A multi-light-center dynamic evolution type cellulose room temperature phosphorescent material, a preparation method and application thereof

By constructing a synergistic effect between the reconstructed oxygen cluster cellulose matrix, arylboronic acid luminescent units, and zinc iodide regulation units, the problem of difficulty in activating multiple luminescent centers in cellulose-based room temperature phosphorescent materials is solved, achieving efficient afterglow output and time-dependent color changes, which are suitable for time-gated encryption and anti-counterfeiting identification.

CN123132008APending Publication Date: 2026-11-20GUANGXI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611580428.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In existing cellulose-based room temperature phosphorescent materials, multiple luminescent centers are difficult to activate and fully utilize effectively. Triplete excitons are easily affected by factors such as molecular motion, oxygen, and moisture, resulting in low phosphorescence quantum yield and lifetime. It is difficult to achieve continuous evolution of multiple luminescent centers and multicolor switching over a wide spectral range, which limits their application in dynamic anti-counterfeiting and high-security information encryption.

Method used

By constructing a reconstructed oxygen cluster cellulose matrix, combined with arylboronic acid luminescent units and zinc iodide regulatory units, a stable cluster confinement environment is formed, improving intersystem crossing efficiency, promoting the activation and temporal evolution of different phosphorescent centers, and realizing the dynamic evolution of multiple luminescent centers.

Benefits of technology

It realizes the competition and temporal evolution of multiple phosphorescent centers in the single phosphorescence decay process of cellulose room temperature phosphorescent materials, producing time-dependent color changes, with efficient afterglow output and dynamic color evolution capabilities, and is suitable for time-gated encryption, anti-counterfeiting identification and dynamic information display.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123132008A_ABST
    Figure CN123132008A_ABST
Patent Text Reader

Abstract

The application discloses a multi-light-center dynamic evolution type cellulose room-temperature phosphorescent material and a preparation method and application thereof, and belongs to the technical field of biomass room-temperature phosphorescent functional materials. The material takes oxygen cluster-containing cellulose obtained by redox reconstruction of microcrystalline cellulose as a matrix, forms a basic phosphorescent center through anchoring of an aryl light-emitting unit, and takes zinc iodide as a key regulation unit. The local light-emitting environment of the cellulose matrix is regulated by adjusting the mass addition ratio of the zinc iodide, so that the activation, competition and time sequence evolution of multiple phosphorescent centers are promoted. The highest phosphorescent quantum yield of the obtained material can reach 19.42%, and the longest afterglow lifetime can reach 1.6263 s. A specific material can present a dynamic afterglow process of orange-red color to white color and then to blue-green color after the excitation light is turned off, and an identifiable color authentication signal can be formed at a specific delay time. The material can be used for time-gated encryption, anti-counterfeiting identification and dynamic information display and other high-security optical applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of biomass room temperature phosphorescent functional materials, specifically relating to a multi-luminescent-center dynamically evolving cellulose room temperature phosphorescent material and its preparation method, as well as the application of this material in time-gated information encryption. Background Technology

[0002] Room-temperature phosphorescent (RTP) materials, due to their ability to generate long-lived afterglow signals even after the excitation light is turned off and to effectively reduce background fluorescence and light scattering interference, have become important optical functional materials for dynamic anti-counterfeiting and information encryption. In recent years, various RTP materials have emerged, including small organic molecules, polymer systems, carbon dots, inorganic phosphors, and organic-inorganic hybrid systems. Among them, cellulose, as a typical natural polymer, is widely available and easily chemically modified. Its abundant oxygen-containing groups can form various luminescent clusters through hydrogen bonding and spatial proximity, providing a potential foundation for constructing multi-phosphorescent biomass room-temperature phosphorescent materials.

[0003] However, due to the intrinsic structure of cellulose, the multiple luminescent centers in existing cellulose-based room-temperature phosphorescent materials are difficult to activate and fully utilize effectively. Firstly, the lack of structural units that effectively promote intersystem crossing results in low triplet exciton generation efficiency. Secondly, triplet excitons are susceptible to non-radiative dissipation due to molecular motion, oxygen, and moisture, making it difficult to improve the phosphorescence quantum yield and lifetime of the material. While existing technologies have achieved color modulation and performance enhancement of cellulose-based room-temperature phosphorescent materials by introducing luminescent groups, constructing rigid networks, or applying external stimuli, this color modulation is mostly manifested as static color display, changes in similar hues, or responses to external stimuli. It is difficult to achieve continuous evolution of multiple luminescent centers and wide-spectrum multicolor switching during a single phosphorescence decay process, limiting the application of such materials in scenarios such as dynamic anti-counterfeiting and high-security information encryption.

