Preparation method and application of tin-based perovskite single crystal luminescent material
By combining monoproton amines and diproton amine organic ligands with tin-based perovskite materials, the problems of instability and luminescence performance regulation of tin-based perovskites were solved, realizing the preparation of efficient and stable tin-based perovskite luminescent materials suitable for Sn²⁺ and Sn⁴⁺ systems, thus improving device performance and environmental safety.
Patent Information
- Application Number
- CN202611274639.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-20
AI Technical Summary
Tin-based perovskite materials suffer from instability and challenges in controlling luminescence performance, especially the problem of Sn²⁺ being easily oxidized to Sn⁴⁺, which affects device performance and environmental safety. Furthermore, traditional lead-based perovskites exhibit self-absorption effects and narrow emission spectra, impacting color rendering index and lighting quality.
By combining monoprotic amines and diprotic amine organic ligands with Sn²⁺ and Sn⁴⁺ systems, and heating the mixed solution under an inert atmosphere using a solution method, tin-based perovskite single-crystal luminescent materials with different structures were prepared, overcoming instability and improving luminescence performance.
It significantly improves the photoluminescence quantum yield of tin-based perovskites, enhances luminescence intensity and stability, broadens the compositional range of materials, simplifies the preparation process, and meets the requirements of environmental friendliness.
Smart Images

Figure CN123132006A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of perovskite luminescent materials technology, specifically to tin-based perovskite single-crystal luminescent materials, and more specifically to a method for preparing tin-based perovskite single-crystal luminescent materials based on monoprotonated amines and diprotonated amine organic ligands, and their applications. Background Technology
[0002] Semiconductor materials are the cornerstone of modern information society. Traditional semiconductors, represented by silicon and III-V compounds, have achieved large-scale production of large-size, high-quality wafers through decades of crystal fabrication technology development, laying the foundation for the integrated circuit and optoelectronic industries. Meanwhile, organometal halide perovskite materials, with their superior properties such as high optical absorption coefficient, balanced electron-hole mobility, long carrier lifetime, and micron-level diffusion length, have become core candidate materials for next-generation optoelectronic functional devices. They exhibit superior optoelectronic properties and greater multifunctionality in a wide range of applications, including solar cells, light-emitting diodes (LEDs), laser diodes, high-energy (such as X-ray and gamma-ray) radiation detectors, and scintillators. In recent years, perovskite materials have received significant attention in the fields of detectors and luminescent materials due to their unique photophysical properties. Researchers are focusing on perovskite morphology, chemical composition, and ion doping, striving to control the emission color and efficiency of perovskite devices. It is one of the fastest-growing optoelectronic technologies in recent years, demonstrating strong development potential.
[0003] Lead halide perovskites currently show promising applications in luminescence, but their practical use is limited by several key issues. A major problem is the self-absorption effect and narrow emission spectrum, which ultimately reduces the Color Rendering Index (CRI), thus affecting lighting quality. Furthermore, the presence of toxic heavy metals such as lead (Pb) poses serious environmental and health problems, creating significant challenges to their long-term sustainability and regulatory approval in consumer products. To address these limitations and meet the growing demand for safe, efficient, and high-CRI lighting, developing lead-free perovskite materials as ideal candidates for next-generation, environmentally friendly optoelectronic devices is crucial.
[0004] Based on the aforementioned issues, tin-based perovskites have emerged and are currently considered one of the most promising lead-free materials, attracting widespread attention. Tin and lead have similar ionic radii, electronic configurations, and coordination behaviors, thus possessing comparable electronic structures and optoelectronic properties. These similarities make tin-based perovskites a strong candidate for next-generation optoelectronic applications. However, due to the lack of Pb... 2+ The inert pair effect, Sn 2+Tin halide perovskites readily oxidize from the +2 state to the +4 state, even in the absence of oxygen and water, leading to severe deep-seated defects. This instability significantly impacts device performance, severely limiting their commercial potential and long-term operational stability.
[0005] Besides stability issues, regulating the luminescence properties of tin-based perovskites is a key research focus and challenge. Studies have shown that altering the structure of organic ligands (such as chain length, type and number of functional groups) can effectively modulate the dimensionality and electronic structure of perovskites, thereby affecting their luminescence behavior. Among these, monoproton and diproton amine organic ligands, due to their different bonding modes with the inorganic layer, can form RP (Ruddlesden-Popper) and DJ (Dion-Jacobson) type perovskites, respectively, exhibiting significant differences in exciton binding energy, carrier dynamics, and luminescence efficiency. Currently, research based on monoproton and diproton amine ligands mainly focuses on lead-based perovskite systems, while systematic comparative studies on tin-based perovskites are scarce. In particular, whether diproton amine ligands can achieve equally efficient luminescence in tin-based systems and whether they are simultaneously applicable to Sn... 2+ and Sn 4+ The two valence states, and whether they can alleviate the inherent oxidation instability of tin-based perovskites, require further investigation.
[0006] Therefore, developing a method for preparing and controlling the luminescence of tin-based perovskite single-crystal luminescent materials based on monoprotonated amines and diprotonated amine organic ligands, systematically studying the influence of ligand structure and metal valence state on luminescence performance, and realizing efficient, stable, and environmentally friendly tin-based perovskite luminescent materials has important scientific significance and application value. Summary of the Invention
[0007] This invention addresses the aforementioned problems by providing a method for regulating the luminescence properties of tin-based perovskites, a tin-based perovskite material prepared based on this method, and an optoelectronic device containing the tin-based perovskite material.
