A 1.2 mu m wave band Ho 3+ RbCaF3 doped fluorescent powder and preparation method thereof
By using low-phonon-energy RbCaF₃ fluoride as the Ho³⁺ doping matrix, Ho³⁺-doped RbCaF₃ phosphors were prepared, solving the problem of weak luminescence intensity of rare earth ions in the 1.2 μm band. Stable and efficient 1.2 μm luminescence was achieved, which is suitable for near-infrared fluorescence conversion light sources and laser gain materials, and has good industrialization prospects.
Patent Information
- Application Number
- CN202611095325.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-22
- Publication Date
- 2026-11-20
AI Technical Summary
Existing rare-earth ion-doped materials exhibit weak luminescence intensity in the 1.2 μm band, and the emission peak position and bandwidth are easily affected by the matrix environment, making it difficult to achieve stable and efficient 1.2 μm luminescence.
Low-phonon-energy RbCaF₃ fluoride was used as the luminescent matrix for Ho³⁺. Ho³⁺-doped RbCaF₃ phosphors were prepared by high-temperature sintering to reduce the multiphonon nonradiative relaxation rate of the Ho³⁺ excited state and improve the 1.2 μm luminescence of the ⁵I₆→⁵I₈ transition.
It achieves significant 1.2 μm near-infrared emission under blue light excitation, and is suitable for near-infrared fluorescence conversion light sources, anti-counterfeiting materials and laser gain materials. The process is simple and easy to industrialize.
Smart Images

Figure CN123132011A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of luminescent and laser materials technology, specifically relating to a Ho-type emission spectrum that can effectively cover the 1.2 µm wavelength band. 3+ Doped RbCaF3 phosphor and its preparation method. Background Technology
[0002] Near-infrared luminescent materials have attracted widespread attention in recent years due to their strong tissue penetration, low background interference, and excellent optical response characteristics. Among them, the 1.2 μm band light source has significant application value in biomedical imaging, remote sensing, medical diagnosis and treatment, mid-infrared laser pumping, and precision materials processing. Existing research shows that the 1.2 μm band, located in the biological near-infrared optical window, possesses low scattering and low background characteristics, making it suitable for deep tissue imaging, in vivo cell and tissue imaging, tumor diagnosis and in vivo white blood cell measurement, coronary artery plaque identification, laser therapy, and minimally invasive surgery in biomedical applications. Furthermore, some plastics and resins exhibit high absorption rates in the 1.2 μm band, giving it advantages in transparent polymer welding and precision materials processing. Simultaneously, this band can also serve as a pump source for certain fiber lasers and has potential applications in medicine, astronomy, and atmospheric measurement.
[0003] However, current research on near-infrared luminescent materials mainly focuses on mainstream wavelengths such as 1.0 μm, 1.5 μm, and 2.0 μm, while luminescent material systems for the 1.2 μm wavelength band are still underdeveloped. Transition metal ions (such as Cr...) 3+ While chromium ions and main group ions (such as Bi) can achieve emission in the 1.2 μm band, their emission peak position and bandwidth are easily affected by the matrix environment. The valence state and aggregation state of the luminescent center are sensitive to the preparation conditions, resulting in insufficient spectral controllability and repeatability, making it difficult to obtain stable and efficient 1.2 μm luminescence (Song Z, Tanner PA, Liu Q. Host dependency of boundary between strong and weak crystal field strength of Cr). 3+ luminescence[J]. The Journal of Physical Chemistry Letters, 2024, 15(9): 2319-2324.). Although rare earth ions have a well-defined energy level structure and high luminescence stability, current research in the 1.2 μm band still has shortcomings: Yb 3+ and Nd 3+ The advantage of Pr emission is concentrated in the 1.0-1.1 μm range; 3+The emission is closer to 1.3 μm (Wang W, Xue Y, Dong J, et al. Yb 3+ Sensitization effect to Pr 3+ Originated from 1G4 level broadband near-infrared emission and up-conversion in BaF2crystal[J]. Optical Materials Express, 2023, 13(5):1267-1277.); Tm 3+ and Ho 3+ Emission at 1.2 μm is susceptible to low-level relaxation competition, resulting in a low luminescence branching ratio and weak intensity (Wang Y, Zhang Z, Ma F, et al. Enhanced the quantum efficiency of Tm). 3+ 2 μm laser in crystal through an energy transfer process of 3H5 level[J]. Ceramics International, 2025, 51(1): 716-721.). Therefore, developing a novel luminescent material system capable of achieving efficient and stable emission in the 1.2 μm band and its simple preparation method is of significant research importance and application value. Based on this, the present invention provides a Ho 3+ Doped RbCaF3 near-infrared phosphor and its preparation method. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention provides a 1.2 µm band Ho 3+ RbCaF3 doped phosphor and its preparation method. This method aims to overcome the technical challenge of weak luminescence intensity in the 1.2 µm wavelength band of existing rare earth ion doped materials, and to provide a simple, reproducible preparation technique suitable for large-scale production.
