An industrial method for the continuous suspension polymerization of thermoset resin proppants
By using a continuous suspension polymerization process and an aqueous closed-loop circulation system, the problems of high density and poor sphericity of traditional proppants have been solved, enabling efficient and stable production of thermosetting resin proppants across the entire particle size range, thus meeting the needs of deep oil and gas extraction.
Patent Information
- Application Number
- CN202611360141.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies make it difficult to achieve efficient, stable, and large-scale production of thermosetting resin proppants across the entire particle size range, especially ultrafine particle size products. Furthermore, traditional proppants have high density and poor sphericity, which cannot meet the needs of deep oil and gas extraction.
A continuous suspension polymerization process is adopted, which uses a continuous premixing and dispersion unit, a three-stage series gradient curing reactor group and a continuous solid-liquid separation unit, combined with an aqueous phase closed-loop circulation system, to achieve continuous and stable production of thermosetting resin proppant of 6 to 300 mesh.
It enables the production of proppants with narrow particle size range, high sphericity, low density, and high compressive strength, improving production efficiency and product consistency, reducing wastewater discharge and operating costs, and adapting to different reservoir requirements.
Smart Images

Figure CN123132003A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of oil and gas extraction technology, specifically to proppant materials for hydraulic fracturing, and in particular to a method for the industrial production of thermosetting resin-based spherical proppants with a full particle size range (6-300 mesh) using a continuous suspension polymerization process, which is suitable for large-scale, continuous production in large industrial reactors. Background Technology
[0002] The efficient development of unconventional oil and gas resources such as shale gas, tight oil, and coalbed methane heavily relies on hydraulic fracturing technology. This technology injects fracturing fluid into the formation under high pressure. The fracturing fluid carries proppant into artificial fractures. After the pressure is removed, the proppant provides support within the fractures, forming oil and gas flow channels with sufficient conductivity. The performance of the proppant, especially its particle size distribution, sphericity, density, and compressive strength, directly determines the effective supported area of the fractures, the conductivity, and the ultimate recovery rate and lifespan of the oil and gas well.
[0003] Currently, the most widely used proppants in the industry are natural quartz sand, artificial ceramsite, and resin-based proppants. However, as oil and gas extraction extends to deeper, lower-permeability, and more complex lithological reservoirs, the inherent technical shortcomings of these traditional proppants are becoming increasingly apparent. First, the high density of traditional proppants (natural quartz sand and artificial ceramsite) severely limits their penetration ability and effective placement distance at deep formations. The bulk density of quartz sand and ceramsite is generally between 2.6 and 2.8 g / cm³. 3 The range is significantly higher than the proppant carrying capacity of existing fracturing fluid systems. The high density increases friction during pumping, raising energy consumption; on the other hand, the proppant settles prematurely under gravity, accumulating in large quantities near the wellbore and becoming difficult to carry effectively to the far end of the fracture.
[0004] Secondly, for deep shale formations and other conditions requiring ultrafine particle size (e.g., 200-400 mesh) proppant, traditional mechanical crushing methods struggle to produce qualified products. Effective support for micro-fractures necessitates proppants with small particle size and high sphericity. However, ultrafine particles prepared by mechanical crushing are generally angular or irregular in shape, with extremely poor sphericity, and are accompanied by a large amount of ineffective dust. More importantly, the crushing process introduces numerous micro-cracks within the particles, creating stress concentration points. This significantly reduces the compressive strength of the particles, making them unable to withstand the high closure pressure of deep formations. Consequently, they are prone to breakage or pulverization downhole, losing their supporting function.
[0005] In addition, existing reports on resin proppant are all limited by batch suspension polymerization processes, which cannot achieve continuous and stable large-scale industrial production. Specifically, existing technologies generally use batch single-reactor suspension polymerization to prepare resin proppant. This method has the following fundamental defects: (1) Low production efficiency. Each batch of production must complete non-production auxiliary steps such as feeding, heating, isothermal polymerization, cooling, cleaning and discharge in sequence. The equipment utilization rate is low and the production cycle is long; (2) Poor product quality uniformity. There are inevitably dead zones and temperature gradients in the large reactor, which makes it easy for droplets to stick together and agglomerate during the polymerization process. The product has a wide particle size distribution (the particle size span in a single batch is usually greater than 2 times), and the reactor wall is severely stuck with material. The performance fluctuates significantly between batches, which cannot meet the stringent requirements of oil and gas fields for narrow distribution and high consistency of proppant; (3) Lack of flexible production capability. It is difficult for a production line to stably and quickly switch to produce products of different mesh sizes (e.g., from coarse particle size 6 mesh to ultrafine 300 mesh), which cannot adapt to the differentiated needs of different reservoirs for proppant particle size.