[0008] This invention uses Sn 2+ System and Sn 4+ As a tin-based material, different tin-based perovskites were prepared using monoprotonated and diprotonated amine organic ligands. Samples prepared by solution methods with SnO and SnBr4 using 4-aminobenzylamine (4-ABZA), a diprotonated amine-like organic ligand, showed significantly improved luminescence properties compared to samples prepared with benzylamine (BZA), a monoprotonated amine-like organic ligand, and to some extent, overcame the instability of tin-based perovskites. This modulation method is applicable to Sn... 2+ The system also applies to Sn. 4+ system.
[0009] Based on the above research, the technical solution of the present invention is as follows:
[0010] In a first aspect, this invention provides a method for preparing a tin-based perovskite single-crystal luminescent material. The tin-based perovskite single-crystal luminescent material includes divalent tin-based perovskite single-crystal luminescent materials and tetravalent tin-based perovskite single-crystal luminescent materials. The specific preparation methods for the two luminescent materials are described below:
[0011] Preparation of monovalent and divalent tin-based perovskite single-crystal luminescent materials
[0012] A mixed solution is prepared by mixing divalent tin oxide or halide, hypophosphorous acid, hydrobromic acid, and an amine organic ligand. The mixed solution is heated at 90-120°C under an inert gas atmosphere until clear. The clarified reaction solution is allowed to stand and crystallize to obtain the divalent tin-based perovskite single-crystal luminescent material. The amine organic ligand is either a monoprotonated amine with one amino group or a diprotonated amine with two amino groups.
[0013] Preferably, the divalent tin oxide or halide is selected from stannous oxide (SnO), stannous chloride (SnCl2), or stannous bromide (SnBr2).
[0014] The monoprotic amine is selected from any one or more combinations of benzylamine (BZA), phenethylamine (PEA), 3-methylbenzylamine, n-hexylamine, hexamethylenediamine, n-octylamine, and octyldiamine;
[0015] The diproton amine is selected from any one or a combination of 4-aminobenzylamine (4-ABZA), 4-aminophenylethylamine (4-APEA), 3-aminobenzylamine, and 4-(aminomethyl)phenylethylamine.
[0016] Furthermore, the molar ratio of tin oxide or halide to monoprotic amine organic ligand is in the range of 1-3:1, preferably 1:1; the molar ratio of tin oxide or halide to diprotic amine organic ligand is in the range of 1-3:1, preferably 2:1.
[0017] Furthermore, the molar volume ratio of tin oxide or halide to hypophosphite and hydrobromic acid is 1 mol: 1-10 mL, preferably 1 mol: 3-7 mL, and most preferably 1 mol: 5 mL; the volume ratio of hydrobromic acid to hypophosphite is 3:1.
[0018] Furthermore, the heating time is 1-2 hours, and the conditions for static crystallization are 2-48 hours at room temperature.
[0019] II. Preparation of tetravalent tin-based perovskite single-crystal luminescent materials
[0020] A mixed solution is obtained by mixing tetravalent tin oxide or halide, a polar aprotic organic solvent and / or hydrobromic acid, and an amine organic ligand; the mixed solution is heated at 90~120℃ under an inert gas atmosphere until it becomes clear, and the clear reaction solution is allowed to stand and crystallize to obtain a tetravalent tin-based perovskite single crystal luminescent material.
[0021] Wherein, the amine organic ligand is a monoprotic amine with one amino group or a diprotic amine with two amino groups; when the organic ligand is a monoprotic amine, hydrobromic acid is used as the solvent; when the organic ligand is a diprotic amine, a polar aprotic organic solvent is used, and hydrobromic acid is used as the acid reaction reagent.
[0022] Preferably, the tin oxide or halide is selected from tin oxide, tin chloride, or tin bromide;
[0023] The monoprotic amine is selected from any one or more combinations of benzylamine (BZA), phenethylamine (PEA), 3-methylbenzylamine, n-hexylamine, hexamethylenediamine, n-octylamine, and octyldiamine;
[0024] The diprotonated amine is selected from any one or a combination of 4-aminobenzylamine (4-ABZA), 4-aminophenylethylamine (4-APEA), 3-aminobenzylamine, and 4-(aminomethyl)phenylethylamine;
[0025] The polar aprotic organic solvent is selected from any one or more of dimethyl sulfoxide, N,N-dimethylformamide, tetrahydrofuran, and dichloromethane, preferably dimethyl sulfoxide or N,N-dimethylformamide.
[0026] Furthermore, the molar ratio of tin oxide or halide to the amine organic ligand is in the range of 1-3:1. When the amine organic ligand is a monoprotic amine, the ratio is preferably 1:1; when the amine organic ligand is a diprotic amine, the ratio is preferably 2:1.
[0027] The molar ratio of diprotic amine to hydrogen bromide is 1 to 3:1. The two first form diprotic amine bromide, which then reacts with tin oxide or halide.
[0028] Furthermore, the heating time is 1-2 hours, and the conditions for static crystallization are 2-48 hours at room temperature.
[0029] In a preferred embodiment of the present invention, when preparing divalent tin-based perovskite single-crystal luminescent materials, stannous oxide (SnO) is used as a representative of divalent tin materials, and benzylamine (BZA) and 4-aminobenzylamine (4-ABZA) are used as representatives of monoproton amine and diproton amine, respectively, to prepare BZA2SnBr4 and 4-ABZA2SnBr4 perovskites, as follows:
[0030] (1) Mix the mixed solution of SnO, HBr and H3PO2 with BZA and 4-ABZA respectively to obtain mixed solution reaction solution 1 and 2;
[0031] (2) Under an inert atmosphere, heat the mixed solution reaction liquid at 90~120℃ for 1-2 hours until the reaction liquid becomes clear;
[0032] (3) Let the clarified reaction solution stand for a period of time to obtain the perovskite single crystal material.
