A green fluorescent carbon dot-doped silica nano tracer particle and a preparation method thereof

By preparing carbon dot-doped silica nanoparticles, the problems of insufficient fluorescence stability and particle size control in the existing technology have been solved, and high-precision hydrological tracing effect has been achieved, which is suitable for complex heterogeneous media.

CN123132017APending Publication Date: 2026-11-20SHANDONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611360510.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing silica-based fluorescent nanoparticles have shortcomings in terms of the stability of fluorescent functional units and particle size control, making it difficult to meet the tracking requirements of complex heterogeneous media. Furthermore, they have high detection limits and weak anti-interference capabilities.

Method used

Nanoparticle tracers using carbon dots as the fluorescence source and silica as the carrier are prepared via hydrothermal reaction and microemulsion method. The particle size range is controlled to be 20nm~5000nm, and the emitted green light has a wavelength of 515nm, avoiding background fluorescence interference in groundwater.

Benefits of technology

It achieves improved fluorescence signal stability, concentrated particle size distribution, and lower detection limit, making it suitable for hydrological tracing at different pore sizes. It is also environmentally friendly and applicable to complex heterogeneous media.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123132017A_ABST
    Figure CN123132017A_ABST
Patent Text Reader

Abstract

The application provides a kind of green fluorescent carbon dot doped silica nano tracer particle and preparation method, belong to fluorescent nano tracer material technical field.The tracer particle includes silica carrier and carbon dot fluorescent unit embedded in the interior of silica carrier, particle size is 20nm-5000nm, emits green fluorescence with wavelength of 515nm under 450nm wavelength excitation;Preparation method includes: using citric acid and urea as raw material, carbon dot is prepared by hydrothermal reaction;Carbon dot is introduced into silica synthesis reaction in the form of aqueous solution or ethanol solution, carbon dot is involved in the hydrolysis-condensation and deposition process of silica by microemulsion method or sol-gel method, and is obtained by centrifugal separation, washing.The tracer particle provided by the application has stable fluorescent signal, carbon dot is not easy to be released from the carrier, does not contain toxic and harmful components, different particle sizes can be obtained by adjusting the synthesis conditions, and the hydrological tracing demand of different pore scale medium can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of fluorescent nano-tracer materials technology, and in particular to a green fluorescent carbon dot-doped silica nano-tracer particle and its preparation method. Background Technology

[0002] In engineering fields such as hydrogeological exploration, mine water inrush source tracing, and identification of seepage channels in fractured rock masses, tracer experiments are an important technical means to obtain groundwater flow field parameters and determine the connectivity of aquifer media. Traditional solute-based tracers, such as sodium fluorescein and inorganic salt ions, have a long history of application, but their transport processes are significantly affected by molecular diffusion and mechanical dispersion, limiting their accuracy in characterizing dominant underground seepage channels and making it difficult to meet the tracer requirements of complex heterogeneous media. In recent years, the development of nanomaterials technology has provided new ideas for the tracer field. Nanoparticles possess colloidal transport characteristics and can be loaded with fluorescent substances to achieve signal labeling functions. Their particle size and interfacial properties can be adjusted through synthesis conditions, and they are highly sensitive to the pore and fracture structures of the medium, gradually becoming one of the research directions in the field of underground seepage characterization. Among them, silica nanoparticles are chemically stable, biocompatible, and have mature preparation processes, often used as carrier materials to load fluorescent functional components, constituting fluorescent nanoparticles, and are currently one of the most widely studied types of nanoparticle tracer materials.

[0003] However, existing silica-based fluorescent nanoparticles still face several challenges in practical applications: Regarding fluorescent functional units, organic fluorescent dyes are prone to leakage from the silica carrier, and their photostability is insufficient; semiconductor quantum dots contain heavy metals such as cadmium and lead, posing environmental risks and incurring high preparation costs; while carbon dots exhibit good environmental compatibility, their particle size is typically only 2–10 nm, making it difficult to meet the tracer requirements of porous media at different scales. Furthermore, when used directly as tracers, their surface properties are easily affected by groundwater ionic strength and pH, resulting in poor stability during transport. In terms of particle size control, the reverse microemulsion method is generally only suitable for preparing particles with a diameter below 100 nm, while the traditional sol-gel method struggles to stably obtain well-dispersed micron-sized particles. These two methods have different applicable particle size ranges, making it impossible to achieve continuous adjustment from tens of nanometers to several micrometers, thus hindering the flexible selection of appropriate tracer particle sizes based on actual media conditions. In terms of detection performance, most existing products have fluorescence emission wavelengths concentrated in the blue light band, which is prone to overlap with the background fluorescence of substances such as humic substances in groundwater, resulting in weak anti-interference ability in actual use; the detection limit of some materials is high, and the effective signal is weak under large water volume conditions, making on-site monitoring difficult.