[0006] In summary, developing an industrial method for the continuous, stable, and large-scale preparation of thermosetting resin proppants with a narrow particle size distribution across the entire particle size range (especially ultrafine particle size) while ensuring high strength, low density, and excellent sphericity is a technical challenge that urgently needs to be solved but has remained unresolved for a long time. Summary of the Invention
[0007] The technical problem this invention aims to solve is to overcome the shortcomings of existing technologies and provide an industrial method for the continuous suspension polymerization preparation of thermosetting resin fracturing proppant. The core of this invention lies in constructing a fully continuous production system consisting of a continuous premixing and dispersion unit, a three-stage series gradient curing reactor group, a continuous solid-liquid separation unit, and an aqueous phase closed-loop circulation unit. The entire system operates under sealed conditions and nitrogen protection.
[0008] This invention enables continuous, stable, and large-scale production of a full range of proppants from 6 to 300 mesh. The products feature a narrow particle size range (≤2 times), high sphericity (≥0.95), low density, high compressive strength, and excellent deep-penetration performance. This invention solves the technical problems of low production efficiency, wide particle size distribution, poor adaptability to large reactors, difficulty in forming ultrafine particles, and significant water phase waste in existing batch suspension polymerization processes.
[0009] The technical solution adopted by this invention to solve its technical problem is: an industrial method for preparing thermosetting resin fracturing proppant by continuous suspension polymerization, specifically including the following steps: Step S1, Raw material preparation: Prepare oil phase component and aqueous phase component separately. The oil phase component is stored in an oil tank and the aqueous phase component is stored in a water tank. Step S2, High-speed shear dispersion: The oil phase component is continuously pumped to the oil phase inlet of the online high-speed shear emulsifier via a constant flow pump, and the aqueous phase component is continuously pumped to the aqueous phase inlet of the online high-speed shear emulsifier via a constant flow pump; the oil phase component and the aqueous phase component are instantaneously mixed and dispersed in the high-speed shear emulsifier to form a stable oil-in-water suspension; Step S3, Three-stage series gradient temperature field continuous curing: The water-in-oil suspension obtained in step S2 is sequentially fed into a primary molding reactor, a secondary pre-curing reactor, and a tertiary deep curing reactor arranged in series, respectively to complete spherical shaping, surface cross-linking, and deep curing, to obtain a cured slurry with spherical particles; the reaction temperature of the three reactors is gradient-increased, the stirring speed of the three reactors is gradient-increased, and the three reactors are continuously cured under nitrogen protection; Step S4, solid-liquid separation, drying and grading and closed-loop circulation of aqueous phase: The solidified slurry obtained in step S3 is fed into a solid-liquid separation device for solid-liquid separation. The separated solid particles are washed, dried, screened and packaged into a warehouse in sequence. The separated aqueous slurry is filtered and then circulated in a closed loop to a water tank.
[0010] The finished proppant obtained by this invention has a particle size range of 6–300 mesh and a sphericity ≥0.95; simultaneously, the particle size span of a single batch of the proppant is ≤2 times, and the bulk density is 0.7–1.1 g / cm³. 3 The breakage rate at 52 MPa is less than 2.5%.
[0011] Further, in step S1, the oil phase component includes the following raw materials in parts by weight: 100 parts of thermosetting resin (phenolic resin or epoxy resin, free monomer content <0.5%), 8-15 parts of latent microcapsule curing agent (microencapsulated hexamethylenetetramine, with a coating layer of modified polyethylene wax), and 0.5-2 parts of chain regulator (dodecyl mercaptan). The aqueous phase component includes the following raw materials in parts by weight: 300-500 parts deionized water, 2-5 parts composite dispersant, and 0.3-1 parts pH buffer adjuster (sodium dihydrogen phosphate-disodium hydrogen phosphate buffer system).