[0033] Preferably, the molar ratio of SnO to BZA is in the range of 1-3:1, and the molar ratio of SnO to 4-ABZA is in the range of 1-3:1.
[0034] The molar volume ratio of SnO and HBr:H3PO2 is in the range of 1mol:1-10mL, preferably 1mol:5mL; the volume ratio of HBr and H3PO2 is 3:1.
[0035] In the preparation of tetravalent tin-based perovskite single-crystal luminescent materials, tin bromide (SnBr4) is used as the representative of tetratin materials, and benzylamine (BZA) and 4-aminobenzylamine (4-ABZA) are used as the representatives of monoproton amine and diproton amine, respectively, to prepare BZA2SnBr6 and 4-ABZA2SnBr6·2Br perovskites, as follows:
[0036] (1) Mix SnBr4 and HBr with BZA respectively to obtain mixed solution reaction solution 3;
[0037] (2) 4-ABZA is first mixed with HBr, and the mixed solution is placed in an ice-water bath for 2-3 hours. The mixed solvent after the ice-water bath is then rotary evaporated to obtain 4-ABZABr2.
[0038] (3) Mix SnBr4, organic solvent and 4-ABZABr2 respectively to obtain mixed solution reaction solution 4;
[0039] (4) Heat either the mixed solution reaction solution 3 or the mixed solution reaction solution 4 for 1-2 hours until the reaction solution becomes clear;
[0040] (5) Let the clarified reaction solution stand for a period of time to obtain the perovskite single crystal material.
[0041] Preferably, the molar ratio of 4-ABZA to HBr is 2:1;
[0042] Preferably, the molar ratio of SnBr4 to BZA is in the range of 1-3:1, and the molar ratio of SnBr4 to 4-ABZABr2 is in the range of 1-3:1.
[0043] According to a preferred embodiment of the present invention, BZA2SnBr4 and 4-ABZASnBr4 are both two-dimensional structures with good crystallinity and belong to the orthorhombic crystal system; BZA2SnBr6 and 4-ABZA2SnBr6·2Br are zero-dimensional structures with good crystallinity; BZA2SnBr6 belongs to the orthorhombic crystal system and 4-ABZA2SnBr6·2Br belongs to the monoclinic crystal system.
[0044] Among divalent tin-based perovskite single-crystal luminescent materials, 4-ABZASnBr4 perovskite material exhibits higher luminescence intensity. The PLQY of 4-ABZASnBr4 is 28.6%, while that of BZA2SnBr4 is 3.4%. The PLQY is improved by adding an amino group at the para-position of the benzene ring.
[0045] Among tetravalent tin-based perovskite single-crystal luminescent materials, the luminescence intensity of 4-ABZA2SnBr6·2Br perovskite material is higher than that of BZA2SnBr6, with a PLQY of 8.2% compared to 2.1% for BZA2SnBr6.
[0046] Therefore, in this invention, diprotic amines are preferably used as amine organic ligands to prepare tin-based perovskite single-crystal luminescent materials or tetravalent tin-based perovskite single-crystal luminescent materials.
[0047] In a second aspect, this invention provides a tin-based perovskite single-crystal luminescent material, prepared by any of the methods described above, preferably using a diprotonated amine as the amine organic ligand. Experimental results show that the luminescent material prepared using a diprotonated amine as the amine organic ligand exhibits superior fluorescence lifetime, luminescence intensity, band gap, thermal stability, and luminescence color purity compared to that prepared using a monoprotonated amine organic ligand.
[0048] Therefore, this invention provides a new way to regulate the luminescence properties of tin-based perovskite single-crystal luminescent materials by selecting different types of amine organic ligands.
[0049] In a third aspect, the present invention provides the application of the aforementioned tin-based perovskite single-crystal luminescent material in the fabrication of optoelectronic functional devices.
[0050] In a fourth aspect, this invention provides an optoelectronic functional device prepared from the above-described materials, including a solar cell, a light-emitting diode, a laser diode, a radiation detector, and a scintillator. By using a performance-optimized tin-based perovskite single-crystal light-emitting material, the stability and luminous performance of the device are improved.
[0051] The role and effect of invention
[0052] The modulation method involved in this invention can significantly improve luminescence performance: By introducing organic ligands containing diprotonated amine groups, this invention significantly improves the photoluminescence quantum yield (PLQY) of tin-based perovskite materials compared to traditional monoprotonated amine ligands. Specifically, the PLQY of 4-ABZASnBr4 reaches 28.6%, while that of BZA2SnBr4 is only 3.4%; the PLQY of 4-ABZA2SnBr6·2Br is 8.2%, while that of BZA2SnBr6 is only 2.1%. This indicates that adding amino functional groups at the para-position of the benzene ring can effectively modulate the electronic structure and radiative recombination efficiency of the material, significantly enhancing the luminescence intensity.