[0005] This invention uses low phonon energy RbCaF3 fluoride as Ho 3+ The luminescent matrix, due to the lower maximum phonon energy of fluoride matrices compared to most oxide matrices, can effectively reduce Ho... 3+ The multiphonon nonradiative relaxation rate of the excited state is reduced. 5 I6 level towards 5 The nonradiative relaxation loss of the I7 level, thereby improving 5 I6→ 5The 1.2 μm emission corresponds to the I8 transition.
[0006] To achieve the above objectives, the present invention adopts the following technical solution: A 1.2 µm band Ho 3+ The nominal chemical formula of RbCaF3 doped phosphor is: RbCa 1-x Ho x F3, where x is Ho 3+ The mole fraction of doped ions, where 0.01 ≤ x ≤ 0.10.
[0007] The above-mentioned Ho 3+ The preparation method of RbCaF3 doped phosphor includes the following steps: (1) According to the nominal chemical formula RbCa 1-x Ho x F3 is prepared by weighing rubidium-containing compounds, calcium-containing compounds, holmium-containing compounds and fluorine-containing compounds as the main raw materials, adding flux, grinding them to make them fine and mixed evenly, and then sieving the mixture. (2) The sieve material obtained in step (1) is placed in an air atmosphere and subjected to high-temperature sintering treatment. After cooling to room temperature, it is taken out, ground to make it fine, and sieved to obtain the RbCa. 1-x Ho x F3 phosphor.
[0008] Preferably, in step (1), the flux is selected from at least one or more of ammonium fluoride and rubidium fluoride, and its total addition amount is 0.5 wt.%-10 wt.% of the total mass of the main raw materials.
[0009] Preferably, in step (1), the rubidium-containing compound is selected from at least one of rubidium fluoride, rubidium carbonate, rubidium nitrate, or rubidium chloride; the calcium-containing compound is selected from at least one of calcium fluoride, calcium carbonate, calcium nitrate, or calcium oxide; the holmium-containing compound is selected from at least one of holmium oxide, holmium fluoride, holmium nitrate, holmium carbonate, or holmium oxalate; and the fluorine-containing compound is selected from one or more of ammonium fluoride, rubidium fluoride, calcium fluoride, or lithium fluoride. When the rubidium-containing compound, calcium-containing compound, or holmium-containing compound is a non-fluoride, the amount of the fluorine-containing compound added should be supplemented to meet the fluorine stoichiometry required for the RbCaF3 matrix.
[0010] More preferably, in step (1), the rubidium-containing compound is selected from rubidium fluoride; the calcium-containing compound is selected from calcium fluoride; the holmium-containing compound is selected from holmium fluoride; and the fluorine-containing compound is selected from rubidium fluoride or calcium fluoride.
