure. Existing technologies primarily enhance oxidation resistance through surface coatings (such as phosphates, borates, and boron nitrides). However, these exogenous coatings have weak adhesion to the graphite matrix and are easily peeled off under thermal shock and long-term mechanical vibration; moreover, once the coating is partially damaged, it loses its protective function and cannot achieve self-repair. Furthermore, surface coatings are insufficient to prevent oxygen from penetrating and oxidizing through the micropores within the graphite, constituting a passive and non-persistent protection mechanism.

[0004] Finally, traditional chemical crosslinking modification struggles to balance the mechanical strength and dynamic resilience of the matrix. To improve the structural stability of sealing materials, existing technologies attempt to chemically modify expanded graphite by introducing resins or crosslinking agents. However, traditional covalent crosslinking networks typically form irreversible rigid structures. While this increases the material's strength, it severely sacrifices the original flexibility and compressive resilience of graphite. Furthermore, the crosslinking network is prone to irreversible degradation at high temperatures, making it impossible to achieve stress relaxation and self-healing during service.

[0005] Therefore, there is an urgent need to develop a flexible expanded graphite sealing material that combines long-lasting dynamic sealing capability, endogenous high-temperature oxidation protection, and a matrix with high strength, toughness, and self-healing function. Summary of the Invention

[0006] The purpose of this invention is to address the shortcomings of existing technologies by proposing a flexible expandable graphite sealing material and its molding method.

[0007] To achieve the above objectives, the present invention adopts the following technical solution: A flexible expanded graphite sealing material, comprising the following components by weight: 100 parts of graft-modified expanded graphite; 10-50 portions of dual-response microcapsules; The grafted modified expanded graphite is formed by grafting epoxy-modified expanded graphite with a dynamic covalent network polymer via covalent bonds. The dynamic covalent network polymer is formed by cross-linking bisphenol A diglycidyl ether, 3,3'-dithiodipropionic acid and sebacic acid through a ring-opening esterification reaction of epoxy and carboxyl groups, and the polymer network backbone contains dynamic disulfide bonds. The dual-response microcapsule has a three-layer core-shell structure, consisting of, from the inside out: an inner aqueous core containing an antioxidant precursor, an intermediate oil layer containing phenyl silicone oil and a low-melting-point phase change material, and a dual-network hydrogel shell composed of a poly(N-isopropylacrylamide-polyethylene glycol diacrylate) covalent crosslinked network and a calcium alginate ion network.

[0008] Preferably, the molar ratio of sebacic acid to 3,3'-dithiodipropionic acid is 1:0.1-50.

[0009] Sebacic acid provides a flexible, long-chain structure, which is beneficial for imparting flexibility and high resilience to the network; 3,3'-dithiodipropionic acid provides dynamic disulfide bonds, giving the network dynamic exchange capacity. The molar ratio of the two can be adjusted within a wide range of 1:0.1-50 to meet the requirements of mechanical properties and self-healing properties in different application scenarios. By adjusting the ratio of sebacic acid to 3,3'-dithiodipropionic acid, the glass transition temperature and stress relaxation behavior of the covalently cross-linked network can be effectively controlled, thereby achieving a balance between mechanical strength and self-healing properties in grafted modified expanded graphite.

[0010] Preferably, the method for preparing the dual-response microcapsules includes the following steps: (1) Preparation of each phase: a) Preparation of the internal aqueous phase: Weigh out 5-20% nano zinc borate, 10-25% aluminum dihydrogen phosphate liquid, 3-15% tetraethyl orthosilicate, 2-8% ethanol, 0.5-3% Tween 80, and 0.2-2% polyethylene glycol 400 by mass percentage, with the remainder being deionized water; add nano zinc borate and polyethylene glycol 400 to the deionized water and ultrasonically disperse in an ice bath for 30-60 min; add aluminum dihydrogen phosphate liquid, ethanol, and Tween 80, and magnetically stir for 20-40 min; slowly add tetraethyl orthosilicate dropwise while stirring, and continue magnetically stirring for 30-60 min after the addition is complete; adjust the pH to 4.0-5.0, filter and degas to obtain the internal aqueous phase; b) Preparation of the intermediate oil phase: Weigh out 5-15% low-melting-point phase change material, 2-20% hydrophobically modified nano zinc borate, and 0.2-5% Span 80 by mass percentage, with the balance being phenyl silicone oil; mix the above components, heat to 50-70℃ and stir, ultrasonically disperse for 20-40 min; homogenize at 10000-15000 rpm for 3-5 min and then degas under vacuum to obtain the intermediate oil phase; c) Preparation of the external aqueous phase: Weigh out 3-25% N-isopropylacrylamide, 3-15% polyethylene glycol diacrylate, 0.5-3% sodium alginate, 0.2-2% photoinitiator, and 0.5-3% polyvinyl alcohol by mass percentage, with the remainder being deionized water; stir and dissolve in the dark, then filter to obtain the external aqueous phase; d) Preparation of continuous oil phase: Weigh out 1-8% of Span 80 by mass percentage, with the remainder being liquid paraffin, and mix thoroughly to obtain a continuous oil phase; (2) Microfluidic generation of four-fold emulsion droplets: A coaxial glass capillary microfluidic chip is used, wherein the inner diameter of the inner injection tube tip is 50-100 μm and the inner diameter of the middle injection tube tip is 200-300 μm; the flow rates of the inner aqueous phase, the middle oil phase, the outer aqueous phase, and the continuous oil phase are adjusted to 100-500 μL / h, 200-800 μL / h, 2000-6000 μL / h, and 4000-10000 μL / h, respectively, to form monodisperse fourfold emulsion droplets; (3) Double cross-linking curing and post-treatment of hydrogel shell: a) Photocrosslinking: The collected four-emulsion droplets are placed in an ice bath at 4-10℃ and irradiated with 365nm ultraviolet light for 10-30 minutes to form a covalent crosslinking network; b) Demulsification and washing: Add an equal volume of isopropanol or ethanol to the photocrosslinked tetraemulsion droplet suspension to demulsify, collect the microcapsules by centrifugation and wash them. c) Ionic crosslinking: The microcapsules were dispersed in deionized water, and calcium chloride aqueous solution was added to make the final calcium ion concentration of the system 10-50 mmol / L. The mixture was stirred to crosslink sodium alginate to form a calcium alginate ion network. d) Sieving and drying: The microcapsules are sieved through 200μm and 50μm standard inspection sieves and freeze-dried to obtain the dual-response microcapsule product.

[0011] The dual-response microcapsules were prepared using a W1 / O1 / W2 / O2 quadruple emulsion template via microfluidic technology and possess a three-layer core-shell structure. The inner aqueous core material contains zinc borate, aluminum dihydrogen phosphate, and tetraethyl orthosilicate antioxidant precursors; the intermediate oil phase consists of phenyl silicone oil and a low-melting-point phase change material; and the outer layer is a dual-network hydrogel shell composed of a poly(N-isopropylacrylamide-polyethylene glycol diacrylate) covalently crosslinked network and a calcium alginate ion network.

[0012] In the intermediate oil phase, the low-melting-point phase change material is solid at room temperature, which helps maintain the stability of the oil layer structure. When the temperature rises above its melting point, the phase change material melts, the oil layer viscosity decreases significantly, and the diffusion coefficient increases, thereby triggering temperature-controlled release. This design, together with the poly(N-isopropylacrylamide) thermosensitive shell, forms a dual temperature control barrier, which helps to broaden the release window and improve controllability.