[0053] The control method involved in this invention can overcome the instability of tin-based perovskites: traditional tin-based perovskites are confined by Sn 2+ Easily oxidized to Sn 4+ This problem leads to a decrease in device performance. The light emission modulation method proposed in this invention is not only applicable to Sn 2 + The system can also be applied to Sn. 4+ The system successfully prepared 4-ABZASnBr4 and 4-ABZA2SnBr6·2Br materials with good luminescence properties. 4+ The system also exhibits excellent luminescent properties, breaking through traditional understanding. This broadens the compositional range of tin-based perovskites, effectively alleviates the performance degradation problem caused by oxidation, and enhances the environmental stability and application potential of the material.
[0054] The control method involved in this invention is simple and the synthesis conditions are mild: the solution preparation process used in this invention only requires heating the mixed reaction solution under an inert atmosphere for 1-2 hours until it becomes clear, and then allowing it to stand at room temperature for 2-48 hours to obtain high-quality single crystals. The entire process does not require complex equipment or extreme conditions, and is simple to operate and has good repeatability.
[0055] The synthesis method involved in this invention is environmentally friendly and meets the needs of sustainable development: this invention completely eliminates the toxic lead element and uses non-toxic tin-based materials, while the solvents and ligands used in the synthesis process are all common chemicals.
[0056] In summary, this invention successfully modulates the luminescence properties of tin-based perovskites by introducing diproton amine organic ligands, demonstrating significant technological advancement and practical value. Attached Figure Description
[0057] Figure 1Microscopic images of BZA2SnBr4 (a), 4-ABZASnBr4 (b), BZA2SnBr6 (c), and 4-ABZA2SnBr6·2Br (d) prepared in Examples 1-4: BZA2SnBr4 is bright yellow overall and is a bright yellow, highly symmetrical plate-like crystal; 4-ABZASnBr4 exhibits a typical elongated crystal morphology; BZA2SnBr6 maintains a highly symmetrical polygonal outline overall, and the crystal shape is well regular; 4-ABZA2SnBr6·2Br exhibits a typical double-pointed leaf morphology.
[0058] Figure 2 The images show the crystal structures of BZA2SnBr4 (a, e), 4-ABZASnBr4 (b, f), BZA2SnBr6 (c, g), and 4-ABZA2SnBr6·2Br (d, h) prepared in Examples 1-4. BZA2SnBr4 exhibits a typical two-dimensional layered perovskite structure, with the inorganic portion being [SnBr4]. 2− Octahedral layers form a continuous planar layer; BZA2SnBr6 is an isolated, discrete [SnBr6] layer. 2− Octahedral, with organic cations distributed in the interstices of the octahedrons, separating the inorganic octahedrons from each other; the inorganic part of 4-ABZASnBr4 is [SnBr4]. 2− Octahedral layers form a continuous planar layer; 4-ABZA2SnBr6·2Br is an organic cation and free Br⁻ co-filling [SnBr6]. 2− In the octahedral interstices;
[0059] Figure 3 X-ray powder diffraction patterns of BZA2SnBr4 (a), 4-ABZASnBr4 (b), BZA2SnBr6 (c) and 4-ABZA2SnBr6·2Br (d) prepared in Examples 1-4;
[0060] Figure 4 X-ray powder diffraction patterns and simulated X-ray powder diffraction comparison diagrams of BZA2SnBr4, 4-ABZASnBr4, BZA2SnBr6 and 4-ABZA2SnBr6·2Br prepared in Examples 1-4.
[0061] Figure 5 The bond length distribution diagrams of BZA2SnBr4 and 4-ABZASnBr4 (a), BZA2SnBr6 and 4-ABZA2SnBr6·2Br (b) prepared in Examples 1-4 are shown.
[0062] Figure 6Bond angle distribution diagrams of BZA2SnBr4 and 4-ABZASnBr4 (a), BZA2SnBr6 and 4-ABZA2SnBr6·2Br (b) prepared in Examples 1-4;
[0063] Figure 7 The fluorescence lifetimes of BZA2SnBr4 and 4-ABZASnBr4 (a), BZA2SnBr6 and 4-ABZA2SnBr6·2Br (b) prepared in Examples 1-4 are shown. The fluorescence lifetime of BZA2SnBr4 is 2.13 ns, that of 4-ABZASnBr4 is 3.39 ns, that of BZA2SnBr6 is 1.10 ns, and that of 4-ABZA2SnBr6·2Br is 2.13 ns.
[0064] Figure 8 The fluorescence spectra of BZA2SnBr4 and 4-ABZASnBr4 (a), BZA2SnBr6 and 4-ABZA2SnBr6·2Br (b) prepared in Examples 1-4 are shown. Among them, BZA2SnBr4 has almost no obvious fluorescence emission signal and extremely low luminescence intensity; while 4-ABZASnBr4 exhibits a very strong single-peak characteristic emission, with the emission peak located in the 600–700 nm range; the overall fluorescence signal of BZA2SnBr6 is very weak, while the emission range of 4-ABZA2SnBr6·2Br covers 500–750 nm, and the emission intensity is significantly higher than that of BZA2SnBr6.