[0011] Preferably, in step (1), the grinding and mixing process fully refines and evenly disperses the raw materials. After grinding, the mixture is sieved through a 300-mesh standard sieve, and the mass of the material passing through the sieve accounts for more than 95 wt.% of the total mass of the mixture. Preferably, the grinding time is 20 to 60 minutes.
[0012] Preferably, in step (2), the heating rate of the sintering treatment is 5~20℃ / min, the sintering temperature is 600~900℃, and the holding time is 4~8 hours.
[0013] A Ho prepared by the above method 3+ The application of RbCaF3-doped near-infrared phosphors in 1.2 µm band fluorescence conversion light sources, anti-counterfeiting, optical sensing, or laser gain media is particularly suitable for specific application scenarios that require 1.2 µm band light sources (such as imaging and treatment of deep tissues, processing of special materials, etc.).
[0014] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) This invention uses low phonon energy RbCaF3 fluoride as Ho 3+ The luminescent matrix can reduce Ho 3+ Excited-state multiphonon nonradiative relaxation loss, reducing 5 I6 level towards 5 The nonradiative relaxation loss of the I7 level is beneficial for enhancing... 5 I6→ 5 The 1.2 μm near-infrared emission corresponding to the I8 transition.
[0015] (2) Ho prepared by the present invention 3+ The doped RbCaF3 phosphor has a strong excitation peak near 450 nm, which has good spectral matching with commercial blue LED chips and blue semiconductor laser diode (LD) pump sources.
[0016] (3) Ho prepared by the present invention 3+ Doped RbCaF3 phosphors can produce significant near-infrared emission of 1.2 µm under blue light excitation, and can be used to construct near-infrared fluorescence conversion light sources, near-infrared anti-counterfeiting materials, optical sensing materials, and potential laser gain materials.
[0017] (4) The process route provided by the present invention has the advantages of being simple and easy to implement, requiring no atmosphere protection, and having high product phase purity. The preparation method adopted by the present invention does not require high production equipment, the process operation is simple and has good repeatability, which is conducive to industrial mass production. Attached Figure Description
[0018] Figure 1 RbCa prepared in Example 1 0.99 Ho0.01 A comparison of the X-ray powder diffraction pattern of F3 phosphor with the RbCaF3 standard card (PDF#77-1578).
[0019] Figure 2 Different Ho prepared in Examples 1 to 4 3+ Doping concentration RbCa 1-x Ho x A comparison of the X-ray powder diffraction pattern of F3 phosphor with the RbCaF3 standard card (PDF#77-1578), where x=0.01, 0.02, 0.05, 0.10.
[0020] Figure 3 RbCa prepared in Example 3 0.95 Ho 0.05 The monitoring wavelength of F3 phosphor is the excitation spectrum at 1202 nm.
[0021] Figure 4 RbCa prepared in Examples 1 to 4 1-x Ho x Near-infrared emission spectrum of F3 phosphor under 452 nm excitation. Detailed Implementation
[0022] To better understand the present invention, the following embodiments are provided for further explanation. However, the described embodiments are merely some, not all, of the embodiments of the present invention, and the scope of protection claimed by the present invention is not limited thereto. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0023] Example 1 The phosphor composition (S1) of this embodiment is: nominal chemical composition RbCa 0.99 Ho 0.01 F3. The raw materials selected were rubidium fluoride, calcium fluoride, and holmium fluoride, all with a purity of 99.99%. The main raw materials were weighed according to stoichiometric ratios. 10 wt.% ammonium fluoride was added as a flux to the main raw materials, and the mixture was ground in a mortar for 30 minutes. The mixture was then passed through a 300-mesh sieve, with the residue not exceeding 5 wt.%. The sieved material was then transferred to a dense corundum crucible and sintered at 600℃ for 8 hours at a heating rate of 20℃ / min. Afterward, the mixture was cooled to room temperature in the furnace, and the sample was removed, ground, and passed through a 300-mesh sieve to obtain RbCa. 0.99 Ho 0.01 F3 phosphor.