[0013] The hydrogel shell employs a covalent-ionic dual-network structure. The covalent network, formed by the copolymerization of N-isopropylacrylamide monomer and polyethylene glycol diacrylate under UV light initiation, constitutes the basic mechanical framework of the shell. The N-isopropylacrylamide segments impart temperature-responsive characteristics to the shell: when the temperature is below its lower critical solution temperature (LCST), the N-isopropylacrylamide segments are highly hydrophilic, the hydrogel is in a swollen state, the shell is relatively dense, and the diffusion resistance of the core material is high; when the temperature rises above the LCST, the N-isopropylacrylamide segments undergo a hydrophilic-hydrophobic transition, the segments collapse, the hydrogel shrinks, the shell pore size increases, and the diffusion rate significantly improves. By adjusting the ratio of N-isopropylacrylamide to polyethylene glycol diacrylate, the LCST of the shell can be controlled to approach the target service temperature range. The ionic network, formed by the coordination crosslinking of sodium alginate and calcium ions, provides additional mechanical support and stability to the shell. Calcium ions diffuse from the outer aqueous phase into the shell and coordinate with the carboxylate groups on the alginate chain segments to form an ionic cross-linked network. By controlling the calcium ion concentration and cross-linking time, the cross-linking density of the calcium alginate network can be adjusted, thereby optimizing the mechanical strength and permeability of the shell. The dual-network structure gives the shell both good mechanical strength and responsiveness.

[0014] The compression fracture behavior of microcapsules is determined by the mechanical properties and geometry of the shell material, and can be controlled by shell thickness, crosslinking density, and the ratio of dual networks. This invention designs the compression fracture strength of microcapsules to match the molding pressure window of flexible graphite sealing materials by controlling the degree of crosslinking of polyethylene glycol diacrylate and the calcium alginate content. This allows for the microcapsules to rupture and release the core material during compression molding, while remaining intact under low-pressure conditions such as transportation and mixing.

[0015] The aqueous core material contains antioxidant precursors such as zinc borate, aluminum dihydrogen phosphate, and tetraethyl orthosilicate. During high-temperature heat treatment, aluminum dihydrogen phosphate undergoes dehydration and condensation at 200-300℃, gradually transforming into aluminum metaphosphate and aluminum phosphate; tetraethyl orthosilicate undergoes pre-hydrolysis and condensation under acidic conditions to form a SiO2 network; zinc borate gradually releases its water of crystallization and transforms into B2O3 above approximately 400℃. When the temperature rises to 500-600℃, SiO2, B2O3, and AlPO4 melt and flow on the graphite surface and recombine with each other to form a dense B2O3-SiO2-AlPO4-based composite ceramic film. This ceramic film bonds well with the graphite matrix, which is beneficial for preventing oxygen from diffusing into the graphite matrix. In addition, phenyl silicone oil pyrolyzes in a high-temperature aerobic environment to generate amorphous SiO2, which synergistically forms a denser protective layer with the aqueous ceramic precursors, jointly constructing a relay-style high-temperature protection mechanism of "silicone oil sealing → precursor diffusion → ceramic film formation".

[0016] Preferably, the preparation method of the grafted modified expanded graphite includes the following steps: A1: Preparation of functionalized expanded graphite: Expandable graphite is expanded at 850-950℃ for 20-40s to obtain expanded graphite; the expanded graphite is added to a nitric acid solution with a volume fraction of 30-60%, and stirred at 60-80℃ for 2-4h, and then washed and dried to obtain functionalized expanded graphite. A2: Silane coupling agent grafting: γ-glycidyl etheroxypropyltrimethoxysilane was pre-hydrolyzed in an ethanol / water mixed solvent, then functionalized expanded graphite was added and dispersed. The reaction was carried out at 60-80℃ under nitrogen protection for 4-8 hours, and the product was washed and dried to obtain epoxy-functionalized expanded graphite. A3: In-situ synthesis of dynamic covalent network: Weigh epoxy-functionalized expanded graphite, bisphenol A diglycidyl ether, 3,3'-dithiodipropionic acid, sebacic acid and catalyst zinc acetylacetonate, disperse and degas under ultrasonication, pre-cur under nitrogen protection at 100-120℃ for 1-2h, and then cure at 150-180℃ for 2-4h to obtain the cured product; A4: Purification: The cured product was extracted with a Soxhlet extractor in an acetone-ethanol mixture and dried under vacuum to obtain grafted modified expanded graphite.

[0017] Through the above technical solution, expanded graphite, after being oxidized with nitric acid, introduces active groups such as hydroxyl and carboxyl groups onto its surface, providing reaction sites for subsequent chemical grafting. After hydrolysis of γ-glycidoxypropyltrimethoxysilane (KH-560) in a mixed solvent, its silanol groups undergo dehydration condensation with the hydroxyl groups on the graphite surface, forming Si-OC covalent bonds, anchoring the silane to the graphite surface. The epoxy groups at the ends of KH-560 are retained, serving as reaction anchors for subsequent dynamic covalent network polymerization. Through this grafting method, the dynamic covalent network is covalently bonded to the expanded graphite surface, rather than through simple physical mixing, which is beneficial for improving interfacial bonding strength and mitigating the problem of easy peeling off surface coatings or fillers.

[0018] The dynamic covalent network uses bisphenol A diglycidyl ether as the epoxy monomer, 3,3'-dithiodipropionic acid as the disulfide-containing crosslinking agent, and sebacic acid as the flexible long-chain co-crosslinking agent. Under the catalysis of zinc acetylacetonate, the carboxyl and epoxy groups undergo ring-opening esterification to form a three-dimensional crosslinked network containing β-hydroxy ester bonds and dynamic disulfide bonds. The disulfide bonds can undergo reversible breakage and recombination under thermal excitation, and the ester bonds can undergo dynamic transesterification under the action of a catalyst and high temperature. The synergistic effect of both enables the network to have topological rearrangement capabilities over a wide temperature range, thus facilitating stress relaxation and microcrack healing. When the gasket develops microcracks due to thermal stress or mechanical vibration, the dynamic disulfide bonds undergo transesterification under heating conditions, promoting the reconnection of network segments on both sides of the crack and facilitating the self-repair of the microcrack.

[0019] A molding method for a flexible expanded graphite sealing material includes the following steps: loading the flexible expanded graphite sealing material into a mold, molding it under pressure of 15-30MPa and temperature of 25-60℃, holding the pressure for 10-15 minutes to demold, and vacuum drying at 50-60℃ for 2 hours to obtain the finished sealing gasket.

[0020] During compression molding, expanded graphite worms align perpendicular to the pressure direction under pressure. The graphite microflakes interlock through mechanical meshing and van der Waals forces, forming a dense sheet with a certain mechanical strength. The pressure is controlled between 15-30 MPa to match the compressive strength of the microcapsules with the molding pressure. Within this pressure range, the shells of the dual-response microcapsules yield and shear fracture, releasing phenyl silicone oil and antioxidant precursors from the core material. The phenyl silicone oil, with its high viscosity, spreads along the graphite interlayers under pressure, filling micron-sized pores and forming a continuous sealing oil film. Vacuum drying removes residual moisture, reducing the negative impact of water vapor on sealing performance. A holding time of 10-15 minutes ensures thorough compaction of the graphite worms and complete rupture of the microcapsules.

[0021] A sealing gasket is obtained by compression molding of the aforementioned flexible expanded graphite sealing material.

[0022] This sealing gasket exhibits a three-tiered protection mechanism during service: During installation, the molding pressure triggers the microcapsule rupture, releasing silicone oil to fill the graphite pores and achieve immediate sealing. In the early stages of service, when the temperature rises to 200-400℃, the poly(N-isopropylacrylamide) shell shrinks, leading to an increase in the pore size of the hydrogel shell and a decrease in the viscosity of the intermediate oil layer. Phenyl silicone oil is continuously and slowly released, replenishing the sealing oil film, while antioxidant precursors begin to gradually diffuse towards the graphite surface. During high-temperature service (400-600℃), the phenyl silicone oil pyrolyzes to generate SiO2, which melts and combines in situ with B2O3 (generated from zinc borate) and AlPO4 (generated from aluminum dihydrogen phosphate) on the graphite surface, forming a dense B2O3-SiO2-AlPO4-based composite ceramic protective film. This ceramic film effectively prevents oxygen from diffusing into the graphite matrix, thereby reducing the gasket's oxidation weight loss rate. The disulfide bonds in the dynamic covalent network undergo exchange reactions upon heating, enabling stress relaxation and self-repair of microcracks within the dynamic covalent network. In summary, this sealing gasket achieves full-cycle protection functions of "pressure sealing - high-temperature passivation - dynamic self-healing".