[0065] Figure 9 The luminescence of 4-ABZASnBr4 (a) and 4-ABZA2SnBr6·2Br (b) prepared in Examples 2 and 4 under UV light;
[0066] Figure 10 CIE chromaticity diagrams of 4-ABZASnBr4 and 4-ABZA2SnBr6·2Br prepared in Examples 2 and 4;
[0067] Figure 11 The UV-Vis absorption spectra and band gap diagrams of BZA2SnBr4 (a), 4-ABZASnBr4 (b), BZA2SnBr6 (c), and 4-ABZA2SnBr6·2Br (d) prepared in Examples 1-4 are shown. The band gaps of the four materials are 2.49, 3.16, 2.64, and 2.42 eV, respectively. Among the two-dimensional layered structures, the band gap of 4-ABZASnBr4 is significantly larger than that of BZA2SnBr4. Among the zero-dimensional structures, BZA2SnBr6 and 4-ABZA2SnBr6·2Br have different band gaps. - The introduction of this effectively narrows the bandgap of 4-ABZA2SnBr6·2Br;
[0068] Figure 12 The excitation and emission spectra of BZA2SnBr4 (a), 4-ABZASnBr4 (b), BZA2SnBr6 (c) and 4-ABZA2SnBr6·2Br (d) prepared in Examples 1-4 are shown. Both types of BZA-based crystals exhibit obvious fluorescence quenching and extremely low visible light emission intensity. Both types of 4-ABZA-based crystals can produce strong emission.
[0069] Figure 13 The light intensity-dependent PL spectra of BZA2SnBr4 (a), 4-ABZASnBr4 (b), BZA2SnBr6 (c) and 4-ABZA2SnBr6·2Br (d) prepared in Examples 1-4 are shown. BZA2SnBr4 and BZA2SnBr6 show no obvious emission signal in the entire spectrum, 4-ABZASnBr4 can achieve high-purity narrowband orange-red light emission, and 4-ABZA2SnBr6·2Br exhibits broad-spectrum yellow-green light emission.
[0070] Figure 14 Temperature-dependent PL spectra of 4-ABZASnBr4 (a) and 4-ABZA2SnBr6·2Br (b) prepared in Examples 2 and 4. Detailed Implementation
[0071] Experimental methods in the following examples, unless otherwise specified, are generally performed under standard conditions or as recommended by the manufacturer. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of skill in the art. Furthermore, any methods and materials similar or equivalent to those described herein may be used in this invention. The preferred embodiments and materials described herein are for illustrative purposes only.
[0072] I. Preparation of Tin-based Perovskite Single-Crystal Luminescent Materials
[0073] Example 1: Preparation of divalent tin-based perovskite single-crystal luminescent materials using monoprotic amines as amine organic ligands
[0074] Weigh 1 mmol of stannous oxide and 1 mmol of benzylamine into a 10 ml glass bottle using an analytical balance in a glove box at room temperature. Dissolve the 1 mmol in a 5 ml solution of HBr:H3PO2 in a 3:1 ratio to obtain a 0.2 mol / L perovskite solution. Purge the glass bottle with nitrogen and heat to 100 °C with stirring for 2 hours. After standing at room temperature for a period of time, the product precipitates. The product is then crushed, ground, washed, and processed to obtain a tin-based perovskite material with the molecular formula (C7H2O). 10 N)2SnBr4.
[0075] Example 2: Preparation of divalent tin-based perovskite single-crystal luminescent materials using diprotonated amines as amine organic ligands
[0076] Weigh 2 mmol of stannous oxide and 1 mmol of 4-aminobenzylamine using an analytical balance in a glove box at room temperature. Place them in a 10 ml glass bottle and dissolve them in 5 ml of a 3:1 HBr:H3PO2 mixed solution. This helps prevent Sn from forming. 2+ Oxidation was performed to obtain a 0.2 mol / L perovskite mixed solution. Nitrogen gas was bubbled into a glass bottle, and the solution was heated to 100°C with stirring for 2 hours. After standing at room temperature for a period of time, the product precipitated. The product was then crushed, ground, washed, and post-processed to obtain a tin-based perovskite material with the molecular formula (C7H). 12 N2)SnBr4.
[0077] The crystal prepared in this example has an actual composition of (C7H). 13 N2) 0.5 (C7H 12 N2) 1.5 Sn2Br 7.75 The crystal exhibits atomic partial occupancy and lattice disorder, and its main chemical framework corresponds to an integral compound (C7H). 12 N2)SnBr4.
[0078] Example 3: Preparation of tetravalent tin-based perovskite single-crystal luminescent materials using monoprotic amines as amine organic ligands
[0079] Weigh out 1 mmol of tin tetrabromide and 1 mmol of benzylamine using an analytical balance and place them in a 25 ml beaker. Add 10 ml of HBr to obtain a perovskite mixed solution with a concentration of 0.1 mol / L. Heat the solution to 100 °C at 700 rpm with stirring for 2 hours until the solution becomes clear. After standing at room temperature for a period of time, the product precipitates. The product is then crushed, ground, washed, and post-processed to obtain a tin-based perovskite material with the molecular formula (C7H). 10 N)2SnBr6.
[0080] Example 4: Preparation of tetravalent tin-based perovskite single-crystal luminescent materials using diprotonated amines as amine organic ligands
[0081] Weigh 4-ABZA and HBr at a molar ratio of 2:1. Mix the 4-ABZA raw material with hydrobromic acid thoroughly to obtain a homogeneous mixed solution. Place the mixed solution in an ice-water bath and stir for 2-3 hours. After the ice-water bath treatment, remove the solvent by rotary evaporation under reduced pressure to obtain the solid precursor 4-ABZABr2 for later use. Weigh tin tetrabromide (SnBr4) and the prepared 4-ABZABr2 solid at a molar ratio of 1-3:1. Add both to an organic solvent, such as dimethyl sulfoxide (DMSO) or N,N-dimethylformamide (DMF), and stir continuously to obtain a homogeneous and transparent mixed reaction solution. Heat the prepared mixed reaction solution at 700 rpm to 100°C and stir for 2 hours until the solid in the system is completely dissolved and the reaction solution is completely clear with no visible precipitate. The heated and clarified reaction solution was transferred to a room-temperature static environment for slow crystallization. After a period of static growth, crystals precipitated. The crystals were collected, washed, and dried to obtain the target hybrid perovskite single crystal material with the molecular formula (C7H). 12 N2)2SnBr6·2Br.