[0004] Therefore, there is an urgent need to develop a cellulose room-temperature phosphorescent material that combines high efficiency, long afterglow lifetime, and dynamic evolution capability of multiple luminescent centers, and to form a color authentication signal that can be identified at a specific delay time, thereby meeting the requirements of high-security optical applications such as time-gated encryption and anti-counterfeiting identification. Inspired by the dynamic color changes generated by the synergy of multi-color units in nature, the ideal solution should revolve around stable confinement, efficient excited-state modulation, and multi-center temporal modulation: first, a stable clustered confinement environment should be constructed to suppress the non-radiative dissipation of triplet excitons; then, suitable luminescent units should be introduced to improve intersystem crossing efficiency and enrich phosphorescent centers; and finally, local electronic modulation should be used to promote the activation and temporal evolution of different phosphorescent centers, forming a cellulose phosphorescent system with efficient afterglow output and time-dependent color evolution. This multi-level synergistic design strategy is expected to open up a new technical route for creating next-generation high-performance time-gated anti-counterfeiting encryption polymer materials. Summary of the Invention

[0005] This invention provides a multi-emissivity cellulose room-temperature phosphorescent material, its preparation method, and its time-gated encryption application. The invention aims to construct a cellulose room-temperature phosphorescent material with high efficiency, long afterglow lifetime, and the ability to dynamically evolve multiple emissivity centers by redox reconstruction of cellulose to form an oxygen-containing clustered framework, combined with the synergistic effect of arylboronic acid luminescent unit anchoring and zinc iodide local electronic modulation. This material can generate time-dependent color changes during phosphorescence decay after excitation light is turned off, and form a recognizable color authentication signal at a specific delay time. Therefore, it provides a novel cellulose-based phosphorescent functional material for high-security optical applications such as time-gated encryption, anti-counterfeiting identification, and dynamic information display.

[0006] The above-mentioned objectives of the present invention are achieved through the following technical solutions:

[0007] A multi-luminescent-center dynamically evolving cellulose room-temperature phosphorescent material comprises a reconstructed oxygen cluster cellulose matrix, aryl luminescent units anchored to the reconstructed oxygen cluster cellulose matrix via BO bonds, and a zinc iodide control unit; wherein the zinc iodide control unit contains Zn 2+ Coordinated with oxygen-containing sites in the reconstructed oxygen cluster cellulose matrix, I - The neighboring luminescent clusters generate a local heavy atom effect, which synergistically regulates the local luminescence environment of the aryl luminescent unit. During the single phosphorescence decay process after the material is excited and turned off by 310 nm ultraviolet light, multiple phosphorescent centers compete and evolve over time, exhibiting time-dependent afterglow color changes.

[0008] Furthermore, the reconstructed oxygen cluster cellulose matrix is ​​prepared by selective oxidation of microcrystalline cellulose with sodium periodate and reduction with sodium borohydride, and the aryl luminescent unit is provided by arylboronic acid, which is selected from one of 3-aminophenylboronic acid, 4-biphenylboronic acid, 9-phenanthrolineboronic acid, and 1-pyreneboronic acid.

[0009] Furthermore, the mass addition ratio of zinc iodide is the ratio of the mass of zinc iodide to the mass of the reconstructed oxygen cluster cellulose matrix, and the mass addition ratio is from 1:100 to 50:100.

[0010] Furthermore, when the aryl luminescent unit is provided by 1-pyreneboronic acid, the material exhibits a dynamic afterglow process that changes from orange-red to white and then to blue-green during a single phosphorescence decay process after being turned off by 310 nm ultraviolet light excitation, and forms a white color authentication signal with a delay time of 0.3 s.

[0011] Furthermore, when the arylboronic acid is selected from one of 3-aminophenylboronic acid, 4-biphenylboronic acid, 9-phenanthroboronic acid, and 1-pyreneboronic acid, and the mass ratio of zinc iodide to the reconstructed oxygen cluster cellulose matrix is ​​25:100, the resulting material exhibits a phosphorescence quantum yield of 12.01% to 19.42% and an afterglow lifetime of 0.3729 s to 1.6263 s.

[0012] This invention also provides a method for preparing the aforementioned multi-luminescent-center dynamically evolving cellulose room-temperature phosphorescent material, comprising the following steps:

[0013] S1. Microcrystalline cellulose was sequentially subjected to selective oxidation with sodium periodate and reduction with sodium borohydride, and after dialysis and drying, a reconstructed oxygen cluster cellulose matrix was obtained.