[0023] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention grafts a dynamic disulfide bond crosslinking network onto the surface of expanded graphite in the form of covalent bonds, enabling the sealing material to undergo a disulfide bond exchange reaction under heating conditions, promoting microcrack healing, thereby endowing the matrix with self-healing ability, while improving the tensile strength and resilience of the material, solving the problem that traditional chemical crosslinking modification leads to brittle materials that cannot self-heal.

[0024] 2. This invention employs dual-response microcapsules with a three-layer core-shell structure. The compressive strength of the microcapsule is matched with the molding pressure. During molding, the shell of the microcapsule ruptures and releases phenyl silicone oil, which fills the micron-level pores inside the graphite to form a continuous sealing oil film. This effectively reduces the leakage rate of the gasket and overcomes the defect of existing impregnating agents that can only statically fill and cannot dynamically replenish the seal.

[0025] 3. This invention adds a low-melting-point phase change material to the intermediate oil phase of the microcapsule, and works synergistically with the poly(N-isopropylacrylamide) thermosensitive shell to form a dual temperature control barrier. This causes the oil layer viscosity to decrease and the shell pore size to increase when the gasket temperature rises in the early stage of service, and the phenyl silicone oil to be released continuously and slowly, thereby achieving dynamic replenishment of the sealing oil film and extending the sealing life.

[0026] 4. In this invention, zinc borate, aluminum dihydrogen phosphate, and tetraethyl orthosilicate are encapsulated as antioxidant precursors in an aqueous phase within microcapsules. During high-temperature service, the precursors are released and react in situ on the graphite surface to form a B2O3-SiO2-AlPO4-based composite ceramic film. This ceramic film has good bonding with the graphite matrix and can block oxygen from diffusing inward, achieving bulk self-passivation protection within the material and avoiding the problems of easy peeling and short-lasting protection of surface coatings.

[0027] 5. This invention enables the sealing gasket to simultaneously possess the functions of pressure-induced instant sealing during installation, temperature-controlled slow-release sealing during the initial service phase, and in-situ ceramic anti-oxidation during the high-temperature phase through the synergistic effect of grafted modified expanded graphite and dual-response microcapsules. Combined with the dynamic disulfide bond self-repair of the matrix, a full-cycle protection system is formed, and its comprehensive performance is superior to single modification or existing technical solutions. Detailed Implementation

[0028] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with existing known technologies. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.

[0029] Example 1: A flexible expanded graphite sealing material, comprising the following components: 100g of grafted modified expanded graphite; 10g of dual-response microcapsules; The method for preparing the dual-response microcapsules includes the following steps: (1) Preparation of each phase: a) Preparation of the internal aqueous phase: Weigh out the following by mass percentage: 5% zinc borate nano (average particle size 200nm, purity ≥99%), 10% aluminum dihydrogen phosphate liquid (solid content 40%), 3% tetraethyl orthosilicate, 2% ethanol, 0.5% Tween 80, 0.2% polyethylene glycol 400, and 79.3% deionized water; add zinc borate nano and polyethylene glycol 400 to deionized water and ultrasonically disperse in an ice bath for 30 min; add aluminum dihydrogen phosphate liquid, ethanol, and Tween 80, and magnetically stir for 20 min; slowly add tetraethyl orthosilicate dropwise while stirring, and continue magnetically stirring for 30 min after the addition is complete; adjust the pH to 4.0, filter and degas to obtain the internal aqueous phase; b) Preparation of the intermediate oil phase: Weigh out 5% by mass of low-melting-point phase change material (60℃ phase change paraffin), 2% by mass of hydrophobically modified nano zinc borate (200nm particle size, hydrophobically treated with stearic acid), 0.2% by mass of Span 80, and 92.8% by mass of phenyl silicone oil; mix the above components, heat to 50℃ and stir, ultrasonically disperse for 20 min; homogenize at 10000 rpm for 3 min and then degas under vacuum to obtain the intermediate oil phase; c) Preparation of the external aqueous phase: Weigh out 3% N-isopropylacrylamide, 3% polyethylene glycol diacrylate (Mn=575), 0.5% sodium alginate, 0.2% photoinitiator Irgacure2959, 0.5% polyvinyl alcohol, and 92.8% deionized water by mass percentage; stir and dissolve in the dark, and filter to obtain the external aqueous phase; d) Preparation of continuous oil phase: Weigh out 80 1% Span and 99% liquid paraffin by mass percentage, and mix them evenly to obtain a continuous oil phase; (2) Microfluidic generation of four-fold emulsion droplets: A coaxial glass capillary microfluidic chip is used, with the inner layer injection tube tip having an inner diameter of 50 μm and the middle layer injection tube tip having an inner diameter of 200 μm. The flow rates of the inner aqueous phase, the middle oil phase, the outer aqueous phase, and the continuous oil phase are adjusted to 100 μL / h, 200 μL / h, 2000 μL / h, and 4000 μL / h, respectively, to form monodisperse fourfold emulsion droplets. (3) Double cross-linking curing and post-treatment of hydrogel shell: a) Photocrosslinking: The collected four-emulsion droplets were placed in an ice bath at 4°C and irradiated with 365nm ultraviolet light for 10 minutes to form a covalent crosslinking network; b) Demulsification and washing: Isopropanol of equal volume to the suspension was added to the photocrosslinked tetraemulsion droplet suspension to demulsify, and the microcapsules were collected by centrifugation and washed. c) Ionic crosslinking: The microcapsules were dispersed in deionized water, and calcium chloride aqueous solution was added to make the final calcium ion concentration of the system 10 mmol / L. The mixture was stirred to crosslink sodium alginate to form a calcium alginate ion network. d) Sieving and drying: The microcapsules are sieved through 200μm and 50μm standard inspection sieves and freeze-dried to obtain the dual-response microcapsule product.

[0030] The preparation method of the grafted modified expanded graphite includes the following steps: A1: Preparation of functionalized expanded graphite: Expandable graphite (50 mesh, expansion ratio 250 times) was expanded at 850℃ for 20s to obtain expanded graphite; 100g of expanded graphite was added to 500mL of 30% nitric acid solution, stirred and reacted at 60℃ for 2h, washed and dried to obtain functionalized expanded graphite. A2: Silane coupling agent grafting: 10g of γ-glycidyl etheroxypropyltrimethoxysilane was pre-hydrolyzed in an ethanol / water mixed solvent, 100g of functionalized expanded graphite was added and dispersed, and the reaction was carried out at 60℃ under nitrogen protection for 4h. After washing and drying, epoxy-functionalized expanded graphite was obtained. A3: In-situ synthesis of dynamic covalent network: 100g of epoxy-functionalized expanded graphite, 20g of bisphenol A diglycidyl ether, 1.04g of 3,3'-dithiodipropionic acid, 10g of sebacic acid and 0.5g of zinc acetylacetonate were weighed, ultrasonically dispersed and degassed, pre-cured at 100℃ for 1h under nitrogen protection, and then cured at 150℃ for 2h to obtain the cured product; the molar ratio of sebacic acid to 3,3'-dithiodipropionic acid was 1:0.1; A4: Purification: The cured product was extracted with a Soxhlet extractor in an acetone-ethanol mixture and dried under vacuum to obtain grafted modified expanded graphite.

[0031] A method for molding a flexible expanded graphite sealing material includes the following steps: the flexible expanded graphite sealing material obtained above is loaded into a mold, molded under a pressure of 15MPa and a temperature of 25℃, demolded after holding the pressure for 10 minutes, and vacuum dried at 50℃ for 2 hours to obtain a finished sealing gasket.