[0082] II. Performance Characterization
[0083] 1. Physical property characterization
[0084] Figure 1 These are microscopic images of BZA2SnBr4, 4-ABZASnBr4, BZA2SnBr6, and 4-ABZA2SnBr6·2Br prepared in Examples 1-4. The results show that BZA2SnBr4 is generally bright yellow and is a bright yellow, highly symmetrical plate-like crystal. Figure 1 a); 4-ABZASnBr4 exhibits a typical elongated crystalline morphology ( Figure 1 b); BZA2SnBr6 maintains a highly symmetrical polygonal outline, and the crystals have good regularity in shape. Figure 1 c); 4-ABZA2SnBr6·2Br exhibits a typical double-cusped leaf morphology ( Figure 1 d).
[0085] Figure 2 Crystal structure diagrams of BZA2SnBr4, 4-ABZASnBr4, BZA2SnBr6, and 4-ABZA2SnBr6·2Br prepared in Examples 1-4 are shown. The results show that BZA2SnBr4 is a typical two-dimensional layered perovskite structure. Figure 2 a) The inorganic component is [SnBr4]. 2− Octahedrons form continuous planar layers ( Figure 2 e); BZA2SnBr6 is an isolated [SnBr6] component. 2− Octahedron ( Figure 2(b) Organic cations are distributed in the interstices of the octahedrons, separating the inorganic octahedrons from each other. Figure 2 f); 4-ABZASnBr4 also has a two-dimensional layered perovskite structure ( Figure 2 c) The inorganic part is [SnBr4]. 2− Octahedrons form continuous planar layers ( Figure 2 g); 4-ABZA2SnBr6·2Br is an organic cation and free Br⁻ co-filling [SnBr6]. 2− In the octahedral interstices ( Figure 2 d, 2h).
[0086] Figure 3 X-ray powder diffraction patterns of BZA2SnBr4, 4-ABZASnBr4, BZA2SnBr6 and 4-ABZA2SnBr6·2Br prepared in Examples 1-4; Figure 4 X-ray powder diffraction patterns and simulated X-ray powder diffraction comparisons of BZA2SnBr4, 4-ABZASnBr4, BZA2SnBr6, and 4-ABZA2SnBr6·2Br prepared in Examples 1-4 are shown. The results indicate that the two-dimensional perovskite single-crystal material BZA2SnBr4 obtained in Example 1 has good crystallinity; its diffraction peak positions and relative intensities are consistent with the simulated single-crystal diffraction data, belonging to the orthorhombic crystal system. Figure 4 a); The perovskite single crystal material 4-ABZASnBr4 obtained in Example 2 has diffraction peak positions and relative intensities consistent with the simulated single crystal diffraction data, and also belongs to the orthorhombic crystal system ( Figure 4 b); The BZA2SnBr6 zero-dimensional perovskite single crystal material obtained in Example 3 has good crystallinity, and its diffraction peak positions and relative intensities are consistent with the simulated single crystal diffraction data, belonging to the orthorhombic crystal system ( Figure 4 c); The 4-ABZA2SnBr6·2Br zero-dimensional perovskite single crystal material obtained in Example 4 has good crystallinity, and its diffraction peak positions and relative intensities are consistent with the simulated single crystal diffraction data, belonging to the monoclinic crystal system ( Figure 4 d).
[0087] Figure 5 The bond length distribution diagrams for BZA2SnBr4, 4-ABZASnBr4, BZA2SnBr6, and 4-ABZA2SnBr6·2Br prepared in Examples 1-4 are shown. The results indicate that in the divalent tin-based perovskite single-crystal luminescent materials, the bond length of 4-ABZASnBr4 is greater than that of BZA2SnBr4; conversely, in the tetravalent tin-based perovskite single-crystal luminescent materials, the bond length of 4-ABZA2SnBr6·2Br is shorter than that of BZA2SnBr6.
[0088] Figure 6The image shows the bond angle distribution of BZA2SnBr4, 4-ABZASnBr4, BZA2SnBr6, and 4-ABZA2SnBr6·2Br prepared in Examples 1-4. The results show that in divalent and tin-based perovskite single-crystal luminescent materials, the bond angle of 4-ABZASnBr4 is larger than that of BZA2SnBr4; the tetravalent tin-based perovskite single-crystal luminescent materials also show a similar trend, with the bond angle of 4-ABZA2SnBr6·2Br also longer than that of BZA2SnBr6. However, the difference between the materials prepared using diprotonated amine ligands and those prepared using monoprotonated amine ligands is smaller in the tetravalent tin-based perovskite single-crystal luminescent material images.
[0089] 2. Application performance characterization
[0090] 2.1 Luminescence lifetime test
[0091] The absorbance and fluorescence lifetime of BZA2SnBr4, 4-ABZASnBr4, BZA2SnBr6, and 4-ABZA2SnBr6·2Br prepared in Examples 1-4 were recorded by fluorescence testing. See Table 1 below for details. Figure 7 .