[0012] Furthermore, the composite dispersant is composed of montmorillonite, modified lignin sulfonate, and fatty alcohol polyoxyethylene ether in a mass ratio of 3:5:2.
[0013] Furthermore, when the shear rate of the high-speed shear emulsifier in step S2 is 300-500 rpm, the particle size of the solid particles obtained in step S4 is 6-12 mesh. Alternatively, when the shear rate of the high-speed shear emulsifier in step S2 is 800-1000 rpm, the particle size of the solid particles obtained in step S4 is 20-40 mesh. Alternatively, when the shear rate of the high-speed shear emulsifier in step S2 is 1800–2200 rpm, the particle size of the solid particles obtained in step S4 is 200–300 mesh.
[0014] Furthermore, in step S3, the temperature of the primary molding reactor is 25–65°C and the stirring speed is 80–120 rpm; the temperature of the secondary pre-curing reactor is 65–95°C and the stirring speed is 120–160 rpm; and the temperature of the tertiary deep curing reactor is 95–125°C and the stirring speed is 150–200 rpm.
[0015] Furthermore, in step S4, the solid-liquid separation device is a continuous horizontal screw centrifuge.
[0016] Furthermore, in step S4, the filtration accuracy of the filtration device for the aqueous slurry is ≤5μm.
[0017] The beneficial effects of this invention are that it is rationally designed and has the following advantages: 1. Continuous production mode: Adopting a three-stage series reactor continuous process, it completely gets rid of the batch limitation of intermittent production, and the production efficiency is increased by more than 50% compared with the traditional intermittent reactor. There is no need for frequent reactor cleaning, and there is zero difference between product batches.
[0018] 2. Precise control of particle size range: Through a three-level linkage control strategy of "shear rate - temperature gradient - stirring speed", the first industrial stable production of a full range of particles from 6 mesh coarse particles to 300 mesh ultrafine powder has been achieved on the same production line. The particle size range of a single batch of products is strictly controlled within 2 times, and the sphericity is as high as 0.95 or above.
[0019] 3. Excellent product performance: The bulk density of the finished proppant is only 0.7–1.1 g / cm³. 3 Its density is far lower than that of ceramsite / quartz sand. At a closure pressure of 52 MPa, the breakage rate is <2.5%, and its mechanical strength surpasses that of traditional proppant of the same specifications. Its extremely low density and perfect spherical shape give it excellent suspension and deep penetration capabilities in fracturing fluids.
[0020] 4. Green and environmentally friendly with low cost: The unique water phase closed-loop circulation system reduces wastewater discharge by more than 90%, and effectively reuses dispersants and heat, significantly reducing overall operating costs and meeting the requirements of green chemical industry.
[0021] 5. Flexible production: A single production line can switch between producing products of different mesh sizes (or mixed sand) by quickly adjusting the shearing rate and temperature control parameters without stopping the machine or changing the core equipment, thus responding quickly to market demands. Attached Figure Description
[0022] The present invention will be further described below with reference to the accompanying drawings and embodiments.
[0023] Figure 1 This is a process flow diagram of the present invention. Detailed Implementation
[0024] The present invention will now be described in further detail with reference to the accompanying drawings. These drawings are simplified schematic diagrams, illustrating only the basic structure of the invention, and therefore only show the components relevant to the invention.