[0004] Therefore, providing a nano-tracer particle with carbon dots as fluorescent units and silica as a carrier, and providing a preparation method that can cover a wide particle size range, is of great practical significance for expanding the application scenarios of nano-tracer technology and improving the accuracy of tracer testing. Summary of the Invention

[0005] To overcome the shortcomings of the prior art, the purpose of this invention is to provide a green fluorescent carbon dot-doped silica nanoparticle tracer and its preparation method. The tracer uses carbon dots as the fluorescence source and silica as the carrier. The fluorescence signal is stable, the carbon dots are not easily extracted from the carrier, and it does not contain toxic or harmful components. Particles of different sizes can be obtained according to the changes in synthesis conditions. Moreover, the emission wavelength is located in the green light band, which can effectively avoid the interference of common background fluorescent substances in groundwater. It is suitable for use in hydrological tracer scenarios with different pore sizes.

[0006] To achieve the above objectives, the present invention provides the following solution: On one hand, the present invention provides a green fluorescent carbon dot-doped silica nanoparticle tracer, comprising a silica carrier and carbon dot fluorescent units embedded within the silica carrier; the tracer particles have a particle size of 20 nm to 5000 nm and emit green fluorescence with a wavelength of 515 nm under irradiation with 450 nm wavelength excitation light.

[0007] Preferably, the tracer particles have a narrow, single-peak particle size distribution and a detection limit ≤ 10. -5 g / m 3 .

[0008] On the other hand, the present invention also provides a method for preparing the above-mentioned green fluorescent carbon dot-doped silica nanoparticles, comprising the following steps: S1. Citric acid and urea are added to deionized water at a mass ratio of 1:1, and the solid-liquid mass ratio is 1:10. After stirring until completely dissolved, the mixture is transferred to a hydrothermal reactor and reacted at a constant temperature of 180°C for 2 hours. After natural cooling, the mixture is filtered, centrifuged, purified by dialysis, and concentrated by rotary evaporation to obtain carbon dots. S2. The carbon dots obtained in step S1 are introduced into the silica synthesis reaction in the form of an aqueous solution or an ethanol solution, so that the carbon dots participate in the hydrolysis-condensation and deposition process of silica. After centrifugation and washing, the tracer particles are obtained.

[0009] Preferably, in step S2, the silica synthesis reaction is carried out in a W / O reverse microemulsion, and the carbon dots are introduced into the microemulsion in the form of an aqueous solution; the W / O reverse microemulsion is composed of cyclohexane, Triton X-100 and n-hexanol, with tetraethyl orthosilicate as the silicon source and ammonia as the catalyst, and the concentration of the carbon dot aqueous solution is 0.01 mol / L.

[0010] Preferably, step S2 specifically involves: mixing and stirring cyclohexane, Triton X-100, n-hexanol, and the carbon point aqueous solution to form a transparent and stable W / O microemulsion; then adding the ammonia and the tetraethyl orthosilicate; stirring and reacting at room temperature; adding ethanol to break the emulsion after the reaction is complete; and obtaining the tracer particles by centrifugation and alternating washing with ethanol and water.

[0011] Preferably, in step S2, the amount of the carbon dot aqueous solution is 350~550μL, the amount of tetraethyl orthosilicate is 100~150μL, and the stirring reaction time is 6~18h, to obtain the tracer particles with a particle size of 20~100nm.

[0012] Preferably, in step S2, the sol-gel reaction is carried out in an alcohol-water mixed medium, and the carbon dots are introduced into the alcohol-water mixed medium in the form of an ethanol solution; the sol-gel reaction uses tetraethyl orthosilicate as the silicon source and ammonia as the catalyst, and the concentration of the carbon dot ethanol solution is 0.05 mol / L.

[0013] Preferably, KCl is added as an electrolyte regulator in the alcohol-water mixed medium, and the particle size is gradually increased by continuously adding tetraethyl orthosilicate. The addition rate of tetraethyl orthosilicate is 0.05 mL / min to 0.5 mL / min, resulting in tracer particles with a particle size of 300 nm to 5 μm.