[0032] Example 2: A flexible expanded graphite sealing material, comprising the following components: 100g of grafted modified expanded graphite; 20g of dual-response microcapsules; The method for preparing the dual-response microcapsules includes the following steps: (1) Preparation of each phase: a) Preparation of the internal aqueous phase: Weigh out the following by mass percentage: 10% zinc borate nano (average particle size 200nm, purity ≥99%), 18% aluminum dihydrogen phosphate liquid (solid content 40%), 9% tetraethyl orthosilicate, 3% ethanol, 1.0% Tween 80, 1.0% polyethylene glycol 400, and 58% deionized water; add zinc borate nano and polyethylene glycol 400 to deionized water and ultrasonically disperse in an ice bath for 40 min; add aluminum dihydrogen phosphate liquid, ethanol, and Tween 80, and magnetically stir for 25 min; slowly add tetraethyl orthosilicate dropwise while stirring, and continue magnetically stirring for 40 min after the addition is complete; adjust the pH to 4.3, filter and degas to obtain the internal aqueous phase; b) Preparation of the intermediate oil phase: Weigh out the following components by mass percentage: 8% low-melting-point phase change material (60℃ phase change paraffin), 9% hydrophobically modified nano zinc borate (200nm particle size, hydrophobically treated with stearic acid), 1.5% Span 80, and 81.5% phenyl silicone oil; mix the above components, heat to 55℃ and stir, ultrasonically disperse for 25 min; homogenize at 12000 rpm for 3.5 min and then degas under vacuum to obtain the intermediate oil phase; c) Preparation of the external aqueous phase: Weigh out the following by mass percentage: 9% N-isopropylacrylamide, 6% polyethylene glycol diacrylate (Mn=575), 1.2% sodium alginate, 0.6% photoinitiator Irgacure2959, 1.2% polyvinyl alcohol, and 81.0% deionized water; stir and dissolve in the dark, then filter to obtain the external aqueous phase; d) Preparation of continuous oil phase: Weigh out 80.3% Span and 97% liquid paraffin by mass percentage, and mix them evenly to obtain a continuous oil phase; (2) Microfluidic generation of four-fold emulsion droplets: A coaxial glass capillary microfluidic chip is used, with the inner layer injection tube tip having an inner diameter of 65 μm and the middle layer injection tube tip having an inner diameter of 230 μm. The flow rates of the inner aqueous phase, the middle oil phase, the outer aqueous phase, and the continuous oil phase are adjusted to 200 μL / h, 350 μL / h, 3000 μL / h, and 6000 μL / h, respectively, to form monodisperse fourfold emulsion droplets. (3) Double cross-linking curing and post-treatment of hydrogel shell: a) Photocrosslinking: The collected four-emulsion droplets were placed in an ice bath at 6°C and irradiated with 365nm ultraviolet light for 15 minutes to form a covalent crosslinking network; b) Demulsification and washing: Ethanol of the same volume as the suspension was added to the photocrosslinked tetraemulsion droplet suspension to demulsify, and the microcapsules were collected by centrifugation and washed. c) Ionic crosslinking: The microcapsules were dispersed in deionized water, and calcium chloride aqueous solution was added to make the final calcium ion concentration of the system 20 mmol / L. The mixture was stirred to crosslink sodium alginate to form a calcium alginate ion network. d) Sieving and drying: The microcapsules are sieved through 200μm and 50μm standard inspection sieves and freeze-dried to obtain the dual-response microcapsule product.

[0033] The preparation method of the grafted modified expanded graphite includes the following steps: A1: Preparation of functionalized expanded graphite: Expandable graphite (50 mesh, expansion ratio 250 times) is expanded at 880℃ for 25s to obtain expanded graphite; 100g of expanded graphite is added to 500mL of 40% nitric acid solution, stirred and reacted at 65℃ for 2.5h, washed and dried to obtain functionalized expanded graphite; A2: Silane coupling agent grafting: 12g of γ-glycidyl etheroxypropyltrimethoxysilane was pre-hydrolyzed in an ethanol / water mixed solvent, 100g of functionalized expanded graphite was added and dispersed, and the reaction was carried out at 65℃ under nitrogen protection for 5h. After washing and drying, epoxy-functionalized expanded graphite was obtained. A3: In-situ synthesis of dynamic covalent network: 100g of epoxy-functionalized expanded graphite, 25g of bisphenol A diglycidyl ether, 10.4g of 3,3'-dithiodipropionic acid, 10g of sebacic acid and 0.6g of zinc acetylacetonate were weighed, ultrasonically dispersed and degassed, pre-cured at 105℃ for 1.2h under nitrogen protection, and then cured at 160℃ for 2.5h to obtain the cured product; the molar ratio of sebacic acid to 3,3'-dithiodipropionic acid was 1:1; A4: Purification: The cured product was extracted with a Soxhlet extractor in an acetone-ethanol mixture and dried under vacuum to obtain grafted modified expanded graphite.

[0034] A method for molding a flexible expanded graphite sealing material includes the following steps: the flexible expanded graphite sealing material obtained above is loaded into a mold, molded under a pressure of 20MPa and a temperature of 35℃, demolded after holding the pressure for 12 minutes, and vacuum dried at 55℃ for 2 hours to obtain a finished sealing gasket.

[0035] Example 3: A flexible expanded graphite sealing material, comprising the following components: 100g of grafted modified expanded graphite; 30g of dual-response microcapsules; The method for preparing the dual-response microcapsules includes the following steps: (1) Preparation of each phase: a) Preparation of the internal aqueous phase: Weigh out the following by mass percentage: 17.5% zinc borate nano (average particle size 200nm, purity ≥99%), 20% aluminum dihydrogen phosphate liquid (solid content 40%), 10% tetraethyl orthosilicate, 4% ethanol, 2.0% Tween 80, 1.2% polyethylene glycol 400, and 45.3% deionized water; add zinc borate nano and polyethylene glycol 400 to deionized water and ultrasonically disperse in an ice bath for 45 min; add aluminum dihydrogen phosphate liquid, ethanol, and Tween 80, and magnetically stir for 30 min; slowly add tetraethyl orthosilicate dropwise while stirring, and continue magnetically stirring for 45 min after the addition is complete; adjust the pH to 4.5, filter and degas to obtain the internal aqueous phase; b) Preparation of the intermediate oil phase: Weigh out the following components by mass percentage: 10% low-melting-point phase change material (60℃ phase change paraffin), 11% hydrophobically modified nano zinc borate (200nm particle size, hydrophobically treated with stearic acid), 2.6% Span 80, and 76.4% phenyl silicone oil; mix the above components, heat to 60℃ and stir, ultrasonically disperse for 30 min; homogenize at 12500 rpm for 4 min and then degas under vacuum to obtain the intermediate oil phase; c) Preparation of the external aqueous phase: Weigh out the following by mass percentage: 14% N-isopropylacrylamide, 9% polyethylene glycol diacrylate (Mn=575), 1.75% sodium alginate, 1.1% photoinitiator Irgacure2959, 1.75% polyvinyl alcohol, and 72.4% deionized water; stir and dissolve in the dark, then filter to obtain the external aqueous phase; d) Preparation of continuous oil phase: Weigh out 4.5% Span 80 and 95.5% liquid paraffin by mass percentage, and mix them evenly to obtain a continuous oil phase; (2) Microfluidic generation of four-fold emulsion droplets: A coaxial glass capillary microfluidic chip is used, with the inner layer injection tube tip having an inner diameter of 75 μm and the middle layer injection tube tip having an inner diameter of 250 μm. The flow rates of the inner aqueous phase, the middle oil phase, the outer aqueous phase, and the continuous oil phase are adjusted to 300 μL / h, 500 μL / h, 4000 μL / h, and 7000 μL / h, respectively, to form monodisperse fourfold emulsion droplets. (3) Double cross-linking curing and post-treatment of hydrogel shell: a) Photocrosslinking: The collected four-emulsion droplets were placed in an ice bath at 7°C and irradiated with 365nm ultraviolet light for 20 minutes to form a covalent crosslinking network; b) Demulsification and washing: Isopropanol of equal volume to the suspension was added to the photocrosslinked tetraemulsion droplet suspension to demulsify, and the microcapsules were collected by centrifugation and washed. c) Ionic crosslinking: The microcapsules were dispersed in deionized water, and calcium chloride aqueous solution was added to make the final calcium ion concentration of the system 30 mmol / L. The mixture was stirred to crosslink sodium alginate to form a calcium alginate ion network. d) Sieving and drying: The microcapsules are sieved through 200μm and 50μm standard inspection sieves and freeze-dried to obtain the dual-response microcapsule product.