[0092] Table 1 Absorbance and fluorescence lifetime of tin-based perovskite single-crystal luminescent materials in Examples 1-4
[0093]
[0094] Under laser excitation, the BZA2SnBr4 two-dimensional perovskite single crystal material obtained in Example 1 exhibited a double-exponential decay fluorescence lifetime pattern with a fluorescence lifetime of 2.13 ns; the perovskite single crystal material obtained in Example 2 also exhibited a double-exponential decay fluorescence lifetime pattern with a fluorescence lifetime of 3.39 ns. This indicates that adding amino functional groups at the para-position of the benzene ring can effectively regulate the electronic structure and radiative recombination efficiency of the material, significantly enhancing the minority carrier lifetime. Figure 7 a). The BZA2SnBr6 zero-dimensional perovskite single crystal material obtained in Example 3 exhibits a fluorescence lifetime diagram with double exponential decay, with a fluorescence lifetime of 1.10 ns, which is lower than that of BZA2SnBr4; the 4-ABZA2SnBr6·2Br zero-dimensional perovskite single crystal material obtained in Example 4 exhibits a fluorescence lifetime diagram with double exponential decay ( Figure 7 b). The fluorescence lifetime of 4-ABZA2SnBr6·2Br is higher than that of BZA2SnBr6, but slightly lower than that of 4-ABZASnBr4, indicating that the diproton amine ligand is associated with Sn. 4+ The system is equally effective, but Sn 4+ Intrinsic defects still have some impact on carrier lifetime.
[0095] 2.2 Detection of luminous intensity and type
[0096] Figure 8 The fluorescence spectra of BZA2SnBr4, 4-ABZASnBr4, BZA2SnBr6, and 4-ABZA2SnBr6·2Br prepared in Examples 1-4 are shown. The results show that BZA2SnBr4 exhibits almost no obvious fluorescence emission signal and extremely low luminescence intensity; while 4-ABZASnBr4 displays a very strong single-peak characteristic emission, with the emission peak located in the 600–700 nm range; the overall fluorescence signal of BZA2SnBr6 is very weak, and the emission range of 4-ABZA2SnBr6·2Br covers 500–750 nm, with a significantly higher emission intensity than BZA2SnBr6.
[0097] Specifically, BZA2SnBr4, under 395 nm UV excitation, exhibits an emission spectrum covering 500–700 nm, with a distinct broad emission peak and a PLQY of 3.4%, indicating weak luminescence. 4-ABZASnBr4, under 395 nm UV excitation, has an emission spectrum covering 600–700 nm, with its emission peak mainly located around 625 nm and a PLQY of 28.6%. The addition of an amino functional group at the para-position of the benzene ring improves the luminescence efficiency. Figure 8 a) Under 395 nm UV excitation, BZA2SnBr6 emits a spectrum covering 400–700 nm with a relatively broad emission peak and a PLQY of 2.1%. Compared to BZA2SnBr4, its overall performance is lower. 4-ABZA2SnBr6·2Br, under 395 nm UV excitation, emits a spectrum covering 500–750 nm with a peak mainly around 514 nm, exhibiting bimodal emission and a PLQY of 8.2%. The addition of an amino functional group at the para-position of the benzene ring improves the luminescence efficiency. Figure 8 b).
[0098] Figure 9 The image shows the luminescence of 4-ABZASnBr4 and 4-ABZA2SnBr6·2Br prepared in Examples 2 and 4 under UV light. 4-ABZASnBr4 emits orange-red light under UV light. Figure 9 a), 4-ABZA2SnBr6·2Br emits a yellow light under UV light ( Figure 9 b).
[0099] Figure 10 The CIE chromaticity diagrams of 4-ABZASnBr4 and 4-ABZA2SnBr6·2Br prepared in Examples 2 and 4 are shown. Under UV light, 4-ABZASnBr4 is orange and 4-ABZA2SnBr6·2Br is yellow, showing a clear difference between the two.
[0100] 2.3 Detection of luminous width
[0101] Figure 11 The UV-Vis absorption spectra and band gap diagrams of BZA2SnBr4, 4-ABZASnBr4, BZA2SnBr6, and 4-ABZA2SnBr6·2Br prepared in Examples 1-4 are shown. The band gaps of the four materials are 2.49 (…). Figure 11 a) 3.16 Figure 11 b), 2.64 ( Figure 11 c), 2.42 eV ( Figure 11 d) In the two-dimensional layered structure, 4-ABZA2SnBr4 has a significantly larger band gap than BZA2SnBr4. In the zero-dimensional structures, BZA2SnBr6 and 4-ABZA2SnBr6·2Br have different band gaps in their free Br content. - The introduction of this effectively narrows the bandgap of 4-ABZA2SnBr6·2Br.
[0102] 2.4 Stability Testing
[0103] Figure 12 The excitation and emission spectra of BZA2SnBr4, 4-ABZASnBr4, BZA2SnBr6 and 4-ABZA2SnBr6·2Br prepared in Examples 1-4 are shown. Both types of BZA-based crystals exhibit obvious fluorescence quenching and extremely low visible light emission intensity. Both types of 4-ABZA-based crystals can produce strong emission.
[0104] Figure 13 The light intensity-dependent PL spectra of BZA2SnBr4, 4-ABZASnBr4, BZA2SnBr6 and 4-ABZA2SnBr6·2Br prepared in Examples 1-4 are shown. BZA2SnBr4 and BZA2SnBr6 show no obvious emission signal in the entire spectrum, 4-ABZASnBr4 can achieve high-purity narrowband orange-red light emission, and 4-ABZA2SnBr6·2Br exhibits broadband yellow-green light emission.