[0014] Preferably, step S2 specifically involves: mixing the carbon dot ethanol solution, deionized water, and ammonia water evenly, adding KCl to fully dissolve and obtain solution A; mixing the tetraethyl orthosilicate with ethanol to obtain solution B; continuously adding solution B to solution A using a micro-injection pump, continuing to stir the reaction after the addition is complete, and obtaining the tracer particles by centrifugation and washing.

[0015] Compared with the prior art, the present invention discloses at least the following technical effects: (1) The carbon dots of the tracer particles provided by this invention are embedded inside silica, which is firmly bound to the carrier and not easily detached from the particles. The fluorescence signal is stable, which can effectively avoid the leakage and photobleaching problems that easily occur in organic fluorescent dyes during use. The emission wavelength of the tracer particles is 515nm, which belongs to the green light band. Compared with tracer materials that emit blue light, green light can effectively avoid the background fluorescence generated by natural organic matter such as humic substances in groundwater in the blue light region, resulting in higher signal recognition and a detection limit of up to 10. -5 g / m 3 .

[0016] (2) By adjusting the synthesis conditions, the present invention can obtain tracer particles of different sizes, covering a particle size range of 20nm~5μm. The particle size distribution of each particle size is concentrated and the monodispersity is good. The appropriate particle size tracer particles can be selected according to the pore structure of different media.

[0017] (3) The hydrostatic diffusion coefficient of the tracer particles provided by the present invention is significantly lower than that of traditional solute tracers. During the transport process, the signal dilution caused by molecular diffusion is not easily caused, which is beneficial to improving the identification accuracy of the dominant flow channel in the tracer experiment. At the same time, the raw materials used in the present invention are citric acid and urea, which do not contain toxic and harmful heavy metal components. The preparation method is simple and has little impact on the ecological environment, making it suitable for use in on-site tracer experiments. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1 The images show the appearance of TNCS tracer particles under natural light and ultraviolet light irradiation, as provided in the embodiments of the present invention.

[0020] Figure 2 Transmission electron microscope (TEM) images of TNCS tracer particles of different sizes provided in embodiments of the present invention; wherein, (a) is a TEM image of 20 nm TNCS, (b) is a TEM image of 50 nm TNCS, (c) is a TEM image of 100 nm TNCS, (d) is a TEM image of 300 nm TNCS, (e) is a TEM image of 500 nm TNCS, (f) is a TEM image of 800 nm TNCS, (g) is a TEM image of 1 μm TNCS, and (h) is a TEM image of 5 μm TNCS.

[0021] Figure 3 The following are nanoparticle size distribution maps of TNCS tracer particles with different particle sizes provided in the embodiments of the present invention; wherein, (a) is the particle size distribution map of 20nm TNCS, (b) is the particle size distribution map of 50nm TNCS, (c) is the particle size distribution map of 100nm TNCS, (d) is the particle size distribution map of 300nm TNCS, (e) is the particle size distribution map of 500nm TNCS, (f) is the particle size distribution map of 800nm ​​TNCS, (g) is the particle size distribution map of 1μm TNCS, and (h) is the particle size distribution map of 5μm TNCS.

[0022] Figure 4The XRD comparison spectra of TNCS tracer particles and pure SiO2 provided in the embodiments of the present invention.

[0023] Figure 5 The Fourier transform infrared spectra of TNCS tracer particles and pure SiO2 are compared in this embodiment of the invention.

[0024] Figure 6 Laser confocal fluorescence microscopy image of TNCS tracer particles provided in an embodiment of the present invention.

[0025] Figure 7 The fluorescence spectra of TNCS tracer particles provided in the embodiments of the present invention are shown in (a) and (b).

[0026] Figure 8 The figures show the still water diffusion test data fitting curves of FLNa, 50nm TNCS and 300nm TNCS provided in the embodiments of the present invention; wherein, (a) is the diffusion fitting curve of FLNa, (b) is the diffusion fitting curve of 50nm TNCS and (c) is the diffusion fitting curve of 300nm TNCS.

[0027] Figure 9 The graph shows the variation of the hydrostatic diffusion coefficient of TNCS tracer particles and comparative materials with different particle sizes provided in the embodiments of the present invention; wherein, (a) is a bar chart of the diffusion coefficient of each material, and (b) is a scatter plot of the diffusion coefficient versus particle size.

[0028] Figure 10 The figure shows the fitting relationship between the particle size of the tracer material and the hydrostatic diffusion coefficient provided in the embodiments of the present invention; wherein, (a) is the fitting curve of the particle material and (b) is the fitting curve of all materials. Detailed Implementation

[0029] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0030] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.