[0014] S2. The reconstructed oxygen cluster cellulose matrix obtained in step S1 is dispersed in water, and arylboronic acid dispersion, zinc iodide, and ammonia are added. The mixture is reacted under heating conditions, allowing the arylboronic acid to be anchored to the reconstructed oxygen cluster cellulose matrix via BO bonds to form aryl luminescent units. Simultaneously, the mass ratio of zinc iodide added to the reaction system is adjusted to control the amount of zinc iodide added. 2+ Coordination and I - The heavy atom effect synergistically regulates the local luminescence environment of the reconstructed oxygen cluster cellulose matrix; after the reaction is completed, the cellulose room temperature phosphorescent material with multiple luminescent centers and dynamic evolution is obtained by drying.

[0015] Further, in step S1, microcrystalline cellulose and sodium periodate are dispersed in deionized water and reacted at 60 °C in the dark for 12 h. After terminating the reaction with ethylene glycol, the mixture is dialyzed. The resulting oxidized cellulose is dispersed in a methanol / water mixed solvent with a methanol volume fraction of 80% to form a 5 wt% dispersion. Sodium borohydride is added at 50 °C and reacted for 2 h. The mixture is then dialyzed and freeze-dried to obtain the reconstructed oxygen cluster cellulose matrix.

[0016] Furthermore, in step S2, the mass ratio of the reconstructed oxygen cluster cellulose matrix, arylboronic acid, and zinc iodide is 100:1:25, the volume ratio of ammonia to deionized water is 1:8, the reaction temperature is 80 ℃, and the reaction time is 10 min.

[0017] This invention also provides the application of the aforementioned multi-luminescent-center dynamically evolving cellulose room-temperature phosphorescent material in time-gated information encryption, anti-counterfeiting identification, or dynamic information display. This includes fabricating the material into a pattern or array, exciting it with 310 nm ultraviolet light, then turning off the light source, and reading a white color authentication signal as valid authentication information after a 0.3 s delay. The correct excitation wavelength, the 0.3 s delay, and the white color authentication signal together constitute the decryption conditions. Initially, the pattern or array exhibits an orange-red afterglow as induction information during the initial stage after the excitation light is turned off. After a 0.3 s delay, a white afterglow authentication signal is presented as valid encryption information. After a further delay, the white authentication signal disappears, entering a failed reading state.

[0018] The dynamic evolution effect of multiple luminescent centers in this invention mainly originates from the synergistic effect between the reconstructed oxygen cluster cellulose matrix, the aryl luminescent unit, and the zinc iodide regulatory unit: the reconstructed oxygen cluster cellulose matrix provides a confined environment for oxygen-containing cluster aggregation, which is beneficial for suppressing the nonradiative dissipation of triplet excitons; the aryl luminescent unit forms the basic phosphorescent center and enriches the luminescent components of the material; zinc iodide, as a key regulatory unit, can be controlled by Zn 2+ Coordination with oxygen-containing sites and I - The heavy atom effect generated by neighboring luminescent clusters promotes intersystem crossing and modulates the temporal evolution of different phosphorescent centers. As a result, the material can produce time-dependent color changes during a single phosphorescence decay process and form a recognizable color authentication signal at a specific delay time, making it suitable for high-security optical applications such as time-gated encryption, anti-counterfeiting identification, and dynamic information display.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) This invention proposes and realizes for the first time the dynamic evolution control of multiple luminescent centers in cellulose room temperature phosphorescent materials. The competition and temporal evolution of multiple phosphorescent centers during the single phosphorescence decay process enable the material to produce color changes in a wide spectral range. This overcomes the problem that the luminescent centers in existing cellulose-based room temperature phosphorescent materials are difficult to be effectively activated and fully utilized, and the color control is mostly limited to static display or similar hue changes.

[0021] (2) This invention innovatively uses zinc iodide as a key regulatory unit, and by adjusting the mass addition ratio of zinc iodide in the reaction system, it achieves effective control of the local luminescence environment of the cellulose matrix. Zinc iodide contains Zn... 2+ It can coordinate with oxygen-containing sites in cellulose, I -This method can generate local heavy atom effects in adjacent luminescent clusters, synergistically promoting intersystem crossing and regulating the activation level and decay behavior of different phosphorescent centers. Unlike color modulation methods that simply change the type of luminescent group or rely on external stimuli, this method has the advantages of a clear modulation path, stable material structure, and strong applicability.

[0022] (3) The cellulose room temperature phosphorescent material obtained by the present invention has both high phosphorescence quantum yield and long afterglow lifetime. After being regulated by zinc iodide, the highest phosphorescence quantum yield of the material can reach 19.42%, and the longest afterglow lifetime can reach 1.6263 s, achieving a balance between efficient afterglow output and visible afterglow continuity.