[0025] like Figure 1 As shown, the industrial method for preparing thermosetting resin fracturing proppant by continuous suspension polymerization of the present invention specifically includes the following steps: Step S1, Raw material preparation: (1) Preparation of oil phase components: by mass, 100 parts of thermosetting resin (phenolic resin or epoxy resin, free monomer content <0.5%), 8-15 parts of latent microcapsule curing agent (microencapsulated hexamethylenetetramine, with modified polyethylene wax as the coating layer), and 0.5-2 parts of chain regulator (dodecyl mercaptan) are mixed evenly in an oil phase storage tank with stirring, and continuously transported to the oil phase inlet of the online high-speed shear emulsifier by a constant flow pump; (2) Preparation of aqueous phase components: In an aqueous phase storage tank with stirring, 300-500 parts of deionized water, 2-5 parts of composite dispersant (montmorillonite, modified lignin sulfonate, and fatty alcohol polyoxyethylene ether compounded in a mass ratio of 3:5:2) and 0.3-1 parts of pH buffer adjuster (sodium dihydrogen phosphate-disodium hydrogen phosphate buffer system) are mixed evenly and continuously pumped into the aqueous phase inlet of the online high-speed shear emulsifier through a constant flow pump; Step S2, High-Speed Shear Dispersion: The oil phase component and the aqueous phase component are instantaneously mixed and dispersed in a high-speed shear emulsifier to form a stable oil-in-water suspension; by precisely adjusting the rotor speed of the shearer, the initial resin droplet particle size can be locked, thereby controlling the final product mesh size. Step S3, Three-stage series gradient temperature field continuous curing: The water-in-oil suspension obtained in step S2 is sequentially fed into a primary molding reactor, a secondary pre-curing reactor, and a tertiary deep curing reactor arranged in series, respectively to complete spherical shaping, surface cross-linking, and deep curing, to obtain a cured slurry with spherical particles; the reaction temperature of the three reactors is gradient-increased, the stirring speed of the three reactors is gradient-increased, and the three reactors are continuously cured under nitrogen protection; Step S4, solid-liquid separation, drying and classification and closed-loop circulation of aqueous phase: The solidified slurry (containing spherical particles and aqueous phase) obtained in step S3 is directly fed into a continuous horizontal screw centrifuge to achieve rapid and continuous separation of solid and liquid. The separated solid wet particles are washed by a continuous belt washer (using deionized water to clean the surface of residual dispersant), then enter a continuous fluidized bed dryer (hot air temperature 80-105℃), and finally pass through an air classifying and screening system to be directly packaged and stored according to different mesh standards (6 / 12, 12 / 20, 20 / 40, 40 / 70, 70 / 140, 140 / 200, 200 / 300 mesh, etc.). The hot wastewater phase separated by the continuous horizontal screw centrifuge first enters a multi-media filter and a precision filter (filtration accuracy ≤5μm) to remove trace amounts of fine powder and unreacted substances. After adding 5%–10% of the lost amount of composite dispersant and a small amount of deionized water, it is pumped back to the aqueous phase storage tank of the premixing and dispersion unit, achieving nearly 100% closed-loop recycling of the aqueous phase and dispersant, significantly reducing wastewater discharge and production costs.
[0026] When the shear rate of the high-speed shear emulsifier in step S2 is 300-500 rpm, the particle size of the solid particles obtained in step S4 is 6-12 mesh. Alternatively, when the shear rate of the high-speed shear emulsifier in step S2 is 800-1000 rpm, the particle size of the solid particles obtained in step S4 is 20-40 mesh. Alternatively, when the shear rate of the high-speed shear emulsifier in step S2 is 1800–2200 rpm, the particle size of the solid particles obtained in step S4 is 200–300 mesh.
[0027] In step S3, three industrial reactors (each with an effective volume of 5–50 m³) are used: a primary molding reactor, a secondary pre-curing reactor, and a tertiary deep curing reactor. 3 () are connected in series. Each reactor is equipped with: (1) A closed nitrogen protection system is used to maintain a slight positive pressure and prevent oxygen from accumulating. (2) Automatic wall scraping device, which periodically scrapes off the material adhering to the vessel wall to prevent clumping; (3) Online laser particle size monitor, which monitors the particle size distribution of particles in suspension in real time and feeds the data back to the control system; (4) Variable frequency speed control mixer.
[0028] The process parameters of the three industrial reactors were designed in a gradient manner, as shown in Table 1.
[0029] Table 1
[0030] The curing slurry is continuously transported between the three reactors via overflow, without any intermediate pumping or stopping, achieving uninterrupted and continuous curing.
[0031] Example 1: Preparation of 20-40 mesh thermosetting phenolic resin support The industrialization method of this embodiment is as follows: (1) Raw material ratio Oil phase components: 100 kg phenolic resin, 12 kg microencapsulated hexamethylenetetramine, 1 kg dodecyl mercaptan; Aqueous phase components: 400 kg deionized water, 3.5 kg composite dispersant (montmorillonite: modified lignin sulfonate: fatty alcohol polyoxyethylene ether = 3:5:2), and 0.5 kg sodium dihydrogen phosphate-disodium hydrogen phosphate buffer.