[0031] This invention utilizes carbon dots (CDots) as the fluorescence source and silica as the carrier. Carbon dots are embedded within silica using an encapsulation method to construct green fluorescent carbon dot-doped silica nanoparticles, hereinafter referred to as TNCS tracer particles. The carbon dots are prepared by a hydrothermal reaction of citric acid and urea. The fluorescence emission wavelength of the carbon dots can be controlled by adjusting the ratio of citric acid to urea. Considering that green light emission in hydrological tracing scenarios can effectively avoid background fluorescence interference from natural organic matter such as humic substances in the blue light region, and considering the influence of Stokes shift and emission bandwidth on detection sensitivity and detectability, this invention selects a 1:1 mass ratio of citric acid to urea to prepare the carbon dots.

[0032] Example 1 Weigh 1.0 g of citric acid and 1.0 g of urea, add them to 20 mL of deionized water, and stir magnetically for 30 min until completely dissolved. Sonicate the solution for 10 min at 200 W, 40 kHz, and 30 °C. Transfer the sonicated solution to a hydrothermal reactor, ensuring the solution volume does not exceed 2 / 3 of the reactor's volume. Place the reactor in a forced-air drying oven and react at 180 °C for 2 h. After the reaction, turn off the heating device and allow the reactor to cool naturally to room temperature before removing the reaction solution. Perform preliminary filtration to remove large-sized impurities. Centrifuge the filtrate at 3000 r / min for 2 min to remove larger particles or aggregated products. Place the supernatant after centrifugation in a dialysis bag with a molecular weight cutoff of 300 Da and dialyze in deionized water for 2 days, changing the deionized water every 12 h. After dialysis, remove water from the dialysate by vacuum distillation using a rotary evaporator to obtain concentrated carbon dots.

[0033] Example 2 This embodiment provides a method for preparing TNCS tracer particles with a particle size of 20 nm, including: The CDots obtained in Example 1 were dissolved in deionized water to prepare a 0.01 mol / L aqueous solution of carbon dots. At room temperature, 7.3 mL of cyclohexane, 1.8 mL of Triton X-100, 1.75 mL of n-hexanol, and 350 μL of the aqueous solution of carbon dots were stirred at 800 rpm for 30 min to form a transparent and stable W / O microemulsion. Then, 100 μL of ammonia and 100 μL of tetraethyl orthosilicate were added, and the reaction was continued at room temperature for 6 h. After the reaction was complete, ethanol was added to break the emulsion, and the precipitate was collected by centrifugation at 10000 rpm for 10 min. The precipitate was washed three times alternately with ethanol and deionized water to obtain TNCS tracer particles.

[0034] Example 3 This embodiment provides a method for preparing TNCS tracer particles with a particle size of 50 nm, including: The CDots obtained in Example 1 were dissolved in deionized water to prepare a 0.01 mol / L carbon dot aqueous solution. At room temperature, 7.3 mL of cyclohexane, 1.8 mL of Triton X-100, 1.75 mL of n-hexanol, and 350 μL of the carbon dot aqueous solution were stirred at 800 rpm for 30 min to form a transparent and stable W / O microemulsion. Then, 100 μL of ammonia and 100 μL of tetraethyl orthosilicate were added, and the reaction was continued at room temperature for 18 h. After the reaction was complete, ethanol was added to break the emulsion, and the precipitate was collected by centrifugation at 10000 rpm for 10 min. The precipitate was washed three times alternately with ethanol and deionized water to obtain TNCS tracer particles.

[0035] Example 4 This embodiment provides a method for preparing TNCS tracer particles with a particle size of 100 nm, including: The CDots obtained in Example 1 were dissolved in deionized water to prepare a 0.01 mol / L aqueous solution of carbon dots. At room temperature, 7.3 mL of cyclohexane, 1.8 mL of Triton X-100, 1.75 mL of n-hexanol, and 550 μL of the aqueous solution of carbon dots were stirred at 800 rpm for 30 min to form a transparent and stable W / O microemulsion. Then, 100 μL of ammonia and 150 μL of tetraethyl orthosilicate were added, and the reaction was continued at room temperature for 18 h. After the reaction was complete, ethanol was added to break the emulsion, and the precipitate was collected by centrifugation at 10000 rpm for 10 min. The precipitate was washed three times alternately with ethanol and deionized water to obtain TNCS tracer particles.