[0023] (4) The material obtained by this invention can produce a time-dependent dynamic afterglow color evolution. Specifically, after the excitation light is turned off, the material can exhibit a dynamic afterglow process that changes from orange-red to white and then to blue-green, and form a white or near-white authentication signal at a specific delay time. Compared with traditional anti-counterfeiting materials that rely on a single color or static pattern for identification, this invention uses the excitation condition, the delay reading time, and the color authentication signal together as decryption conditions, thereby improving the complexity of information encryption and the ability to prevent copying. Attached Figure Description

[0024] Figure 1 This is a schematic diagram of the preparation process of a multi-luminescent-center evolved cellulose room-temperature phosphorescent material according to the present invention;

[0025] Figure 2 Afterglow images of reconstructed oxygen cellulose materials modified with different arylboronic acids under 310 nm UV excitation and at different delay times after excitation light is turned off;

[0026] Figure 3 Afterglow photographs of cellulose room-temperature phosphorescent materials modified with different arylboronic acids under zinc iodide regulation under 310 nm ultraviolet light excitation and at different delay times after the excitation light is turned off.

[0027] Figure 4 Phosphorescence emission spectra of ReOC-Phe9-ZnI2 materials with different zinc iodide addition ratios under 310 nm excitation and 0.1 s delay conditions;

[0028] Figure 5 This is a schematic diagram illustrating the construction and decryption verification process of a time-gated encryption array. Figure 5 a is a schematic diagram of the composition and key settings of the phosphorescent array. Figure 5 b is a schematic diagram of the afterglow output process of the array under different reading states and delay times;

[0029] Figure 6 Comparison of dynamic afterglow color evolution behavior of cellulose room temperature phosphorescent materials under the action of different regulating salts. Detailed Implementation

[0030] like Figure 1 As shown, this invention uses microcrystalline cellulose as raw material, and obtains a reconstructed oxygen cluster cellulose matrix ReOC through selective oxidation with sodium periodate and reduction with sodium borohydride. Based on this, arylboronic acid and zinc iodide are introduced. The arylboronic acid is anchored to the ReOC matrix via BO bonds to form aryl luminescent units, and the zinc iodide is converted into Zn... 2+ Coordination and I - The heavy atom effect synergistically modulates the local luminescence environment of the material, thereby obtaining a dynamic evolutionary cellulose room-temperature phosphorescent material with multiple luminescent centers. This preparation route, through the introduction of aryl luminescent units combined with zinc iodide modulation, provides a structural basis for the formation and dynamic evolution of multiple luminescent centers in the material.

[0031] Example 1: Preparation of reconstructed oxygen cluster cellulose matrix

[0032] 70 g of microcrystalline cellulose and 184.8 g of sodium periodate were weighed and dispersed in 800 mL of deionized water. The mixture was stirred at 60 °C for 12 h under light-protected conditions to allow selective oxidation of the microcrystalline cellulose. After the reaction was completed, ethylene glycol was added to terminate the oxidation reaction. The resulting oxidized cellulose was then thoroughly dialyzed with deionized water to remove residual salts and small molecule impurities.

[0033] Subsequently, the obtained oxidized cellulose was redispersed in a methanol / water mixed solvent with a methanol volume fraction of 80%, and a 5 wt% oxidized cellulose dispersion was prepared. 200 mL of the dispersion was taken and stirred at 50 °C. 4 g of sodium borohydride was dissolved in 40 mL of water and added to the dispersion in four equal portions, 30 min apart, for a total reaction time of 2 h. A reflux condenser was used during the reduction reaction to reduce methanol loss and ensure the safe escape of the generated gases. After the reaction, the reaction solution was placed in a dialysis bag with a molecular weight cutoff of 8000-14000 Da and dialyzed with water until residual methanol and small molecule impurities were removed. After freeze-drying, the reconstituted oxygenated cellulose matrix was obtained, denoted as ReOC.

[0034] Example 2: Preparation of ReOC-3Am-ZnI2 phosphorescent material

[0035] 100 mg of ReOC obtained in Example 1 was weighed and dispersed in 1.6 mL of deionized water to obtain a ReOC dispersion. 1 mg of 3-aminophenylboronic acid was weighed and dispersed in 1 mL of an ethanol / water mixture, and then added to the above ReOC dispersion. Subsequently, 25 mg of zinc iodide and 0.2 mL of ammonia were added, and the mixture was stirred at 80 °C for 10 min. During this reaction, 3-aminophenylboronic acid was anchored to the ReOC matrix via BO bonds, forming the basic ReOC-3Am luminescent structure; simultaneously, zinc iodide participated in the regulation of the local luminescence environment in the reaction system, further modulating the activation degree and evolution behavior of the phosphorescent centers. After the reaction, the resulting system was freeze-dried to obtain a zinc iodide-regulated cellulose room-temperature phosphorescent material, denoted as ReOC-3Am-ZnI2.