[0024] The XRD patterns of the phosphors were measured using an Aeris powder X-ray diffractometer (PANalytical Corporation, Netherlands); the excitation and emission spectra of the phosphors were measured using an Edinburgh FLS920 spectrometer.
[0025] like Figure 1 As shown, the RbCa prepared in Example 1 0.99 Ho 0.01 The X-ray powder diffraction peaks of the F3 phosphor matched those of the RbCaF3 standard card (PDF#77-1578). XRD pattern analysis indicated that the obtained sample phase was RbCaF3, belonging to the cubic crystal system, and no obvious diffraction peaks of other phases were observed. Figure 4 As shown, under 452 nm excitation, the RbCa prepared in Example 1 0.99 Ho 0.01 F3 phosphors produce significant near-infrared emission, among which Ho 3+ ion 5 I6→ 5 The main emission peak corresponding to the I8 transition is centered at 1202 nm with a full width at half maximum (FWHM) of 19 nm, indicating that low concentrations of Ho... 3+ The doped sample can achieve near-infrared emission in the 1.2 μm band.
[0026] Example 2 The phosphor composition (S2) in this embodiment is: nominal chemical composition RbCa 0.98 Ho 0.02 F3. The raw materials selected are rubidium carbonate, calcium fluoride, and holmium fluoride with a purity of 99.99%, and are processed according to RbCa... 0.98 Ho 0.02 Ammonium fluoride was added to F3 at the nominal stoichiometric ratio as a supplementary fluorine source to the required fluorine stoichiometry for this chemical formula. Then, an additional 5 wt.% ammonium fluoride was added as a flux, and the mixture was ground in a mortar for 20 minutes. The sample was then passed through a 300-mesh sieve, with a residue not exceeding 5 wt.%. The sieved material was then transferred to a dense corundum crucible and sintered at 800°C for 6 hours at a heating rate of 15°C / min. Afterward, the crucible was cooled to room temperature, the sample was removed, ground, and passed through a 300-mesh sieve to obtain RbCa. 0.98 Ho 0.02 F3 phosphor.
[0027] The XRD patterns of the phosphors were measured using an Aeris powder X-ray diffractometer (PANalytical Corporation, Netherlands); the excitation and emission spectra of the phosphors were measured using an Edinburgh FLS920 spectrometer.
[0028] like Figure 2 As shown, the RbCa prepared in Examples 1 to 41-x Ho x The X-ray powder diffraction peaks of the F3 phosphor matched those of the RbCaF3 standard card (PDF#77-1578), and no obvious impurity phase diffraction peaks were observed, indicating that the peaks at x=0.01, 0.02, 0.05, and 0.10 were within the range of Ho. 3+ The RbCaF3 main phase structure can be obtained within the doping range. For example... Figure 4 As shown, the RbCa prepared in Example 2 0.98 Ho 0.02 The F3 phosphor also exhibits Ho under 452 nm excitation. 3+ ion 5 I6→ 5 The I8 characteristic emission has a main emission peak centered at 1204 nm with a half-maximum width of 19 nm. Compared to Example 1, the emission intensity at 1.2 μm of the sample in Example 2 is significantly enhanced, indicating that with the increase of Ho... 3+ Increasing the doping concentration from x=0.01 to x=0.02 increases the number of luminescent centers, which is beneficial for improving the near-infrared emission intensity at 1.2 μm.