[0032] (2) Process parameters The high-speed shear emulsifier has a shear rate of 950 rpm; the primary reactor temperature is 70℃ and the stirring speed is 100 rpm; the secondary reactor temperature is 80℃ and the stirring speed is 140 rpm; the tertiary reactor temperature is 90℃ and the stirring speed is 180 rpm; the oil phase feed rate is 250 L / h, and the aqueous phase feed rate is 900 L / h. The system operated continuously and stably for 72 hours.
[0033] (3) Product performance Particle size: 20-40 mesh (D90 / D10=1.78), sphericity 0.97.
[0034] Density: Bulk density 0.92 g / cm³ 3 Apparent density 1.35 g / cm³ 3 .
[0035] Strength: 2.1% breakage rate under 52 MPa closing pressure (compared to 3.8% breakage rate of ceramsite and 5.2% breakage rate of quartz sand of the same mesh size).
[0036] Flow conductivity: Under the same closing pressure, the flow conductivity is improved by about 35% compared to ceramsite.
[0037] Water phase recycling rate: 93%.
[0038] Example 2: Preparation of 6-12 mesh large particle size epoxy resin support The industrialization method of this embodiment is as follows: (1) Raw material ratio Oil phase components: 100 kg epoxy resin, 10 kg microcapsule curing agent (same as Example 1), 0.8 kg dodecyl mercaptan; Aqueous phase components: 350 kg of deionized water, 3 kg of composite dispersant (same as in Example 1), and 0.6 kg of pH buffer (same as in Example 1).
[0039] (2) Process parameters The high-speed shear emulsifier has a shear rate of 420 rpm; the temperature of the first-stage reactor is 72℃ and the stirring speed is 90 rpm; the temperature of the second-stage reactor is 82℃ and the stirring speed is 130 rpm; the temperature of the third-stage reactor is 92℃ and the stirring speed is 170 rpm; the oil phase feed rate is 220 L / h and the water phase feed rate is 850 L / h.
[0040] (3) Product performance Particle size 6–12 mesh (span 1.85 times); sphericity 0.96; bulk density 0.88 g / cm³ 3 52 MPa, breakage rate 2.3%.
[0041] Example 3: Preparation of 200-300 mesh ultrafine phenolic resin support The industrialization method of this embodiment is as follows: (1) Raw material ratio Oil phase components: 100 kg phenolic resin, 14 kg microcapsule curing agent (same as Example 1), 1.5 kg dodecyl mercaptan; Aqueous phase components: 450 kg of deionized water, 4.2 kg of composite dispersant (same as in Example 1), and 0.7 kg of pH buffer (same as in Example 1).
[0042] (2) Process parameters The high-speed shear emulsifier has a shear rate of 2100 rpm; the temperature of the first-stage reactor is 69℃ and the stirring speed is 110 rpm; the temperature of the second-stage reactor is 79℃ and the stirring speed is 150 rpm; the temperature of the third-stage reactor is 89℃ and the stirring speed is 190 rpm; the oil phase feed rate is 280 L / h and the water phase feed rate is 950 L / h.
[0043] (3) Product performance Particle size 200–300 mesh (span 1.62 times); sphericity 0.95; bulk density 0.85 g / cm³ 3 The crushing rate at 52 MPa was 2.4% (compared to the crushing rate of ceramsite / quartz sand of the same mesh size >7%).
[0044] Comparative Example 1: Traditional batch reactor process Using the exact same raw material formulation as in Example 1, in a single 5m 3 Intermittent suspension polymerization is carried out in a reactor.
[0045] Results: The product exhibited a high breakage rate of 4.1% at 52 MPa, a particle size range of up to 2.86 times, and a sphericity of only 0.87. Significant batch-to-batch performance fluctuations were observed (RSD > 8%), requiring 2–3 hours of vessel cleaning after each batch. Overall production efficiency was more than 35% lower than that of this invention.
[0046] In summary, the core of this invention lies in constructing a fully continuous production system consisting of a continuous premixing and dispersion unit, a three-stage series gradient solidification reactor assembly, a continuous solid-liquid separation unit, and an aqueous phase closed-loop circulation unit. The entire system operates under sealed conditions and nitrogen protection. This invention enables the continuous, stable, and large-scale production of a full range of proppants from 6 to 300 mesh. The products feature a narrow particle size range (≤2 times), high sphericity (≥0.95), low density, high compressive strength, and excellent deep penetration performance.