[0036] Example 5 This embodiment provides a method for preparing TNCS tracer particles with a particle size of 300 nm, including: The CDots obtained in Example 1 were dissolved in ethanol to prepare a carbon dot ethanol solution with a concentration of 0.05 mol / L. At room temperature, 6.0 mL of this carbon dot ethanol solution, 1.2 mL of deionized water, and 2.8 mL of ammonia were mixed and stirred until homogeneous. Then, 0.8 mL of tetraethyl orthosilicate was added in one batch, and the reaction was continued with stirring for 18 h. After the reaction was completed, the precipitate was collected by centrifugation at 8000 r / min for 10 min, and washed three times alternately with ethanol and deionized water to obtain TNCS tracer particles.

[0037] Example 6 This embodiment provides a method for preparing TNCS tracer particles with a particle size of 500 nm, including: The CDots obtained in Example 1 were dissolved in ethanol to prepare a carbon dot ethanol solution with a concentration of 0.05 mol / L. At room temperature, 6.0 mL of this carbon dot ethanol solution, 1.2 mL of deionized water, and 1.6 mL of ammonia water were mixed and stirred until homogeneous. Then, 0.8 mL of tetraethyl orthosilicate was added at once, and the reaction was continued with stirring for 18 h. After the reaction was completed, the precipitate was collected by centrifugation at 8000 r / min for 10 min, and washed three times alternately with ethanol and deionized water to obtain TNCS tracer particles.

[0038] Example 7 This embodiment provides a method for preparing TNCS tracer particles with a particle size of 800 nm, including: The CDots obtained in Example 1 were dissolved in ethanol to prepare a carbon dot ethanol solution with a concentration of 0.05 mol / L. 50 mL of this carbon dot ethanol solution, 7.8 mL of deionized water, and 6.0 mL of ammonia were mixed thoroughly, and 2.0 mg of KCl was added and dissolved completely to obtain solution A. 4.0 mL of tetraethyl orthosilicate was mixed with 30 mL of ethanol to obtain solution B. Solution B was continuously added to solution A at a rate of 0.5 mL / min using a micro-injection pump. After the addition was complete, the reaction was stirred for 16 h. After the reaction was completed, the precipitate was collected by centrifugation at 6000 r / min for 10 min and washed three times alternately with ethanol and deionized water to obtain TNCS tracer particles.

[0039] Example 8 This embodiment provides a method for preparing TNCS tracer particles with a particle size of 1 μm, including: The CDots obtained in Example 1 were dissolved in ethanol to prepare a carbon dot ethanol solution with a concentration of 0.05 mol / L. 50 mL of this carbon dot ethanol solution, 7.8 mL of deionized water, and 6.0 mL of ammonia were mixed thoroughly, and 2.0 mg of KCl was added and dissolved completely to obtain solution A. 4.0 mL of tetraethyl orthosilicate was mixed with 30 mL of ethanol to obtain solution B. Solution B was continuously added to solution A at a rate of 0.2 mL / min using a micro-injection pump. After the addition was complete, the reaction was stirred for 16 h. After the reaction was completed, the precipitate was collected by centrifugation at 6000 r / min for 10 min and washed three times alternately with ethanol and deionized water to obtain TNCS tracer particles.

[0040] Example 9 This embodiment provides a method for preparing TNCS tracer particles with a particle size of 5 μm, including: The CDots obtained in Example 1 were dissolved in ethanol to prepare a 0.05 mol / L carbon dot ethanol solution. 50 mL of this carbon dot ethanol solution, 5.8 mL of deionized water, and 4.0 mL of ammonia were mixed thoroughly, and 12.5 mg of KCl was added and dissolved completely to obtain solution A. 6.0 mL of tetraethyl orthosilicate was mixed with 30 mL of ethanol to obtain solution B. Solution B was continuously added to solution A at a rate of 0.05 mL / min using a micro-injection pump. After the addition was complete, the reaction was stirred for 6 hours. After the reaction was completed, the precipitate was collected by centrifugation at 6000 r / min for 10 min and washed three times alternately with ethanol and deionized water to obtain TNCS tracer particles.

[0041] Based on the above embodiments, the TNCS tracer particles obtained in Examples 2-9 were dispersed in deionized water, dropped onto a copper mesh support film, and naturally dried before their morphology was observed using a transmission electron microscope. Figure 2 As shown in (a) to (h), the TNCS tracer particles of all sizes are regular spherical with clear boundaries and concentrated particle size distribution. Some degree of local contact or slight aggregation can be observed in small-sized samples, but the particle sphericity is high and no obvious satellite particle attachment is observed; the submicron to micron-sized samples are uniform in size and have good dispersion.