[0036] Example 3: Preparation of ReOC-4Bp-ZnI2 phosphorescent material

[0037] 100 mg of ReOC obtained in Example 1 was weighed and dispersed in 1.6 mL of deionized water to obtain a ReOC dispersion. 1 mg of 4-biphenylboronic acid was weighed and dispersed in 1 mL of an ethanol / water mixture, and then added to the above ReOC dispersion. Subsequently, 25 mg of zinc iodide and 0.2 mL of ammonia were added, and the mixture was stirred at 80 °C for 10 min. During this reaction, 4-biphenylboronic acid was anchored to the ReOC matrix through BO bonds, forming the basic ReOC-4Bp luminescent structure; simultaneously, zinc iodide participated in the regulation of the local luminescence environment in the reaction system, further modulating the activation degree and evolution behavior of the phosphorescent centers. After the reaction, the resulting system was freeze-dried to obtain a zinc iodide-regulated cellulose room-temperature phosphorescent material, denoted as ReOC-4Bp-ZnI2.

[0038] Example 4: Preparation of ReOC-Phe9-ZnI2 phosphorescent material

[0039] 100 mg of ReOC obtained in Example 1 was weighed and dispersed in 1.6 mL of deionized water to obtain a ReOC dispersion. 1 mg of 9-phenanthroline was weighed and dispersed in 1 mL of an ethanol / water mixture, and then added to the above ReOC dispersion. Subsequently, 25 mg of zinc iodide and 0.2 mL of ammonia were added, and the mixture was stirred at 80 °C for 10 min. During this reaction, 9-phenanthroline was anchored to the ReOC matrix via BO bonds, forming the ReOC-Phe9 basic luminescent structure; simultaneously, zinc iodide participated in the regulation of the local luminescence environment in the reaction system, further modulating the activation degree and evolution behavior of the phosphorescent centers. After the reaction, the resulting system was freeze-dried to obtain a zinc iodide-regulated cellulose room-temperature phosphorescent material, denoted as ReOC-Phe9-ZnI2.

[0040] Example 5: Preparation of ReOC-1Py-ZnI2 phosphorescent material

[0041] 100 mg of ReOC obtained in Example 1 was weighed and dispersed in 1.6 mL of deionized water to obtain a ReOC dispersion. 1 mg of 1-pyreneboronic acid was weighed and dispersed in 1 mL of an ethanol / water mixture, and then added to the above ReOC dispersion. Subsequently, 25 mg of zinc iodide and 0.2 mL of ammonia were added, and the mixture was stirred at 80 °C for 10 min. During this reaction, 1-pyreneboronic acid was anchored to the ReOC matrix via BO bonds, forming the ReOC-1Py basic luminescent structure; simultaneously, zinc iodide participated in the regulation of the local luminescence environment in the reaction system, further modulating the activation degree and evolution behavior of the phosphorescent centers. After the reaction, the resulting system was freeze-dried to obtain a zinc iodide-regulated cellulose room-temperature phosphorescent material, denoted as ReOC-1Py-ZnI2.

[0042] Example 6: Experiment on the control of the mass addition ratio of zinc iodide

[0043] To investigate the regulatory effect of zinc iodide on the local luminescence environment and multi-luminescence center evolution behavior of cellulose room-temperature phosphorescent materials, the ReOC-Phe9-ZnI2 system described in Example 4 was used as a representative example. The amounts of ReOC, arylboronic acid, ammonia, reaction temperature, and reaction time were kept constant, and only the mass of zinc iodide was varied to prepare cellulose room-temperature phosphorescent materials with different zinc iodide mass addition ratios. The zinc iodide mass addition ratio is the ratio of the mass of zinc iodide to the mass of ReOC.

[0044] The results showed that the phosphorescence emission intensity of the material changed significantly with the change in the proportion of zinc iodide added, such as... Figure 4 As shown, under the conditions of 310 nm excitation and 0.1 s delay, the phosphorescence emission peaks of all samples were located in the range of 500-530 nm, but the luminescence intensity showed a clear "first increase and then decrease" trend: when the zinc iodide mass addition ratio increased from 1:100 to 25:100, the phosphorescence emission intensity gradually increased, with the 25:100 sample exhibiting the highest phosphorescence emission intensity, followed by the 10:100 sample; when the addition ratio was further increased to 40:100 and 50:100, the phosphorescence emission intensity decreased instead, with the luminescence intensity of the 50:100 sample being lower than that of the 10:100 sample, approaching the level of the samples with lower addition ratios. Therefore, the 25:100 sample exhibited the best phosphorescence emission performance.