[0105] Figure 14 Temperature-dependent PL spectra of 4-ABZASnBr4 and 4-ABZA2SnBr6·2Br prepared in Examples 2 and 4 were obtained. The tests showed that 4-ABZASnBr4 can increase the luminescence intensity of the sample at high temperature, while 4-ABZA2SnBr6·2Br can increase the luminescence intensity of the sample at low temperature. The thermal stability and luminescence color purity of 4-ABZASnBr4 are much better than those of 4-ABZA2SnBr6·2Br.
[0106] In summary, the above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
[0107] The undescribed parts of this invention are the same as or implemented using existing technology. The applicant declares that this invention is illustrated through the above specific embodiments, but the invention is not limited to the above detailed methods, i.e., it does not mean that the invention must rely on the above detailed methods to be implemented. Those skilled in the art should understand that any improvements to this invention, equivalent substitutions of raw materials for the product of this invention, additions of auxiliary components, and selection of specific methods all fall within the protection and disclosure scope of this invention.
Claims
1. A method for preparing a tin-based perovskite single-crystal luminescent material, characterized in that, The tin-based perovskite single-crystal luminescent materials include divalent tin-based perovskite single-crystal luminescent materials and tetravalent tin-based perovskite single-crystal luminescent materials. The preparation method of the divalent tin-based perovskite single-crystal luminescent material is as follows: a mixed solution is obtained by mixing divalent tin oxide or halide, hypophosphite, hydrobromic acid, and an amine organic ligand; the mixed solution is heated at 90-120°C under an inert gas atmosphere until it becomes clear; the clear reaction solution is allowed to stand and crystallize to obtain the divalent tin-based perovskite single-crystal luminescent material; wherein the amine organic ligand is a monoprotonated amine with one amino group or a diprotonated amine with two amino groups; The preparation method of the tetravalent tin-based perovskite single-crystal luminescent material is as follows: a mixed solution is obtained by mixing tetravalent tin oxide or halide, a polar aprotic organic solvent and / or hydrobromic acid, and an amine organic ligand; the mixed solution is heated at 90~120℃ under an inert gas atmosphere until it becomes clear; the clear reaction solution is allowed to stand and crystallize to obtain the tetravalent tin-based perovskite single-crystal luminescent material. Wherein, the amine organic ligand is a monoprotic amine with one amino group or a diprotic amine with two amino groups; when the organic ligand is a monoprotic amine, hydrobromic acid is used as the solvent; when the organic ligand is a diprotic amine, a polar aprotic organic solvent is used, and hydrobromic acid is used as the acid reaction reagent.
2. The method for preparing the tin-based perovskite single-crystal luminescent material according to claim 1, characterized in that, The divalent tin oxide or halide is selected from stannous oxide, stannous chloride, or stannous bromide; The tetravalent tin oxide or halide is selected from tin oxide, tin chloride or tin bromide; The monoprotic amine is selected from benzylamine (BZA), phenethylamine (PEA), 3-methylbenzylamine, n-hexylamine, hexamethylenediamine, etc. Any one or more combinations of n-octylamine and octyldiamine; The diprotonated amine is selected from 4-aminobenzylamine (4-ABZA), 4-aminophenylethylamine (4-APEA), 3-aminobenzylamine, Any one or more combinations of 4-(aminomethyl)phenylethylamine.
3. The method for preparing the tin-based perovskite single-crystal luminescent material according to claim 2, characterized in that, The amine organic ligand is selected from diproton amines.
4. The method for preparing the tin-based perovskite single-crystal luminescent material according to claim 2, characterized in that, In the preparation method of divalent tin-based perovskite single crystal luminescent material, the molar ratio of tin oxide or halide to amine organic ligand is in the range of 1-3:1; The molar volume ratio of the tin oxide or halide to the total volume of hypophosphorous acid and hydrobromic acid is 1 mol: 1-10 mL. The volume ratio of hydrobromic acid to hypophosphoric acid is 3:
1.
5. The method for preparing tin-based perovskite single-crystal luminescent material according to claim 2, characterized in that, In the preparation method of the tetravalent tin-based perovskite single crystal luminescent material, the polar aprotic organic solvent is selected from any one or more of dimethyl sulfoxide, N,N-dimethylformamide, tetrahydrofuran, and dichloromethane. The molar ratio of the tin oxide or halide to the amine organic ligand is in the range of 1-3:1; The molar ratio of diprotic amine to hydrogen bromide is 1-3:
1. The two are first reacted in an ice-water bath for 2-3 hours, and then obtained by rotary evaporation. The brominated ammonium salt is then reacted with a mixture of tin oxide or halide, organic solvent, and brominated ammonium salt.
6. The method for preparing tin-based perovskite single-crystal luminescent material according to claim 2, characterized in that, The heating time is 1-2 hours, and the static crystallization condition is to stand at room temperature for 2-48 hours.
7. A tin-based perovskite single-crystal luminescent material, characterized in that, It is prepared by the method described in any one of claims 1 to 6.
8. The application of the tin-based perovskite single-crystal luminescent material according to claim 7 in the preparation of optoelectronic functional devices.
9. A photoelectric functional device, characterized in that, Contains the tin-based perovskite single-crystal luminescent material as described in claim 7.
10. The optoelectronic functional device according to claim 9, characterized in that, This includes solar cells, light-emitting diodes (LEDs), laser diodes, radiation detectors, and scintillators.