[0042] The particle size distribution of TNCS tracer particles of various sizes prepared in Examples 2-9 was determined using a dynamic light scattering nanoparticle size analyzer. Figure 3 As shown in (a) to (h), the volume distribution histograms of particles of each size all show a single-peak distribution, and the cumulative distribution curve rises steeply and has a narrow range, indicating that the particle size distribution of each sample is concentrated and has good monodispersity.

[0043] The TNCS tracer particles prepared in Examples 2-9 were observed under natural light and ultraviolet light. Figure 1 As shown, TNCS appears white with a slight yellow tinge under natural light and shows no obvious flocculation or sedimentation when dispersed in water; under ultraviolet light, all samples emit clear green fluorescence, indicating that the carbon dots are embedded in the silica particles.

[0044] Then, using Example 3 as a sample example, 50nm TNCS tracer particles and pure SiO2 samples prepared in Example 3 were analyzed using X-ray diffraction, with a test range of 10°~60° (2θ) and a scanning speed of 10° / min. Figure 4 As shown, pure SiO2 exhibits a typical broad, diffuse peak at 20–23°, indicating its amorphous SiO2 structure. The TNCS sample also shows this broad peak, and no new clear crystalline phase diffraction peaks appear, indicating that the overall structure after compositing still maintains the amorphous SiO2 structure. Compared with pure SiO2, the broad peak position of TNCS is slightly shifted to the right, and the peak shape is slightly expanded.

[0045] The functional groups of TNCS and pure SiO2 were compared and analyzed using Fourier transform infrared spectroscopy, with a scanning range of 4000 cm⁻¹. -1 ~500cm -1 4cm resolution -1 .like Figure 5 As shown, both samples exhibit typical absorption characteristics of SiO2: approximately 1070 cm⁻¹. -1 The strong peak at approximately 800 cm⁻¹ belongs to the Si-O-Si asymmetric stretching vibration. -1 The Si-O-Si symmetric stretching vibration at this point indicates that the SiO2 backbone remains unchanged after recombination. Compared with pure SiO2, TNCS exhibits new absorption peaks while retaining the Si-O-Si backbone characteristics: in the range of 3000–2800 cm⁻¹. -1 A CH stretching vibration peak appears in the interval, at approximately 1450 cm⁻¹. -1 A CH2 bending vibration peak appears nearby, at 1500~1700 cm⁻¹. -1 A peak associated with the NH bending vibration, related to nitrogen-containing functional groups, appeared in the range. These newly added absorption peaks confirm that the carbon dots have been successfully embedded in the silica framework.

[0046] Subsequently, the fluorescence performance of the sample prepared in Example 3 was tested. 50 nm TNCS tracer particles obtained in Example 3 were dispersed in deionized water, dropped onto a glass slide, and observed using a laser confocal scanning microscope for bright-field and fluorescence imaging. Figure 6 As shown, the bright-field image shows that the particles are distributed in a near-spherical uniform shape, and the fluorescence image shows that the particles emit green fluorescence. The positions of the emission points are highly coincident with the particle positions in the bright-field image, indicating that the carbon dots are effectively embedded inside the silica.

[0047] The fluorescence spectrum of the 50 nm TNCS tracer particles prepared in Example 3 was scanned using a fluorescence spectrophotometer. Figure 7 As shown in (a), the optimal excitation wavelength for the three-dimensional fluorescence spectrum of TNCS is 450 nm; Figure 7 As shown in (b), the optimal emission wavelength is 515 nm, the Stokes shift is 65 nm, and the full width at half maximum (FWHM) is 72.35 nm. Compared with free carbon dots, the fluorescence main peak is more concentrated and the peak position is more stable after SiO2 coating, and the excitation dependence is reduced.

[0048] The relationship between fluorescence intensity and concentration of TNCS tracer particles was determined using a stepwise dilution method. The 50 nm TNCS tracer particles prepared in Example 3 were stepwise diluted, and their fluorescence intensity was measured. Linear fitting was performed within the instrument's linear response range. The results showed that the fluorescence intensity of the TNCS tracer particles exhibited a good linear relationship with concentration, and the detection limit reached 10. -5 g / m 3 .