[0045] The above results indicate that when the zinc iodide addition is too low (e.g., 1:100, 5:100), Zn 2+ Coordination and I -The heavy atom effect has insufficient control over the local luminescence environment, resulting in limited activation of multiple phosphorescent centers and insignificant phosphorescence enhancement. When the zinc iodide content is too high (e.g., 40:100, 50:100), excessive I⁻ may introduce excessively strong heavy atom perturbations and additional non-radiative dissipation, leading to a decrease in phosphorescence performance. Under the conditions of this embodiment, when the zinc iodide mass addition ratio is 25:100, the material exhibits superior phosphorescence output, indicating that an appropriate amount of zinc iodide can effectively promote the activation and regulation of multiple phosphorescent centers while avoiding performance loss caused by excessive heavy atom perturbations.

[0046] Example 7: Optical Performance Testing of Cellulose Room Temperature Phosphorescent Materials

[0047] Phosphorescence spectroscopy, phosphorescence quantum yield, and afterglow lifetime of the materials obtained in Examples 2 to 5 were tested using steady-state / transient fluorescence spectroscopy. The test results showed that the prepared ReOC-3Am-ZnI2, ReOC-4Bp-ZnI2, ReOC-Phe9-ZnI2, and ReOC-1Py-ZnI2 all exhibited obvious visible afterglow emission and showed different afterglow colors and attenuation characteristics.

[0048] like Figure 2 As shown, the ReOC afterglow signal of unanchored arylboronic acid is weak and decays rapidly, with a phosphorescence quantum yield of only 3.39%. After introducing 3-aminophenylboronic acid, 4-biphenylboronic acid, 9-phenanthrolineboronic acid, and 1-pyreneboronic acid, the phosphorescence quantum yields of the corresponding materials increased to 5.58%, 6.03%, 6.38%, and 7.88%, respectively, while producing significantly different afterglow colors. These results indicate that arylboronic acid anchoring can introduce new luminescent components and form basic phosphorescent centers in the reconstructed oxygen cluster cellulose matrix, providing a structural basis for further regulation of afterglow performance.

[0049] Based on this, after introducing zinc iodide, such as Figure 3 As shown, the afterglow emission of each system was further enhanced, and their luminous efficiency and decay behavior changed significantly. The phosphorescence quantum yields of ReOC-3Am-Zn2, ReOC-4Bp-ZnI2, ReOC-Phe9-ZnI2, and ReOC-1Py-ZnI2 were 19.42%, 16.68%, 12.01%, and 13.25%, respectively, with corresponding afterglow lifetimes of 0.6899 s, 0.8279 s, 1.6263 s, and 0.3729 s. Among them, ReOC-Phe9-ZnI2 showed the most significant changes in afterglow emission. Figure 3Visible afterglow lasting up to approximately 16 s can still be observed in the time-series afterglow photographs. Compared to the corresponding arylboronic acid system without zinc iodide, the phosphorescence quantum yield of all four materials was further improved, indicating that zinc iodide can further modulate the local luminescence environment and enhance phosphorescence output based on the existing basic phosphorescent centers. These results collectively demonstrate that arylboronic acid anchoring and zinc iodide regulation play respective roles in the formation of basic luminescent centers and the regulation of subsequent luminescence properties during material construction, thereby obtaining cellulose room-temperature phosphorescent materials with both high phosphorescence quantum yield and long-lived afterglow characteristics.

[0050] Example 8: Dynamic Evolution Performance Test of Multiple Emitting Centers

[0051] The afterglow color evolution behavior of the ReOC-1Py-ZnI2 material obtained in Example 5 was analyzed using time-resolved delayed emission spectroscopy and CIE color coordinates. During testing, the sample was excited with ultraviolet light, and after the excitation source was turned off, the afterglow spectrum and color changes of the material were recorded at different delay times.

[0052] like Figure 3 As shown, the ReOC-1Py-ZnI2 material obtained in Example 5 exhibits a significant time-dependent color evolution during a single phosphorescence decay process. Approximately 0.1 s after the excitation light is turned off, the material displays an orange-red afterglow. As the delay time increases, the decay rates of different phosphorescent centers differ, and their relative luminescence contributions change accordingly. The material forms a white afterglow signal at approximately 0.3 s, gradually transitioning to blue-green within the range of 0.3-1 s. With further delay, the afterglow further turns to dark green or blue-green and gradually decays. This forms a continuous dynamic afterglow color evolution from orange-red, white to blue-green, where the white signal appearing around 0.3 s can be used as a color authentication signal at a specific delay time.

[0053] This dynamic afterglow process demonstrates that the multiple phosphorescent centers in the material of this invention do not simply coexist statically, but rather exhibit different decay behaviors during phosphorescence decay. They compete and undergo temporal evolution through changes in the relative contributions of each luminescent center, thereby achieving time-dependent afterglow color changes and providing an optical signal basis for subsequent time-gated color authentication and information encryption.

