A multi-crosslinked chitosan-based long afterglow material

By using chitosan-based long afterglow materials with multiple crosslinks, the resource scarcity and stability issues of traditional room temperature phosphorescent materials have been solved, achieving high brightness and long lifespan luminescence performance, which is suitable for anti-counterfeiting and information encryption.

CN123132005APending Publication Date: 2026-11-20WUHAN TEXTILE UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510648124.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-20
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Traditional room-temperature phosphorescent materials suffer from weak luminescence and low efficiency due to scarce resources, non-degradability, high energy consumption, and the fact that polysaccharide biomass materials are prone to quenching in water and high-temperature environments, resulting in poor exciton stability.

Method used

A multi-crosslinked chitosan-based long afterglow material was prepared by using chitosan, boric acid, and inorganic salts through a multi-crosslinking reaction. This formed a dual rigid network of covalent and ionic bonds, which enhanced the rigidity and stability of the material. Doping with halogen salts enhanced spin-orbit coupling and promoted triplet radiative transitions.

Benefits of technology

It significantly enhances the phosphorescence intensity and lifespan of the material, achieving long-term luminescence stability and high-efficiency luminescence performance in air, making it suitable for applications such as anti-counterfeiting and information encryption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The application reports a kind of multiple crosslinking chitosan-based long afterglow material.Chitosan-based material is dissolved with boric acid, then inorganic salt is added, and the long afterglow material is prepared by dehydration reaction. The long afterglow material has a luminescence lifetime close to seconds by means of ion and covalent crosslinking, and the intensity and lifetime can be controlled by adjusting the doping concentration, greatly expanding the use of chitosan long afterglow material. The long afterglow material can be used in the field of anti-counterfeiting and encryption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of organic room temperature phosphorescent materials, specifically to a multi-crosslinked chitosan-based long afterglow material, its preparation method, and its application. Background Technology

[0002] Room-temperature phosphorescence (RTP) materials, as novel optoelectronic functional materials, have shown great potential in flexible displays, information encryption, and bioimaging due to their long-lifetime luminescence, large Stokes shift, and environmental responsiveness. Traditional phosphorescence systems, relying on precious metals, rare earth elements, or fossil-based polymer carriers, face bottlenecks such as resource scarcity, non-degradability, and high energy consumption during synthesis. Developing renewable, low-environmentally impactful RTP materials has become a crucial breakthrough in the field of optoelectronic functional materials. In recent years, many natural compounds that do not contain traditional luminescent groups (such as aromatic rings, aromatic heterocycles, and other unsaturated bonds) have exhibited intrinsic luminescence, a discovery that has attracted considerable research interest. Unlike traditional luminescent materials, the biocompatibility and environmental friendliness of natural substances make them promising candidates for applications in bioimaging and environmental monitoring.

[0003] Driven by the concept of green chemistry, biomass-derived phosphorescent materials have gradually become a research hotspot. However, due to the lack of aromatic ring conjugated structures, these materials exhibit weak light absorption and fewer triplet excitons, resulting in weak and inefficient room-temperature phosphorescence. Furthermore, the flexibility of polysaccharide biomass polymer chains makes it difficult to form a stable rigid environment; vibrations, rotations, and collisions of the chains at room temperature or high temperatures make excited excitons more susceptible to nonradiative transitions and inactivation. Moreover, the abundant hydroxyl groups and other groups on the polysaccharide surface, on the one hand, readily form hydrogen bonds with water molecules as hydrophilic groups, disrupting the spatial conjugated conformation between polysaccharide chains; on the other hand, these groups are easily oxidized, especially at high temperatures. Therefore, the phosphorescence of polysaccharide-based materials will quench in hot or water-enclosed environments. In recent years, many methods for stabilizing luminescence have been developed, such as ion doping / crosslinking (CN113621262 B), organic acid doping / crosslinking (CN202210242865.3), and redox reactions (Natural ultralong hemicelluloses phosphorescence. Cell Rep. Phys. Sci. 2022, 3,101015.). Summary of the Invention