[0047] Based on the above-described preferred embodiments of the present invention, and through the foregoing description, those skilled in the art can make various changes and modifications without departing from the inventive concept. The technical scope of this invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.
Claims
1. An industrial method for preparing thermosetting resin fracturing proppant via continuous suspension polymerization, characterized in that: Specifically, the steps include the following: Step S1, Raw material preparation: Prepare oil phase component and aqueous phase component separately. The oil phase component is stored in an oil tank and the aqueous phase component is stored in a water tank. Step S2, High-speed shear dispersion: The oil phase component is continuously pumped to the oil phase inlet of the online high-speed shear emulsifier via a constant flow pump, and the aqueous phase component is continuously pumped to the aqueous phase inlet of the online high-speed shear emulsifier via a constant flow pump; the oil phase component and the aqueous phase component are instantaneously mixed and dispersed in the high-speed shear emulsifier to form a stable oil-in-water suspension; Step S3, Three-stage series gradient temperature field continuous curing: The water-in-oil suspension obtained in step S2 is sequentially fed into a primary molding reactor, a secondary pre-curing reactor, and a tertiary deep curing reactor arranged in series, respectively to complete spherical shaping, surface cross-linking, and deep curing, to obtain a cured slurry with spherical particles; the reaction temperature of the three reactors is gradient-increased, the stirring speed of the three reactors is gradient-increased, and the three reactors are continuously cured under nitrogen protection; Step S4, solid-liquid separation, drying and grading and closed-loop circulation of aqueous phase: The solidified slurry obtained in step S3 is fed into a solid-liquid separation device for solid-liquid separation. The separated solid particles are washed, dried, screened and packaged into a warehouse in sequence. The separated aqueous slurry is filtered and then circulated in a closed loop to a water tank.
2. The industrial method for preparing thermosetting resin fracturing proppant by continuous suspension polymerization according to claim 1, characterized in that: In step S1, the oil phase component includes the following raw materials in parts by weight: 100 parts of thermosetting resin, 8-15 parts of latent microcapsule curing agent, and 0.5-2 parts of chain regulator. The aqueous phase component comprises the following raw materials in parts by weight: 300-500 parts deionized water, 2-5 parts composite dispersant, and 0.3-1 parts pH buffer adjuster.
3. The industrial method for preparing thermosetting resin fracturing proppant by continuous suspension polymerization according to claim 2, characterized in that: The composite dispersant is composed of montmorillonite, modified lignin sulfonate, and fatty alcohol polyoxyethylene ether in a mass ratio of 3:5:
2.
4. An industrial method for preparing thermosetting resin fracturing proppant by continuous suspension polymerization according to claim 1, characterized in that: When the shear rate of the high-speed shear emulsifier in step S2 is 300-500 rpm, the particle size of the solid particles obtained in step S4 is 6-12 mesh. Alternatively, when the shear rate of the high-speed shear emulsifier in step S2 is 800-1000 rpm, the particle size of the solid particles obtained in step S4 is 20-40 mesh. Alternatively, when the shear rate of the high-speed shear emulsifier in step S2 is 1800–2200 rpm, the particle size of the solid particles obtained in step S4 is 200–300 mesh.
5. An industrial method for preparing thermosetting resin fracturing proppant by continuous suspension polymerization according to claim 1, characterized in that: In step S3, the temperature of the primary molding reactor is 25–65°C and the stirring speed is 80–120 rpm; the temperature of the secondary pre-curing reactor is 65–95°C and the stirring speed is 120–160 rpm; and the temperature of the tertiary deep curing reactor is 95–125°C and the stirring speed is 150–200 rpm.
6. An industrial method for preparing thermosetting resin fracturing proppant by continuous suspension polymerization according to claim 1, characterized in that: In step S4, the solid-liquid separation device is a continuous horizontal screw centrifuge.
7. An industrial method for preparing thermosetting resin fracturing proppant by continuous suspension polymerization according to claim 1, characterized in that: In step S4, the filtration accuracy of the filtration device for the aqueous slurry is ≤5μm.