[0054] Example 9: Time-gated encryption application

[0055] Cellulose room-temperature phosphorescent materials with different afterglow colors and different decay behaviors obtained in Examples 2 to 5 were distributed on the surface of a substrate in a predetermined pattern or array to form a phosphorescent array for time-gated encryption. The array was irradiated with 310 nm ultraviolet light and then the excitation source was turned off, and the change in the afterglow color of the array was observed at different delay times.

[0056] like Figure 5As shown, this invention achieves time-gated encryption and authentication by constructing a 3×3 room-temperature phosphorescent array and setting multiple decryption conditions. Among these, Figure 5 a demonstrates the composition of the phosphorescent array and the key settings, and uses the excitation wavelength, readout state, delay time, and center color as decryption conditions; Figure 5 Demonstrates the afterglow output process of the array under different reading states and delay times. Under ultraviolet light illumination, the array mainly exhibits fluorescence output, which cannot be used as valid authentication information. In the initial stage after the excitation light is turned off, a specific area shows an orange-red afterglow, which can be used as induction information. After a delay of approximately 0.3 seconds, a white or near-white afterglow authentication signal appears in a specific area, at which point valid encrypted information can be read. After a further delay, the white or near-white authentication signal disappears, and the array enters a failed reading state. Therefore, the correct excitation wavelength, the correct delay time, and the specific color authentication signal can be used together as decryption conditions to construct a time-gated logic encryption system, improving the security of anti-counterfeiting identification and information encryption.

[0057] Example 10: Controlled verification experiment on the synergistic regulatory effect of zinc iodide

[0058] To verify the Zn in the zinc iodide regulation unit 2+ Coordination and I - The synergistic regulatory effect of heavy atoms on the dynamic evolution behavior of multiple luminescent centers was investigated by using different metal salts and halide salts as control regulatory units to examine their influence on the afterglow color evolution behavior of the ReOC-1Py system.

[0059] Specifically, using the ReOC-1Py-ZnI2 material obtained in Example 5 as a reference, control materials were prepared by replacing ZnI2 with ZnCl2, ZnBr2, KI, NaI, and MgCl2, respectively, and designated as ReOC-1Py-ZnCl2, ReOC-1Py-ZnBr2, ReOC-1Py-KI, ReOC-1Py-NaI, and ReOC-1Py-MgCl2. Except for the different types of control salts, the preparation process and reaction conditions of each control material were consistent with those in Example 5, including the amount of ReOC, the amount of 1-pyreneboronic acid, the solvent composition, the amount of ammonia added, the reaction temperature, and the reaction time.

[0060] The afterglow color of the above control materials was observed under the same test conditions. The samples were excited with 310 nm ultraviolet light, and after the excitation source was turned off, the afterglow color changes of the materials were recorded at different delay times. Figure 6 As shown, the results indicate that different salt systems significantly affect the afterglow color evolution behavior of the material. Unlike the ZnI2-controlled system, which can achieve continuous-time evolution of orange-red, white, and blue-green afterglow, the system only requires the introduction of Zn... 2+The ReOC-1Py-ZnCl2 system, the ReOC-1Py-ZnBr2 system, and the system with only I - While the ReOC-1Py-KI and ReOC-1Py-NaI systems can both regulate the afterglow of materials to some extent, their color change degree and time-dependent evolution characteristics are relatively weak, failing to exhibit the same complete color evolution process as the ZnI2-regulated system. Furthermore, the ReOC-1Py-MgCl2 system, lacking Zn... 2+ Coordination and I - The heavy atom effect is mainly manifested in the gradual decay of the red afterglow color, without a significant time-dependent color transition. This comparative result further demonstrates that Zn... 2+ Coordination and I - The synergistic regulation of heavy atom effects plays an important role in constructing the dynamic evolution behavior of multiple luminescent centers.

[0061] The above results indicate that Zn in the zinc iodide regulatory unit 2+ Coordination and I - The heavy atom effect generated by the neighboring luminescent clusters does not act independently, but rather coordinates and regulates the local luminescence environment to achieve changes in the competition and relative contribution of multiple phosphorescent centers during the afterglow decay process, thereby endowing the material with time-dependent color evolution characteristics.

Claims

1. A multi-luminescent-center dynamically evolving cellulose room-temperature phosphorescent material, characterized in that, It is composed of a reconstructed oxygen cluster cellulose matrix, aryl luminescent units anchored to the reconstructed oxygen cluster cellulose matrix via BO bonds, and a zinc iodide regulating unit; in the zinc iodide regulating unit, Zn 2+ Coordinated with oxygen-containing sites in the reconstructed oxygen cluster cellulose matrix, I - The neighboring luminescent clusters generate a local heavy atom effect, which synergistically regulates the local luminescence environment of the aryl luminescent unit. During the single phosphorescence decay process after the material is excited and turned off by 310 nm ultraviolet light, multiple phosphorescent centers compete and evolve over time, exhibiting time-dependent afterglow color changes.