[0004] To develop sustainable, environmentally friendly, luminescently stable, and lifetime-adjustable long afterglow materials, this invention discloses a multi-crosslinked chitosan-based long afterglow material. The material is characterized by being prepared from a chitosan-based material through a multi-crosslinking reaction with boric acid and inorganic salts. The molar ratio of boron to nitrogen atoms in the raw materials ranges from 50 to 1, and the molar ratio of inorganic salt to chitosan amino groups is 0.01-1. The chitosan-based material is selected from chitosan, and the inorganic salt is selected from one or more of sodium chloride, potassium chloride, magnesium chloride, calcium chloride, aluminum chloride, zinc chloride, barium chloride, potassium bromide, sodium bromide, magnesium bromide, calcium bromide, aluminum bromide, zinc bromide, and barium bromide. The above materials are derived from chitosan, boric acid, and inorganic salts.

[0005] Chitosan is a natural polysaccharide with a backbone rich in amino and hydroxyl functional groups. After dehydration, chitosan exhibits room-temperature phosphorescence; however, the hydrophilic groups such as hydroxyl and amino groups readily form hydrogen bonds with moisture in the air, inducing excited-state nonradiative relaxation and thus weakening luminescence (see Zeng L, Zhu Z, Mo R, et al. Luminescence lifetimetuning of non-conjugated organic clusters through external heavy-atom effect for smartphone-based time-resolved imaging. Chem Eng J, 2023, 460: 141452.). The amino and hydroxyl groups of chitosan can undergo dehydration condensation with boric acid in hot aqueous solutions, forming numerous covalent bonds. Simultaneously, metal ions can form ionic bonds with amino and hydroxyl groups, not only consuming a large amount of hydroxyl and amino groups capable of forming hydrogen bonds with water, but also making the structure more compact. The combined cross-linking effect of covalent and ionic bonds further increases the rigidity of the material. This cross-linking method significantly reduces nonradiative relaxation and increases the stability of triplet excitons.

[0006] The preparation method of the above material is as follows: Chitosan, boric acid, and inorganic salts are selected and subjected to a dehydration reaction under heated solvent conditions. After cooling, the mixture is placed for vacuum drying / cooling drying / blowing drying to remove residual moisture. The material undergoes multiple cross-linking processes, resulting in a significantly enhanced phosphorescence intensity compared to before cross-linking, with a lifetime of 1-1.3 s. After irradiation with a 365nm ultraviolet lamp, the phosphorescence wavelength is 400 nm-700 nm. Figure 1 The phosphorescence has a long afterglow visible to the naked eye for more than 7 seconds, and its intensity and lifespan are significantly higher than those of chitosan and boric acid. Figure 1-2 ).

[0007] Water is the preferred solvent in the above preparation process, and no other organic solvents are introduced. It is environmentally friendly, safe and harmless, and in line with the concept of green environmental protection.

[0008] To improve the crosslinking degree of materials, this invention discloses a multi-crosslinked chitosan-based long afterglow material, characterized by a chitosan deacetylation degree ≥90% and a molecular weight ≥1000. It is further characterized by the boron-containing compound being boric acid. Higher deacetylation degree and larger molecular weight result in a greater number of crosslinkable amino and hydroxyl groups. The aforementioned long afterglow material has an internal structure of a dual rigid network with covalent bonds as the backbone and ionic and hydrogen bonds as dynamic supplements, which significantly reduces non-radiative transitions.

[0009] Since both amino and boric acid groups, as well as hydroxyl and boric acid groups, can undergo dehydration reactions, a suitable feed ratio is required to ensure effective cross-linking of chitosan and boric acid. Each chitosan structural unit contains two hydroxyl groups and one amino group. To ensure sufficient reaction between chitosan and boric acid, achieve efficient covalent cross-linking, and form a dense product with optimal phosphorescence properties, a further preferred embodiment of the above material is characterized by a molar ratio of boron atoms to nitrogen atoms of 3-1 in the raw materials. Cross-linking causes the exposed hydroxyl groups on the material surface to undergo dehydration, making the surface more rigid and dense, and reducing hydrogen bonding with water.