[0036] The preparation method of the grafted modified expanded graphite includes the following steps: A1: Preparation of functionalized expanded graphite: Expandable graphite (50 mesh, expansion ratio 250 times) was expanded at 900℃ for 30s to obtain expanded graphite; 100g of expanded graphite was added to 500mL of 45% nitric acid solution, stirred and reacted at 70℃ for 3h, washed and dried to obtain functionalized expanded graphite. A2: Silane coupling agent grafting: 15g of γ-glycidyl etheroxypropyltrimethoxysilane was pre-hydrolyzed in an ethanol / water mixed solvent, 100g of functionalized expanded graphite was added and dispersed, and the reaction was carried out at 70℃ under nitrogen protection for 6h. After washing and drying, epoxy-functionalized expanded graphite was obtained. A3: In-situ synthesis of dynamic covalent network: 100g of epoxy-functionalized expanded graphite, 30g of bisphenol A diglycidyl ether, 52g of 3,3'-dithiodipropionic acid, 10g of sebacic acid and 0.7g of zinc acetylacetonate were weighed, ultrasonically dispersed and degassed, pre-cured at 110℃ for 1.5h under nitrogen protection, and then cured at 165℃ for 3h to obtain the cured product; the molar ratio of sebacic acid to 3,3'-dithiodipropionic acid was 1:5; A4: Purification: The cured product was extracted with a Soxhlet extractor in an acetone-ethanol mixture and dried under vacuum to obtain grafted modified expanded graphite.

[0037] A method for molding a flexible expanded graphite sealing material includes the following steps: the flexible expanded graphite sealing material obtained above is loaded into a mold, molded under a pressure of 22.5 MPa and a temperature of 45°C, demolded after holding the pressure for 12 minutes, and vacuum dried at 55°C for 2 hours to obtain a finished sealing gasket.

[0038] Example 4: A flexible expanded graphite sealing material, comprising the following components: 100g of grafted modified expanded graphite; 40g of dual-response microcapsules; The method for preparing the dual-response microcapsules includes the following steps: (1) Preparation of each phase: a) Preparation of the internal aqueous phase: Weigh out the following by mass percentage: 18% zinc borate nano (average particle size 200nm, purity ≥99%), 22% aluminum dihydrogen phosphate liquid (solid content 40%), 12% tetraethyl orthosilicate, 5% ethanol, 2.5% Tween 80, 1.8% polyethylene glycol 400, and 38.7% deionized water; add zinc borate nano and polyethylene glycol 400 to deionized water and ultrasonically disperse in an ice bath for 55 min; add aluminum dihydrogen phosphate liquid, ethanol, and Tween 80, and magnetically stir for 35 min; slowly add tetraethyl orthosilicate dropwise while stirring, and continue magnetically stirring for 55 min after the addition is complete; adjust the pH to 4.8, filter and degas to obtain the internal aqueous phase; b) Preparation of the intermediate oil phase: Weigh out the following components by mass percentage: 12% low-melting-point phase change material (60℃ phase change paraffin), 18% hydrophobically modified nano zinc borate (200nm particle size, hydrophobically treated with stearic acid), 4% Span 80, and 66% phenyl silicone oil; mix the above components, heat to 65℃ and stir, ultrasonically disperse for 35 min; homogenize at 14000 rpm for 4.5 min and then degas under vacuum to obtain the intermediate oil phase; c) Preparation of the external aqueous phase: Weigh out 20% N-isopropylacrylamide, 12% polyethylene glycol diacrylate (Mn=575), 2.5% sodium alginate, 1.8% photoinitiator Irgacure2959, 2.5% polyvinyl alcohol, and 61.2% deionized water by mass percentage; stir and dissolve in the dark, and filter to obtain the external aqueous phase; d) Preparation of continuous oil phase: Weigh out 80.6% Span and 94% liquid paraffin by mass percentage, and mix them evenly to obtain a continuous oil phase; (2) Microfluidic generation of four-fold emulsion droplets: A coaxial glass capillary microfluidic chip is used, with the inner layer injection tube tip having an inner diameter of 90 μm and the middle layer injection tube tip having an inner diameter of 280 μm. The flow rates of the inner aqueous phase, the middle oil phase, the outer aqueous phase, and the continuous oil phase are adjusted to 400 μL / h, 700 μL / h, 5000 μL / h, and 9000 μL / h, respectively, to form monodisperse fourfold emulsion droplets. (3) Double cross-linking curing and post-treatment of hydrogel shell: a) Photocrosslinking: The collected four-emulsion droplets were placed in an ice bath at 9°C and irradiated with 365nm ultraviolet light for 25 minutes to form a covalent crosslinking network; b) Demulsification and washing: Ethanol of the same volume as the suspension was added to the photocrosslinked tetraemulsion droplet suspension to demulsify, and the microcapsules were collected by centrifugation and washed. c) Ionic crosslinking: The microcapsules were dispersed in deionized water, and calcium chloride aqueous solution was added to make the final calcium ion concentration of the system 40 mmol / L. The mixture was stirred to crosslink sodium alginate to form a calcium alginate ion network. d) Sieving and drying: The microcapsules are sieved through 200μm and 50μm standard inspection sieves and freeze-dried to obtain the dual-response microcapsule product.

[0039] The preparation method of the grafted modified expanded graphite includes the following steps: A1: Preparation of functionalized expanded graphite: Expandable graphite (50 mesh, expansion ratio 250 times) was expanded at 930℃ for 35s to obtain expanded graphite; 100g of expanded graphite was added to 500mL of 55% nitric acid solution and stirred at 75℃ for 3.5h. After washing and drying, functionalized expanded graphite was obtained. A2: Silane coupling agent grafting: 18g of γ-glycidyl etheroxypropyltrimethoxysilane was pre-hydrolyzed in an ethanol / water mixed solvent, 100g of functionalized expanded graphite was added for dispersion, and the reaction was carried out at 75℃ under nitrogen protection for 7h. After washing and drying, epoxy-functionalized expanded graphite was obtained. A3: In-situ synthesis of dynamic covalent network: 100g of epoxy-functionalized expanded graphite, 35g of bisphenol A diglycidyl ether, 312g of 3,3'-dithiodipropionic acid, 10g of sebacic acid and 0.8g of zinc acetylacetonate were weighed, ultrasonically dispersed and degassed, pre-cured at 115℃ for 1.8h under nitrogen protection, and then cured at 175℃ for 3.5h to obtain the cured product; the molar ratio of sebacic acid to 3,3'-dithiodipropionic acid was 1:30; A4: Purification: The cured product was extracted with a Soxhlet extractor in an acetone-ethanol mixture and dried under vacuum to obtain grafted modified expanded graphite.

[0040] A method for molding a flexible expanded graphite sealing material includes the following steps: the flexible expanded graphite sealing material obtained above is loaded into a mold, molded under a pressure of 28MPa and a temperature of 55℃, demolded after holding the pressure for 14 minutes, and vacuum dried at 60℃ for 2 hours to obtain a finished sealing gasket.