[0029] Example 3 The phosphor composition (S3) in this embodiment is: nominal chemical composition RbCa 0.95 Ho 0.05 F3. The raw materials selected were rubidium fluoride, calcium fluoride, and holmium fluoride with a purity of 99.99%. The main raw materials were weighed according to stoichiometric ratios. 0.5 wt.% ammonium fluoride flux was added to the main raw materials, and the mixture was ground in a mortar for 40 minutes. The mixture was then passed through a 300-mesh sieve, with a residue not exceeding 5 wt.%. The sieved material was then transferred to a dense corundum crucible and sintered at 700℃ for 7 hours at a heating rate of 10℃ / min. Afterward, the mixture was cooled to room temperature in the furnace, and the sample was removed, ground, and passed through a 300-mesh sieve to obtain RbCa. 0.95 Ho 0.05 F3 phosphor.
[0030] The XRD patterns of the phosphors were measured using an Aeris powder X-ray diffractometer (PANalytical Corporation, Netherlands); the excitation and emission spectra of the phosphors were measured using an Edinburgh FLS920 spectrometer.
[0031] like Figure 3 As shown, when 1202 nm is used as the monitoring wavelength, the RbCa prepared in Example 3... 0.95 Ho 0.05 The F3 phosphor exhibits multiple Ho values in the 300–700 nm range. 3+Characteristic ion excitation peaks were observed, with significant excitation responses near 452 nm, 538 nm, and 640 nm, indicating that the phosphor can be effectively excited by visible light. In particular, the excitation peak near 452 nm shows good spectral matching with commercial blue LED chips and blue semiconductor laser diode pump sources. Figure 4 As shown, under 452 nm excitation, the sample in Example 3 produced the strongest 1.2 μm near-infrared emission, with its Ho... 3+ ion 5 I6→ 5 The main emission peak corresponding to the I8 transition is centered at 1202 nm with a half-maximum width of 19 nm. The emission intensity at 1.2 μm of this sample is about 3.08 times that of Example 1 and about 1.41 times that of Example 2.
[0032] Example 4 The phosphor composition (S4) of this embodiment is: nominal chemical composition RbCa 0.90 Ho 0.10 F3. The raw materials selected were rubidium fluoride, calcium fluoride, and holmium fluoride with a purity of 99.99%. The raw materials were weighed according to the stoichiometric ratio and ground in a mortar for 60 minutes. The mixture was then passed through a 300-mesh sieve, with a residue not exceeding 5 wt.%. The sieved material was then transferred to a dense corundum crucible and sintered at 900℃ for 4 hours at a heating rate of 5℃ / min. Afterward, the crucible was cooled to room temperature, the sample was removed, ground, and passed through a 300-mesh sieve to obtain RbCa. 0.90 Ho 0.10 F3 phosphor.
[0033] The XRD patterns of the phosphors were measured using an Aeris powder X-ray diffractometer (PANalytical Corporation, Netherlands); the excitation and emission spectra of the phosphors were measured using an Edinburgh FLS920 spectrometer.
[0034] like Figure 4 As shown, the RbCa prepared in Example 4 0.90 Ho 0.10 F3 phosphor can still produce Ho under 452 nm excitation. 3+ ion 5 I6→ 5 The I8 characteristic emission shows a main emission peak centered at 1202 nm with a half-maximum width of 21 nm. Compared to Example 3, the emission intensity at 1.2 μm of the sample in Example 4 is reduced, indicating that when Ho... 3+ When the doping mole fraction is further increased to x=0.10, Ho 3 + Enhanced interional energy migration, cross-relaxation, or concentration quenching leads to a decrease in near-infrared emission intensity at 1.2 μm.