[0010] This invention discloses a preferred multi-crosslinked chitosan-based long afterglow material, characterized in that the molar ratio of inorganic salt to chitosan amino group is 0.01-1. The role of the inorganic salt is as follows: with the addition of metal ions from the halogen salt, electrostatic and coordination interactions are introduced, further stabilizing the excited state of chitosan and thus achieving stable phosphorescence (Reference: Chemical Engineering Journal. 2023, 460, 141452.). The large nuclear charge of halogen heavy atoms / ions generates a strong Coulomb field that enhances the interaction between electron motion and spin (i.e., spin-orbit coupling, SOC). This coupling promotes intersystem crossing, generating more triplet states. The previously forbidden radiative transition (phosphorescence) from the triplet state to the ground state becomes permissible due to the enhanced SOC, resulting in higher phosphorescence intensity and the ability to regulate phosphorescence lifetime. The external electron portion of the halide ions participates in absorption transitions, enhancing light utilization. (Reference: Efficient Persistent Luminescence from Cellulose–Halide Mixtures for Optical Encryption. ACSSustainable Chemistry&Engineering 2022, 10(50): 16752-16759.).

[0011] Further preferred embodiments of the above materials include: potassium bromide, sodium bromide, magnesium bromide, calcium bromide, aluminum bromide, zinc bromide, and barium bromide, with magnesium bromide and calcium bromide being even more preferred. Because divalent metal ions can induce stronger electrostatic interactions compared to monovalent ions, reducing electrostatic repulsion of electron-rich groups and suppressing nonradiative relaxation, they enhance clustered luminescence behavior. Among halide ions, bromides enhance phosphorescence more effectively than chlorides because the external electrons of bromide ions are less constrained than those in chlorides, and spin-orbit coupling is enhanced through the heavy atom effect (Reference: Chemical Engineering Journal. 2023, 460, 141452).

[0012] Although inorganic salts are hygroscopic in air, the combined cross-linking of ions and covalent compounds enables higher brightness and more stable phosphorescence. Materials doped with inorganic salts, when placed in air for 7 days, show almost no change in fluorescence, with only a slight decrease in phosphorescence intensity and luminescence lifetime. Figures 3-5 ).

[0013] The long afterglow material has applications in room temperature phosphorescent products. Since different amounts of doped salt can be used to control its luminescence lifetime, it can be used for anti-counterfeiting, information encryption, long-life reuse and other purposes. Attached Figure Description

[0014] Figure 1 Phosphorescence spectra of chitosan, boric acid and cross-linked products.

[0015] Figure 2 Luminescence decay curves of chitosan, boric acid and cross-linked products.

[0016] Figure 3 Fluorescence spectra of the cross-linked product after 0-7 days in air.

[0017] Figure 4 The phosphorescence spectrum of the cross-linked product after 0-7 days in the air.

[0018] Figure 5 Luminescence decay curve of the cross-linked product after 0-7 days in air.

[0019] Figure 6 For the encryption application of materials. Detailed Implementation

[0020] Example 1: Products of chitosan-based multiple crosslinking Preparation Method 1: Weigh 0.018 g (0.1 mmol) of magnesium bromide, 0.026 g (0.42 mmol) of boric acid, and 0.022 g (0.14 mmol) of chitosan (90% degree of deacetylation), dissolve them in water, stir thoroughly to dissolve, and place the mixture in an oven at 80-120℃ for at least 1 hour. Then, remove the moisture from the reactants by vacuum drying to obtain the product. When the product is excited by a 365 nm UV LED in a dark room at room temperature, and after the light is turned off, a bright blue fluorescence and a green afterglow are visible to the naked eye.