[0049] Next, the anti-elution performance of the sample from Example 3 was tested. The 50nm TNCS tracer particles prepared in Example 3 were dispersed in deionized water and subjected to multiple centrifugation and alternating washing with ethanol / water. After each washing, the particles were redispersed in deionized water and the fluorescence was observed under 365nm ultraviolet light. The fluorescence intensity was measured using a fluorescence spectrophotometer. After multiple centrifugation and washing, the particles still emitted clear green fluorescence under ultraviolet light, and the fluorescence intensity did not decrease significantly, indicating that the carbon dots were firmly bound to the silica carrier and were not easily detached from the particles.

[0050] Finally, the static water diffusion coefficient was tested using a static water diffusion coefficient measurement system, which consists of three parts: an excitation source, a spectral acquisition module, and a static water diffusion unit. The static water diffusion unit comprises a solution tank and a clear water tank, connected by a two-way glass tube with a piston. The solution tank holds the solution containing the tracer material, and the clear water tank holds deionized water; the glass tube forms a diffusion channel between the two tanks. The excitation source is a 532nm solid-state laser, introduced to the monitoring point via an optical fiber connected to a fluorescence probe to excite the tracer material to produce fluorescence. The spectral acquisition module consists of an area array spectrometer and matching optical fiber. The fluorescence probe simultaneously receives the fluorescence signal and transmits it through the optical fiber to the area array spectrometer for intensity acquisition, recording the change in fluorescence intensity at the monitoring point over time in real time.

[0051] Before testing, the solution containing the tracer material was injected into the solution tank, and deionized water was injected into the clear water tank. The liquid levels on both sides were adjusted to be consistent to eliminate the convection effect caused by the head difference and ensure that the system was in a static state. The fiber optic fluorescence probe was fixed at a preset monitoring point in the clear water tank at a certain distance from the port of the two-way glass tube. The stopcock of the glass tube was opened to connect the two water bodies, allowing the solute or particles to migrate from the high concentration side to the low concentration side by molecular diffusion. The area array spectrometer was started for time-series monitoring, continuously recording the change curve of the fluorescence signal intensity at the monitoring point over time until the fluorescence intensity tended to stabilize.

[0052] After the test, the obtained fluorescence intensity-time data were processed. Based on the constant concentration boundary diffusion model in a semi-infinite medium using Fick's second law, the concentration changes with time and distance satisfy the following relationship: ; in, For monitoring points Concentration at time, To maintain a constant concentration in the solution tank, The distance from the monitoring point to the diffusion interface. Where is the diffusion coefficient. As a complementary error function, the diffusion coefficient of the tracer material can be obtained by performing nonlinear fitting on the experimentally measured concentration-time data using the above formula.

[0053] Diffusion test data of sodium fluorescein (FLNa), 50 nm TNCS prepared in Example 3, and 300 nm TNCS prepared in Example 5 were selected as examples. All three materials exhibited a rapid growth, gradual slowdown, and eventual stabilization characteristic during hydrostatic diffusion. Figure 8 As shown in (a), FLNa exhibits the fastest fluorescence intensity increase and reaches equilibrium in the shortest time, indicating its strongest diffusion capability; Figure 8 As shown in (b), the diffusion rate of TNCS at 50 nm is significantly reduced, and the time required to reach a stable plateau is prolonged; as Figure 8 As shown in (c), the 300nm TNCS has the lowest diffusion rate and the longest stabilization time.

[0054] The diffusion coefficients of all 10 materials, namely FLNa, carbon dots, and TNCS with different particle sizes prepared in Examples 2-9, were measured. Figure 9 As shown in (a), the diffusion coefficients of different materials differ by a significant order of magnitude; for example... Figure 9 As shown in (b), the diffusion coefficient decreases with increasing particle size. Further nonlinear fitting was performed with particle size as the abscissa and diffusion coefficient as the ordinate. Figure 10 As shown in (a), the diffusion coefficient of particulate materials (20 nm to 5 μm) exhibits an inverse proportional relationship with particle size (D = k / d), and the goodness of fit R0 is [value missing]. 2 Reaching 0.997; such as Figure 10 As shown in (b), after incorporating FLNa and CDots into the global fit, the overall R... 2 It remains above 0.993. Compared with the solute-based tracer FLNa, the diffusion coefficient of TNCS tracer particles is reduced by about 1 to 2 orders of magnitude, indicating that it diffuses slowly in still water and is less prone to signal dilution due to molecular diffusion.