[0035] In summary, the RbCa prepared in Examples 1-4 1-x Ho x F3 phosphors can all produce Ho under 452 nm excitation. 3+ ion 5 I6→ 5 The I8 transition corresponds to near-infrared emission at 1.2 μm, with the main emission peak located in the 1202–1204 nm range and a full width at half maximum (FWHM) of 19–21 nm. With the Ho transition… 3+ As the doping mole fraction increased from x=0.01 to x=0.05, the emission intensity at 1.2 μm gradually increased. This is because, in the lower doping concentration range, increasing the Ho content... 3+ The content can increase the number of effective luminescent centers in the matrix, thereby increasing the probability of absorption of excitation light and 5 An effective layout of the I6 level is beneficial for enhancing... 5 I6→ 5 The 1.2 μm emission corresponds to the I8 transition. When Ho 3+ When the doping mole fraction is further increased to x=0.10, Ho 3+ The shortening of the average distance between ions increases the probability of inter-ion energy migration and cross-relaxation, making it easier for excitation energy to migrate to defects or other non-radiative quenching centers. 5 The decrease in the effective number of particles at the I6 level, coupled with the decrease in emission intensity at 1.2 μm, indicates that x=0.05 is the preferred value in this embodiment of the invention. 3+ Doping molar fraction. In this embodiment of the invention, RbCa 0.95 Ho 0.05 F3 phosphor exhibits the strongest near-infrared emission at 1.2 μm, making it the preferred composition.
[0036] The above embodiments are some implementations of the present invention, but the implementation of the present invention is not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A 1.2 µm band Ho 3+ The RbCaF3 doped phosphor is characterized by: The nominal chemical formula of the phosphor is RbCa. 1-x Ho x F3, where x is Ho 3+ The mole fraction of doped ions, where 0.01 ≤ x ≤ 0.
10.
2. A 1.2 µm band Ho according to claim 1 3+ The RbCaF3 doped phosphor is characterized by: x=0.05。 3. A Ho as described in claim 1 or 2 3+ A method for preparing RbCaF3 doped phosphor, characterized in that: Includes the following steps: (1) According to the nominal chemical formula RbCa 1-x Ho x F3 is prepared by weighing raw materials containing rubidium, calcium, holmium and fluorine in stoichiometric proportions, adding flux, grinding them to make them fine and mixed evenly, and then sieving the mixture. (2) The sieve material obtained in step (1) is placed in an air atmosphere and subjected to high-temperature sintering treatment. After cooling to room temperature, it is taken out, ground, and sieved to obtain the RbCa. 1-x Ho x F3 phosphor.
4. The preparation method according to claim 3, characterized in that: The rubidium-containing compound is selected from one or more of rubidium fluoride, rubidium carbonate, rubidium nitrate, or rubidium chloride; the calcium-containing compound is selected from one or more of calcium fluoride, calcium carbonate, calcium nitrate, or calcium oxide; the holmium-containing compound is selected from one or more of holmium oxide, holmium fluoride, holmium nitrate, holmium carbonate, or holmium oxalate; and the fluorine-containing compound is selected from one or more of ammonium fluoride, rubidium fluoride, calcium fluoride, or lithium fluoride.
5. The preparation method according to claim 3, characterized in that: The rubidium-containing compound is selected from rubidium fluoride; the calcium-containing compound is selected from calcium fluoride; the holmium-containing compound is selected from holmium fluoride; and the fluorine-containing compound is selected from rubidium fluoride or calcium fluoride.
6. The preparation method according to claim 3, characterized in that: In step (1), the flux is selected from one or more of ammonium fluoride and rubidium fluoride.
7. The preparation method according to claim 3, characterized in that: In step (1), the total amount of flux added is 0.5 wt.% to 10 wt.% of the total mass of the main raw materials.
8. The preparation method according to claim 3, characterized in that: In step (1), the grinding and mixing process fully refines and homogenizes the raw materials. After grinding, more than 95 wt.% of the mixture can pass through a 300-mesh standard sieve, and the grinding time is 20 to 60 minutes.
9. The preparation method according to claim 3, characterized in that: In step (2), the heating rate of the sintering treatment is 5~20℃ / min, the sintering temperature is 600~900℃, and the holding time is 4~8 hours.
10. The Ho as claimed in claim 1 3+ Applications of RbCaF3 doped near-infrared phosphors in the preparation of near-infrared fluorescence conversion light sources, anti-counterfeiting, optical sensing, or laser gain media.