2. The multi-luminescent-center dynamically evolving cellulose room-temperature phosphorescent material according to claim 1, characterized in that, The reconstructed oxygen cluster cellulose matrix is ​​prepared by selective oxidation of microcrystalline cellulose with sodium periodate and reduction with sodium borohydride. The aryl luminescent unit is provided by arylboronic acid, which is selected from 3-aminophenylboronic acid, 4-biphenylboronic acid, 9-phenanthroboronic acid, and 1-pyreneboronic acid.

3. The multi-luminescent-center dynamically evolving cellulose room-temperature phosphorescent material according to claim 1, characterized in that, The zinc iodide addition ratio is the ratio of the mass of zinc iodide to the mass of the reconstructed oxygen cluster cellulose matrix, and the mass addition ratio is from 1:100 to 50:

100.

4. The multi-luminescent-center dynamically evolving cellulose room-temperature phosphorescent material according to claim 2, characterized in that, When the aryl luminescent unit is provided by 1-pyreneboronic acid, the material exhibits a dynamic afterglow process that changes from orange-red to white and then to blue-green during a single phosphorescence decay process after being turned off by 310 nm ultraviolet light excitation, and forms a white color authentication signal with a delay time of 0.3 s.

5. The multi-luminescent-center dynamically evolving cellulose room-temperature phosphorescent material according to claim 2, characterized in that, When the arylboronic acid is selected from one of 3-aminophenylboronic acid, 4-biphenylboronic acid, 9-phenanthroboronic acid, and 1-pyreneboronic acid, and the mass ratio of zinc iodide to the reconstructed oxygen cluster cellulose matrix is ​​25:100, the resulting material exhibits a phosphorescence quantum yield of 12.01% to 19.42% and an afterglow lifetime of 0.3729 s to 1.6263 s.

6. A method for preparing a multi-luminescent-center dynamically evolving cellulose room-temperature phosphorescent material as described in any one of claims 1 to 5, characterized in that, Includes the following steps: S1. Microcrystalline cellulose was sequentially subjected to selective oxidation with sodium periodate and reduction with sodium borohydride, and after dialysis and drying, a reconstructed oxygen cluster cellulose matrix was obtained. S2. The reconstructed oxygen cluster cellulose matrix obtained in step S1 is dispersed in water, and arylboronic acid dispersion, zinc iodide, and ammonia are added. The mixture is reacted under heating conditions, allowing the arylboronic acid to be anchored to the reconstructed oxygen cluster cellulose matrix via BO bonds to form aryl luminescent units. Simultaneously, the mass ratio of zinc iodide added to the reaction system is adjusted to control the amount of zinc iodide added. 2+ Coordination and I - The heavy atom effect synergistically regulates the local luminescence environment of the reconstructed oxygen cluster cellulose matrix; after the reaction is completed, the cellulose room temperature phosphorescent material with multiple luminescent centers and dynamic evolution is obtained by drying.

7. The preparation method according to claim 6, characterized in that, In step S1, microcrystalline cellulose and sodium periodate are dispersed in deionized water and reacted at 60 °C in the dark for 12 h. After terminating the reaction with ethylene glycol, the mixture is dialyzed. The resulting oxidized cellulose is dispersed in a methanol / water mixed solvent with a methanol volume fraction of 80% to form a 5 wt% dispersion. Sodium borohydride is added at 50 °C and reacted for 2 h. The mixture is then dialyzed and freeze-dried to obtain the reconstructed oxygen cluster cellulose matrix.

8. The preparation method according to claim 6, characterized in that, In step S2, the mass ratio of reconstructed oxygen cellulose matrix, arylboronic acid and zinc iodide is 100:1:25, the volume ratio of ammonia water to deionized water is 1:8, the reaction temperature is 80℃, and the reaction time is 10 min.

9. The application of the multi-luminescent-center dynamically evolving cellulose room-temperature phosphorescent material according to any one of claims 1 to 5 in time-gated information encryption, anti-counterfeiting identification, or dynamic information display, characterized in that, The material is made into a pattern or array, excited with 310 nm ultraviolet light and then the light source is turned off. The white color authentication signal is read as valid authentication information after a delay of 0.3 s. The correct excitation wavelength, the 0.3 s delay reading time and the white color authentication signal together constitute the decryption conditions.

10. The application according to claim 9, characterized in that, In the initial stage after the excitation light is turned off, the pattern or array presents an orange-red afterglow as induction information. After a delay of 0.3 s, a white afterglow authentication signal is presented as valid encryption information. After a further delay, the white authentication signal disappears and the read failure state is entered.