[0055] Therefore, the present invention employs the above-mentioned green fluorescent carbon dot-doped silica nanoparticle tracer and its preparation method. The tracer particle uses carbon dots as the fluorescence source and silica as the carrier. The fluorescence signal is stable, the carbon dots are not easily extracted from the carrier, and it does not contain toxic or harmful components. It can obtain particles of different sizes according to the changes in synthesis conditions, and the emission wavelength is located in the green light band. It can effectively avoid the interference of common background fluorescent substances in groundwater and is suitable for use in hydrological tracer scenarios with different pore sizes.

[0056] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to each other.

[0057] This document uses specific examples to illustrate the principles and implementation methods of the present invention. The descriptions of the above embodiments are only for the purpose of helping to understand the method and core ideas of the present invention. Furthermore, those skilled in the art will recognize that, based on the ideas of the present invention, there will be changes in the specific implementation methods and application scope. Therefore, the content of this specification should not be construed as a limitation of the present invention.

Claims

1. A green fluorescent carbon dot-doped silica nanoparticle tracer, characterized in that, It includes a silica support and carbon dot fluorescent units embedded within the silica support; the tracer particles have a particle size of 20nm~5000nm and emit green fluorescence with a wavelength of 515nm under irradiation with 450nm wavelength excitation light.

2. The green fluorescent carbon dot-doped silica nanoparticle tracer according to claim 1, characterized in that, The tracer particles exhibit a narrow, single-peak particle size distribution, and the detection limit is ≤10. -5 g / m 3 .

3. A method for preparing green fluorescent carbon dot-doped silica nanoparticles as described in any one of claims 1 to 2, characterized in that, Includes the following steps: S1. Citric acid and urea are added to deionized water at a mass ratio of 1:1, and the solid-liquid mass ratio is 1:

10. After stirring until completely dissolved, the mixture is transferred to a hydrothermal reactor and reacted at a constant temperature of 180°C for 2 hours. After natural cooling, the mixture is filtered, centrifuged, purified by dialysis, and concentrated by rotary evaporation to obtain carbon dots. S2. The carbon dots obtained in step S1 are introduced into the silica synthesis reaction in the form of an aqueous solution or an ethanol solution, so that the carbon dots participate in the hydrolysis-condensation and deposition process of silica. After centrifugation and washing, the tracer particles are obtained.

4. The preparation method according to claim 3, characterized in that, In step S2, the silica synthesis reaction is carried out in a W / O reverse microemulsion, and the carbon dots are introduced into the microemulsion in the form of an aqueous solution. The W / O reverse microemulsion is composed of cyclohexane, Triton X-100 and n-hexanol, with tetraethyl orthosilicate as the silicon source and ammonia as the catalyst. The concentration of the aqueous solution of the carbon dots is 0.01 mol / L.

5. The preparation method according to claim 4, characterized in that, Step S2 specifically involves: mixing and stirring cyclohexane, Triton X-100, n-hexanol, and the carbon point aqueous solution to form a transparent and stable W / O microemulsion; then adding ammonia and tetraethyl orthosilicate; stirring and reacting at room temperature; adding ethanol to break the emulsion after the reaction is complete; and obtaining the tracer particles by centrifugation and alternating washing with ethanol and water.

6. The preparation method according to claim 5, characterized in that, In step S2, the amount of the carbon dot aqueous solution is 350-550 μL, the amount of tetraethyl orthosilicate is 100-150 μL, and the stirring reaction time is 6-18 h, to obtain the tracer particles with a particle size of 20-100 nm.

7. The preparation method according to claim 3, characterized in that, In step S2, a sol-gel reaction is carried out in an alcohol-water mixed medium, and the carbon dots are introduced into the alcohol-water mixed medium in the form of an ethanol solution; the sol-gel reaction uses tetraethyl orthosilicate as the silicon source and ammonia as the catalyst, and the concentration of the carbon dot ethanol solution is 0.05 mol / L.

8. The preparation method according to claim 7, characterized in that, KCl was added as an electrolyte regulator to the alcohol-water mixed medium, and the particle size was gradually increased by continuously adding tetraethyl orthosilicate. The addition rate of tetraethyl orthosilicate was 0.05 mL / min to 0.5 mL / min, resulting in tracer particles with a particle size of 300 nm to 5 μm.

9. The preparation method according to claim 7, characterized in that, Step S2 specifically involves: mixing the carbon dot ethanol solution, deionized water, and ammonia water evenly, adding KCl to fully dissolve and obtain solution A; mixing tetraethyl orthosilicate with ethanol to obtain solution B; continuously adding solution B to solution A using a micro-injection pump, continuing to stir the reaction after the addition is complete, and obtaining the tracer particles by centrifugation and washing.