[0041] Example 5: A flexible expanded graphite sealing material, comprising the following components: 100g of grafted modified expanded graphite; 50g of dual-response microcapsules; The method for preparing the dual-response microcapsules includes the following steps: (1) Preparation of each phase: a) Preparation of the inner aqueous phase: Weigh out the following by mass percentage: 20% nano zinc borate (average particle size 200nm, purity ≥99%), 25% aluminum dihydrogen phosphate liquid (solid content 40%), 15% tetraethyl orthosilicate, 8% ethanol, 3% Tween 80, 2% polyethylene glycol 400, and 27% deionized water; add nano zinc borate and polyethylene glycol 400 to deionized water and ultrasonically disperse in an ice bath for 60 min; add aluminum dihydrogen phosphate liquid, ethanol, and Tween 80, and magnetically stir for 40 min; slowly add tetraethyl orthosilicate dropwise while stirring, and continue magnetically stirring for 60 min after the addition is complete; adjust the pH to 5.0, filter and degas to obtain the inner aqueous phase; b) Preparation of the intermediate oil phase: Weigh out the following components by mass percentage: 15% low-melting-point phase change material (60℃ phase change paraffin), 20% hydrophobically modified nano zinc borate (200nm particle size, hydrophobically treated with stearic acid), 5% Span 80, and 60% phenyl silicone oil; mix the above components, heat to 70℃ and stir, ultrasonically disperse for 40 min; homogenize at 15000 rpm for 5 min and then degas under vacuum to obtain the intermediate oil phase; c) Preparation of the external aqueous phase: Weigh out 25% N-isopropylacrylamide, 15% polyethylene glycol diacrylate (Mn=575), 3% sodium alginate, 2% photoinitiator Irgacure2959, 3% polyvinyl alcohol, and 52% deionized water by mass percentage; stir and dissolve in the dark, and filter to obtain the external aqueous phase; d) Preparation of continuous oil phase: Weigh out 80.8% Span and 92% liquid paraffin by mass percentage, and mix them evenly to obtain a continuous oil phase; (2) Microfluidic generation of four-fold emulsion droplets: A coaxial glass capillary microfluidic chip is used, wherein the inner diameter of the inner injection tube tip is 100 μm and the inner diameter of the middle injection tube tip is 300 μm; the flow rates of the inner aqueous phase, the middle oil phase, the outer aqueous phase, and the continuous oil phase are adjusted to 500 μL / h, 800 μL / h, 6000 μL / h, and 10000 μL / h, respectively, to form monodisperse fourfold emulsion droplets; (3) Double cross-linking curing and post-treatment of hydrogel shell: a) Photocrosslinking: The collected four-emulsion droplets were placed in an ice bath at 10°C and irradiated with 365nm ultraviolet light for 30 minutes to form a covalent crosslinking network; b) Demulsification and washing: Isopropanol of equal volume to the suspension was added to the photocrosslinked tetraemulsion droplet suspension to demulsify, and the microcapsules were collected by centrifugation and washed. c) Ionic crosslinking: The microcapsules were dispersed in deionized water, and calcium chloride aqueous solution was added to make the final calcium ion concentration of the system 50 mmol / L. The mixture was stirred to crosslink sodium alginate to form a calcium alginate ion network. d) Sieving and drying: The microcapsules are sieved through 200μm and 50μm standard inspection sieves and freeze-dried to obtain the dual-response microcapsule product.

[0042] The preparation method of the grafted modified expanded graphite includes the following steps: A1: Preparation of functionalized expanded graphite: Expandable graphite (50 mesh, expansion ratio 250 times) was expanded at 950℃ for 40s to obtain expanded graphite; 100g of expanded graphite was added to 500mL of 60% nitric acid solution, stirred at 80℃ for 4h, washed and dried to obtain functionalized expanded graphite. A2: Silane coupling agent grafting: 20g of γ-glycidyl etheroxypropyltrimethoxysilane was pre-hydrolyzed in an ethanol / water mixed solvent, 100g of functionalized expanded graphite was added and dispersed, and the reaction was carried out at 80℃ under nitrogen protection for 8h. After washing and drying, epoxy-functionalized expanded graphite was obtained. A3: In-situ synthesis of dynamic covalent network: 100g of epoxy-functionalized expanded graphite, 40g of bisphenol A diglycidyl ether, 520g of 3,3'-dithiodipropionic acid, 10g of sebacic acid and 1.0g of zinc acetylacetonate were weighed, ultrasonically dispersed and degassed, pre-cured at 120℃ for 2h under nitrogen protection, and then cured at 180℃ for 4h to obtain the cured product; the molar ratio of sebacic acid to 3,3'-dithiodipropionic acid was 1:50; A4: Purification: The cured product was extracted with a Soxhlet extractor in an acetone-ethanol mixture and dried under vacuum to obtain grafted modified expanded graphite.

[0043] A method for molding a flexible expanded graphite sealing material includes the following steps: loading the above-obtained flexible expanded graphite sealing material into a mold, molding it under a pressure of 30MPa and a temperature of 60℃, holding the pressure for 15 minutes to demold, and vacuum drying at 60℃ for 2 hours to obtain a finished sealing gasket.

[0044] Comparative Example 1: Based on Example 3, the difference is that ordinary expanded graphite without nitric acid oxidation treatment, silane grafting and dynamic covalent network modification was used, and no dual-response microcapsules were added. It was directly molded, and the rest was the same as Example 3.

[0045] Comparative Example 2: Based on Example 3, the difference is that dual-response microcapsules are not added, and only grafted modified expanded graphite is used for compression molding, otherwise it is the same as Example 3.

[0046] Comparative Example 3: Based on Example 3, the difference is that in the dynamic covalent network of grafted modified expanded graphite, 3,3'-dithiodipropionic acid is replaced with an equimolar amount of succinic acid, and no dynamic disulfide bond structure is introduced. The rest is the same as in Example 3.

[0047] Comparative Example 4: Based on Example 3, the difference is that the grafting modification and microcapsule addition were cancelled. Referring to the best impregnation process in the literature (Research on Vacuum Pressure Impregnation Modification of Flexible Graphite Gaskets by Polytetrafluoroethylene, Du Shaochuan et al., Bulletin of the Chinese Ceramic Society, 2023, 42(10):3732-3740), 60% polytetrafluoroethylene emulsion was used for vacuum impregnation modification, with an impregnation vacuum degree of -0.095MPa, a pressure of 0.65MPa, 2 impregnations, 35℃ for 30min, and drying and curing at 80℃. The rest is the same as in Example 3.

[0048] Comparative Example 5: Based on Example 3, the difference is that the grafting modification and microcapsule addition were cancelled. Referring to the optimal spraying process in the literature (Research on Preparation and Modification of Flexible Graphite Sealing Gaskets, Master's Thesis of Wuhan University of Technology, 2022), a coating with a boron nitride to aluminum dihydrogen phosphate mass ratio of 2:1 and a concentration of 25% was sprayed 7 times and dried at 80°C to form a surface coating. The rest is the same as in Example 3.

[0049] Comparative Example 6: Based on Example 3, the difference is that N-isopropylacrylamide monomer was not added to the outer aqueous phase of the dual-response microcapsules, and only polyethylene glycol diacrylate and sodium alginate were used to prepare the temperature-insensitive shell. The rest was the same as in Example 3.

[0050] Comparative Example 7: Based on Example 3, the difference is that the aqueous phase of the dual-response microcapsules does not contain nano zinc borate, aluminum dihydrogen phosphate liquid, or tetraethyl orthosilicate antioxidant precursor, while the rest is the same as in Example 3.

[0051] Performance testing: The sealing gaskets and dual-response microcapsules obtained in Examples 1-5 and Comparative Examples 1-7 were subjected to the following tests. The test methods and results are as follows: Test Example 1: Dual-Response Microcapsule Test 1. Thermal Performance and Encapsulation Efficiency Testing: Using a simultaneous thermal analyzer, 8 mg of microcapsule sample was weighed and placed in an alumina crucible. Under a nitrogen atmosphere, the temperature was increased from room temperature to 800 °C at a rate of 10 °C / min, and the TG curve was recorded. The weight loss rate from room temperature to 200 °C was taken as moisture evaporation (W1), the weight loss rate from 200-600 °C as core material evaporation and decomposition (W2), and the residue above 600 °C as shell carbon residue. Total weight loss (W... 总=W1+W2; Core material content (wt%) =W2; Encapsulation rate (%) = (Measured core material content W2 / Theoretical core material content) × 100%; Wherein, the theoretical core material content is calculated based on the mass ratio of each component in the aqueous phase and intermediate oil phase during microcapsule preparation.

[0052] 2. Compression Rupture Strength Test: A micromechanical compression testing system was used. Microcapsules were dispersed on a glass slide. A single intact microcapsule (initial diameter D0) was placed between two parallel plates and compressed at a rate of 0.5-1 μm / s. The load-displacement curve was recorded, and the point where the curve first showed a significant drop was taken as the rupture point. σ rupture =F rupture / A projection In the formula, σ rupture F is the compressive breaking strength (MPa). rupture A is the compressive load (N) at the time of fracture. projection Projected area of ​​microcapsules (mm²) 2 ), press A projection =π(D0 / 2) 2 Calculation. For each test group, take the average value of ≥20 samples and record the deformation rate upon breakage.