[0021] Preparation Method 2: Weigh 0.0018 g (0.01 mmol) of magnesium bromide, 0.026 g (0.42 mmol) of boric acid, and 0.022 g (0.14 mmol) of chitosan (90% degree of deacetylation), dissolve them in water, stir thoroughly to dissolve, and place the mixture in an oven at 80-120℃ for at least 1 hour. Then, remove the moisture from the reactants by forced-air drying to obtain the product. When the product is excited in a dark room at room temperature using a 365 nm ultraviolet LED, and after the light is turned off, a bright blue fluorescence and a green afterglow are visible to the naked eye.

[0022] The phosphorescence intensity of the salt-containing product was significantly stronger than that of the raw material and the cross-linked product without salt doping. Figure 1 As the concentration of the doped salt increases, the intensity further improves. However, the enhanced effect of external heavy atoms accelerates the intersystem crossing rate, thus shortening the phosphorescence lifetime. Figure 2 By using salt doping, the strength and lifespan of cross-linked products can be effectively controlled. Based on a similar principle, adjusting the raw material ratio within an appropriate range can also yield corresponding cross-linked chitosan products.

[0023] The chitosan-based multi-crosslinked product prepared by method 2 was placed in air for 0-7 days, with the 7-day period including sunny days and cloudy / rainy days with high humidity. Despite the high humidity, the salt-doped product effectively stabilized the material's luminescence due to the fixation effect of the multi-crosslinking; the fluorescence remained almost unchanged, while the phosphorescence intensity and luminescence lifetime showed a slight decrease. Figure 3-5 ). Example 2: Anti-counterfeiting application of chitosan-based cross-linked salt-containing products The chitosan / boric acid crosslinking product and the crosslinking product of MgBr2 with doping ratios of 0.1 and 1 were weighed and dried at 105 °C for 5-6 min. These were then used to fill specific areas to form an "8" shaped pattern, and the afterglow emission was recorded using a smartphone. Under 255 nm, 275 nm, 310 nm, and 365 nm UV irradiation, the number "8" was observed to exhibit blue fluorescence. After the irradiation was turned off, the samples irradiated with 255 nm, 275 nm, and 310 nm UV lamps showed that the blue afterglow of the number "8" evolved into "6" over time. After irradiation with 365 nm UV, a green afterglow gradually appeared, and the number evolved from "8" to "6," and then to "5." Due to the difference in dopant salt concentration, this distinguishable RTP feature can be used for multi-level data encryption. Figure 6 ).

Claims

1. A multi-crosslinked chitosan-based long afterglow material, characterized in that: This material is prepared by multiple cross-linking reactions of chitosan-based material, boric acid, and inorganic salts. The molar ratio of boron atoms to nitrogen atoms in the raw materials ranges from 50 to 1, and the molar ratio of inorganic salts to chitosan amino groups is 0.01-1. The chitosan-based material is selected from chitosan, and the inorganic salts are selected from one or more of sodium chloride, potassium chloride, magnesium chloride, calcium chloride, aluminum chloride, zinc chloride, barium chloride, potassium bromide, sodium bromide, magnesium bromide, calcium bromide, aluminum bromide, zinc bromide, and barium bromide.

2. The long afterglow material as described in claim 1, characterized in that... Chitosan has a degree of deacetylation ≥90% and a molecular weight ≥1000.

3. The long afterglow material as described in claim 2, characterized in that... The molar ratio of boron atoms to nitrogen atoms in the raw material is 3 to 1.

4. The long afterglow material as described in claim 3 is preferably potassium bromide, sodium bromide, magnesium bromide, calcium bromide, aluminum bromide, zinc bromide, barium bromide, or yttrium bromide.

5. The bromide as described in claim 5, preferably magnesium bromide or calcium bromide.

6. The long afterglow material as described in claims 1-5, and its application in products with room temperature phosphorescence properties.

Citation Information

Patent Citations

  • A polysaccharide-based long afterglow material and its application

    CN113621262B

  • Chitosan film with room-temperature phosphorescence characteristic as well as preparation method and application thereof

    CN114605713A