[0053] Test Example 2: Gasket Test 1. Sealing performance test: Based on GB / T12385-2008, leakage test using the cavity pressurization method. The test medium is nitrogen gas with a purity ≥99.9%, the preload stress is 30 MPa, the medium pressure is 2.0 MPa, and the pressure is maintained for 10 minutes. L = (ΔP•V) / (t•P) atm In the formula, L is the leakage rate (cm). 3 / s), ΔP is the pressure drop (Pa) inside the test flange cavity during the pressure holding time, and V is the cavity volume (cm³). 3 ), t is the holding time (s), P atm Standard atmospheric pressure (101325 Pa). Each sample was tested three times and the average value was taken.

[0054] 2. Compression Ratio and Rebound Rate Test: According to GB / T12622-2008 Method A. Initial preload stress of 5 MPa was recorded as thickness T1. Compression amount ΔT1 was recorded after loading to a total preload stress of 30 MPa. Unloading to 5 MPa was recorded as the unrecovered compression amount ΔT2. Compression ratio (%) = ΔT1 / T1 × 100%; Rebound rate (%) = [(ΔT1 - ΔT2) / ΔT1] × 100%; Three tests were performed for each group, and the average value was taken.

[0055] 3. Tensile strength test: According to JB / T9141.2-2013, cut a straight standard specimen with a gauge length of 50 mm, stretch it at a constant speed of 5 mm / min until fracture, and record the fracture load P, σ=P / (b×h); where σ is the tensile strength (MPa), P is the fracture load (N), b is the specimen width (mm), and h is the specimen thickness (mm). Perform 5 tests per group and take the average value.

[0056] 4. High-Temperature Antioxidant Performance Test: Refer to FSA-G-604-07 Standard Method A. Dry the sample (20×20×1.5mm) at 105℃ to constant weight and record the initial mass m0. Place it in an air atmosphere muffle furnace and oxidize isothermally at 600℃ for 4 hours. After cooling, weigh m1: Oxidation weight loss rate (%) = [(m0-m1) / m0] × 100%; To reduce experimental error, three parallel samples were tested at each time point and temperature point, and the arithmetic mean was taken as the oxidation weight loss rate.

[0057] 5. Microcapsule rupture rate test in gaskets: The molded gaskets were subjected to liquid nitrogen brittle fracture to obtain the cross-section, which was then sputter-coated with gold and observed under SEM. At magnification of 500-2000x, ≥10 fields of view were randomly selected, and the total number of microcapsules N was counted. total and the amount N of shell fracture / core material leakage ruptured Fracturing rate (%) = (N) ruptured / N total )×100%; where N ruptured N represents the number of ruptured microcapsules. total This represents the total number of microcapsules. The criteria for determining rupture are: obvious cracks, debris, or signs of core material leakage in the shell. At least 200 microcapsules should be counted for each type of gasket sample.

[0058] 6. Self-healing performance test: A straight scratch with a depth of approximately 20% was pre-made on the gasket surface using a blade. The scratched sample was then heat-treated at 120℃ under nitrogen protection for 4 hours. The self-healing efficiency was characterized by the tensile strength recovery rate; the self-healing efficiency η... tensile =[(σ2-σ1) / (σ0-σ1)]×100%; where: σ0 is the tensile strength of the original unscratched specimen; σ1 is the tensile strength of the unrepaired scratched specimen; and σ2 is the tensile strength of the specimen after scratch repair.

[0059] Table 1. Performance test results of dual-response microcapsules in Examples 1-5 and Comparative Examples 6-7

[0060] Table 2. Performance test results of gaskets in Examples 1-5 and Comparative Examples 1-7

[0061] Data analysis: The sealing gaskets prepared in Examples 1-5 all exhibited lower nitrogen leakage rates, higher tensile strength, moderate compression resilience, and excellent high-temperature oxidation resistance. Example 3 showed the best overall performance, with a nitrogen leakage rate of 1.70 × 10⁻⁶. -4 cm 3 / s, the oxidation weight loss rate at 600℃ is 0.52%, the tensile strength is 5.82MPa, and the self-healing efficiency reaches 85%.

[0062] Comparative Example 1 was an unmodified ordinary expanded graphite gasket, without any grafting modification or microencapsulation. Compared to Example 3, Comparative Example 1 had a leakage rate as high as 10.70 × 10⁻⁶. -4 cm 3 The oxidation weight loss rate is as high as 13% per second, the tensile strength is only 4.96 MPa, and the resilience rate is only 15.9%. This indicates that pure expanded graphite itself has a large number of interconnected pores, is easily oxidized at high temperatures, and has limited mechanical properties.

[0063] Comparative Example 2 grafted a dynamic covalent network onto expanded graphite but did not add dual-response microcapsules. Compared to Comparative Example 1, the leakage rate of Comparative Example 2 was reduced to 8.20 × 10⁻⁶. -4 cm 3 / s, the oxidation weight loss rate decreased to 6.5%, the tensile strength increased to 5.64 MPa, the resilience increased to 21.1%, and the self-healing efficiency reached 81%. This indicates that the dynamic disulfide bond network significantly enhances the mechanical properties and self-healing ability of the matrix. However, grafting modification alone cannot effectively fill the micron-sized pores inside graphite, so the leakage rate is still much higher than in the example.

[0064] Comparative Example 3 used succinic acid instead of 3,3'-dithiodipropionic acid to construct a conventional covalent network without dynamic disulfide bonds. Compared with Comparative Example 2, Comparative Example 3 had a tensile strength of 5.31 MPa, an oxidation weight loss rate of 7.1%, and a leakage rate of 6.12 × 10⁻⁶. -4 cm 3 / s, the self-healing efficiency drops sharply to 10%. This indicates that dynamic disulfide bonds are key to achieving network topology rearrangement and microcrack self-healing. Without disulfide bonds, the material almost loses its self-healing ability, while its mechanical properties and oxidation resistance also decline.

[0065] Comparative Example 4, modified using polytetrafluoroethylene emulsion vacuum impregnation, is representative of existing technologies. Compared to Example 3, the leakage rate of Comparative Example 4 was 4.0 × 10⁻⁶. -4 cm 3 / s, still higher than 1.70 × 10 in Example 3. -4 cm 3 / s; its oxidation weight loss rate is as high as 30%, which is much higher than the 0.52% in Example 3. This is because polytetrafluoroethylene has undergone violent decomposition at 600°C and cannot provide high-temperature protection, while impregnation filling can temporarily improve the sealing performance, but lacks dynamic response capability.

[0066] Comparative Example 5 was modified with a surface coating of boron nitride and aluminum dihydrogen phosphate. The oxidation weight loss rate at 600℃ for 4 hours was 0.65%, which is better than that of pure graphite gaskets and comparable to the typical oxidation resistance level of the coating system reported in the literature at this temperature. This indicates that in short-term high-temperature tests, the surface coating can block oxygen to a certain extent and reduce oxidation weight loss. However, the leakage rate of this comparative example was as high as 11.2 × 10⁻⁶. -4 cm 3 The coating speed is comparable to that of a pure graphite gasket, indicating that the coating only covers the surface and cannot fill the micron-sized pores inside the graphite, thus offering limited improvement in permeation and leakage. Furthermore, the coating has weak adhesion to the substrate, making it prone to cracking and peeling under thermal and mechanical vibrations. Once locally damaged, it loses its protective function, failing to provide long-term protection. Therefore, the surface coating provides passive, short-term protection, fundamentally different from the mechanism of in-situ ceramic formation via microcapsules to achieve bulk self-passivation in this invention.

[0067] Comparative Example 6 used microcapsules without a temperature-sensitive shell, meaning no N-isopropylacrylamide was added to the outer aqueous phase. Compared to Example 3, the leakage rate of Comparative Example 6 was 4.52 × 10⁻⁶. -4 cm 3 / s, and the oxidation weight loss rate was 1.20%, both significantly higher than in Example 3. This is because without the poly-N-isopropylacrylamide temperature-sensitive shell, the microcapsules could not continuously release phenyl silicone oil through shell collapse during the initial service period at 200°C to 400°C, resulting in the sealing oil film not being replenished in time, and the diffusion of the antioxidant precursor was also restricted.

[0068] Comparative Example 7 used microcapsules without antioxidant precursors, and the internal aqueous phase was free of zinc borate, aluminum dihydrogen phosphate, and tetraethyl orthosilicate. Compared to Example 3, the leakage rate of Comparative Example 7 was 3.96 × 10⁻⁶. -4 cm 3 / s, with an oxidation weight loss rate of 1.05%. Although the leakage rate was slightly better than that of Comparative Example 6, the oxidation weight loss rate was still significantly higher than that of Example 3. This is because, without the precursor, the phenyl silicone oil released by the microcapsules can only generate a small amount of SiO2 at high temperatures, and cannot form a B2O3-SiO2-AlPO4 composite ceramic film, resulting in a significant decrease in oxidation protection capability.

[0069] Based on the above comparative analysis, the core innovation of this invention lies in the following: the dynamic disulfide bond grafting network endows the matrix with self-healing capabilities; the pressure-induced rupture of microcapsules releases phenyl silicone oil to fill pores during molding, achieving immediate sealing; the dual temperature control barrier constructed by the temperature-sensitive shell and phase change oil layer ensures continuous sealing during the initial service phase; and the antioxidant precursor in the internal aqueous phase generates a composite ceramic film in situ at high temperatures, providing long-lasting bulk self-passivation protection. The synergistic effect of these four elements results in significantly lower leakage and oxidation weight loss rates in the sealing gaskets of the embodiments compared to the comparative examples.

[0070] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A flexible expanded graphite sealing material, characterized in that, By weight, it includes the following components: 100 parts of graft-modified expanded graphite; 10-50 portions of dual-response microcapsules; The grafted modified expanded graphite is formed by grafting epoxy-modified expanded graphite with a dynamic covalent network polymer via covalent bonds. The dynamic covalent network polymer is formed by cross-linking bisphenol A diglycidyl ether, 3,3'-dithiodipropionic acid and sebacic acid through a ring-opening esterification reaction of epoxy and carboxyl groups, and the polymer network backbone contains dynamic disulfide bonds. The dual-response microcapsule has a three-layer core-shell structure, consisting of, from the inside out: an inner aqueous core containing an antioxidant precursor, an intermediate oil layer containing phenyl silicone oil and a low-melting-point phase change material, and a dual-network hydrogel shell composed of a poly(N-isopropylacrylamide-polyethylene glycol diacrylate) covalent crosslinked network and a calcium alginate ion network.

2. The flexible expanded graphite sealing material according to claim 1, characterized in that, The molar ratio of sebacic acid to 3,3'-dithiodipropionic acid is 1:0.1-50.

3. The flexible expanded graphite sealing material according to claim 1, characterized in that, The method for preparing the dual-response microcapsules includes the following steps: (1) Preparation of each phase: a) Preparation of the internal aqueous phase: Weigh out 5-20% nano zinc borate, 10-25% aluminum dihydrogen phosphate liquid, 3-15% tetraethyl orthosilicate, 2-8% ethanol, 0.5-3% Tween 80, and 0.2-2% polyethylene glycol 400 by mass percentage, with the remainder being deionized water; add nano zinc borate and polyethylene glycol 400 to the deionized water and ultrasonically disperse in an ice bath for 30-60 min; add aluminum dihydrogen phosphate liquid, ethanol, and Tween 80, and magnetically stir for 20-40 min; slowly add tetraethyl orthosilicate dropwise while stirring, and continue magnetically stirring for 30-60 min after the addition is complete; adjust the pH to 4.0-5.0, filter and degas to obtain the internal aqueous phase; b) Preparation of the intermediate oil phase: Weigh out 5-15% low-melting-point phase change material, 2-20% hydrophobically modified nano zinc borate, and 0.2-5% Span 80 by mass percentage, with the balance being phenyl silicone oil; mix the above components, heat to 50-70℃ and stir, ultrasonically disperse for 20-40 min; homogenize at 10000-15000 rpm for 3-5 min and then degas under vacuum to obtain the intermediate oil phase; c) Preparation of the external aqueous phase: Weigh out 3-25% N-isopropylacrylamide, 3-15% polyethylene glycol diacrylate, 0.5-3% sodium alginate, 0.2-2% photoinitiator, and 0.5-3% polyvinyl alcohol by mass percentage, with the remainder being deionized water; stir and dissolve in the dark, then filter to obtain the external aqueous phase; d) Preparation of continuous oil phase: Weigh out 1-8% of Span 80 by mass percentage, with the remainder being liquid paraffin, and mix thoroughly to obtain a continuous oil phase; (2) Microfluidic generation of four-fold emulsion droplets: A coaxial glass capillary microfluidic chip is used, wherein the inner diameter of the inner injection tube tip is 50-100 μm and the inner diameter of the middle injection tube tip is 200-300 μm; the flow rates of the inner aqueous phase, the middle oil phase, the outer aqueous phase, and the continuous oil phase are adjusted to 100-500 μL / h, 200-800 μL / h, 2000-6000 μL / h, and 4000-10000 μL / h, respectively, to form monodisperse fourfold emulsion droplets; (3) Double cross-linking curing and post-treatment of hydrogel shell: a) Photocrosslinking: The collected four-emulsion droplets are placed in an ice bath at 4-10℃ and irradiated with 365nm ultraviolet light for 10-30 minutes to form a covalent crosslinking network; b) Demulsification and washing: Add an equal volume of isopropanol or ethanol to the photocrosslinked tetraemulsion droplet suspension to demulsify, collect the microcapsules by centrifugation and wash them. c) Ionic crosslinking: The microcapsules were dispersed in deionized water, and calcium chloride aqueous solution was added to make the final calcium ion concentration of the system 10-50 mmol / L. The mixture was stirred to crosslink sodium alginate to form a calcium alginate ion network. d) Sieving and drying: The microcapsules are sieved through 200μm and 50μm standard inspection sieves and freeze-dried to obtain the dual-response microcapsule product.

4. The flexible expanded graphite sealing material according to claim 1, characterized in that, The preparation method of the grafted modified expanded graphite includes the following steps: A1: Preparation of functionalized expanded graphite: Expandable graphite is expanded at 850-950℃ for 20-40s to obtain expanded graphite; the expanded graphite is added to a nitric acid solution with a volume fraction of 30-60%, and stirred at 60-80℃ for 2-4h, and then washed and dried to obtain functionalized expanded graphite. A2: Silane coupling agent grafting: γ-glycidyl etheroxypropyltrimethoxysilane was pre-hydrolyzed in an ethanol / water mixed solvent, then functionalized expanded graphite was added and dispersed. The reaction was carried out at 60-80℃ under nitrogen protection for 4-8 hours, and the product was washed and dried to obtain epoxy-functionalized expanded graphite. A3: In-situ synthesis of dynamic covalent network: Weigh epoxy-functionalized expanded graphite, bisphenol A diglycidyl ether, 3,3'-dithiodipropionic acid, sebacic acid and catalyst zinc acetylacetonate, disperse and degas under ultrasonication, pre-cur under nitrogen protection at 100-120℃ for 1-2h, and then cure at 150-180℃ for 2-4h to obtain the cured product; A4: Purification: The cured product was extracted with a Soxhlet extractor in an acetone-ethanol mixture and dried under vacuum to obtain grafted modified expanded graphite.

5. A method for molding a flexible expanded graphite sealing material according to any one of claims 1-4, characterized in that, Includes the following steps: The flexible expanded graphite sealing material is loaded into a mold and molded under a pressure of 15-30 MPa and a temperature of 25-60°C. After holding the pressure for 10-15 minutes, the material is demolded and then vacuum dried at 50-60°C for 2 hours to obtain the finished sealing gasket.

6. A sealing gasket prepared by the molding method of claim 5.