A full inorganic quantum dot light emitting diode based on zinc oxide quantum dot homojunction
By optimizing the homojunction structure of zinc oxide quantum dots and the integrated process, the problems of high interface polarization capacitance and carrier transport imbalance in all-inorganic QLED devices were solved, achieving a green electroluminescence effect with uniformity, high brightness and high stability across the entire domain.
Patent Information
- Application Number
- CN202611315992.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-20
AI Technical Summary
All-inorganic perovskite quantum dot light-emitting diodes (QLEDs) suffer from problems such as high interfacial polarization capacitance, sensitivity to charge carrier transport performance, charge carrier transport imbalance, lack of hole transport materials, difficulty in quantitatively evaluating thin film defects, and unclear control of multilayer quantum dot light-emitting layers, resulting in poor device brightness and uniformity.
A zinc oxide quantum dot homojunction structure was adopted, with core-shell CsPbBr₃@ZnO quantum dots as the light-emitting layer and aminosilane-functionalized ZnO quantum dots as the carrier transport layer. The interface was improved by combining argon plasma treatment, and a fully integrated process system was established, including thin film defect screening, single carrier transport matching and device electrical verification, and the number of stacked light-emitting layers was optimized.
It achieves global uniformity, high brightness and high stability of all-inorganic QLED devices, reduces polarization capacitance, improves interface contact characteristics, accurately matches carrier conduction, broadens the carrier recombination range, and improves luminous uniformity and photoelectric conversion efficiency.
Smart Images

Figure CN123132018A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of quantum dot optoelectronic device technology, specifically relating to an all-inorganic quantum dot light-emitting diode (QLED) based on a zinc oxide quantum dot homojunction. Background Technology
[0002] Perovskite quantum dots (PeQDs) have broad application prospects in displays and solar cells due to their tunable bandgap, high absorption coefficient, high carrier mobility, and solution processability. Based on the material system of each functional layer, QLEDs can be divided into two main categories: organic-inorganic hybrid QLEDs and all-inorganic QLEDs. Studies have shown that commonly used organic materials such as PEDOT:PSS are not only acidic and easily corrode ITO substrates, but also sensitive to water and oxygen, and prone to phase separation under thermal stress, leading to rapid performance degradation. In contrast, all-inorganic QLEDs are constructed entirely of inorganic semiconductor materials, fundamentally avoiding the thermal decomposition and water / oxygen permeation problems of organic components, thus possessing far superior thermal stability and environmental tolerance compared to hybrid systems. However, although the all-inorganic architecture theoretically extends device lifetime, its actual performance is still severely limited by insufficient interface charge injection efficiency and carrier transport imbalance.
[0003] Currently, most mainstream all-inorganic QLEDs employ a heterojunction device structure, where the hole transport layer (HTL), electron transport layer (ETL), and perovskite quantum dot emitting layer (EML) are constructed from different types of inorganic semiconductor materials. This structure suffers from several inherent technical drawbacks. First, high interfacial polarization capacitance easily forms between the heterojunction layers, and the carrier transport performance of the emitting layer is highly sensitive to film thickness. As the film thickness increases, carrier migration and transport capabilities decrease sharply, severely limiting the improvement of the device's photoelectric performance. Simultaneously, while the material systems of each functional layer in the heterojunction are independent, allowing for individual control of photoelectric performance parameters, the interlayer coupling is extremely poor, making it difficult to achieve precise matching of carrier transport rates between the HTL and ETL. Therefore, it cannot fundamentally solve the core problems commonly found in all-inorganic devices, such as charge transport imbalance, high interface defect density, and poor luminous uniformity. Furthermore, the available p-type hole transport materials for all-inorganic QLEDs are extremely limited, particularly lacking high-performance inorganic hole transport materials suitable for CsPbBr3 perovskite quantum dots. Meanwhile, the spin-coating process parameters of the precursor have a significant impact on the thin film performance. Thin films prepared with different spin-coating speeds show significant differences in thickness uniformity, preferred crystal orientation, and oxygen vacancy defect density. Oxygen vacancies, as typical n-type defects, severely negate the p-type conductivity of the thin film, leading to blocked hole injection. However, current research lacks a process screening method that uses the ratio of the intrinsic bandgap emission peak of the PL spectrum to the oxygen vacancy defect peak intensity as a quantitative evaluation of defects. Relying solely on single thin film conductivity tests cannot simultaneously evaluate the film defect level and crystal uniformity. Blindly adjusting spin-coating parameters can easily lead to insufficient hole injection, resulting in devices that only partially illuminate or even fail to emit light at all. On the other hand, current optimization strategies for all-inorganic devices are mostly limited to individually adjusting the performance of HTL or ETL monolayers. A standardized carrier matching characterization process has not been established, and a joint analysis method based on space charge confinement current (SCLC) single carrier JV testing is lacking. This makes it impossible to qualitatively compare the intrinsic transport capabilities of hole and electron thin films and to accurately match the charge conduction rates of the two types of transport layers. When the carrier transport levels of HTL and ETL are unbalanced, a large surplus of individual carriers accumulates at the EML interface. Macroscopically, this manifests as an increase in low-voltage leakage current, a significant rise in the peak capacitance of the CV curve, a substantial increase in non-radiative recombination losses at the interface, and a simultaneous deterioration in device brightness and luminescence uniformity. Therefore, establishing an integrated control method that combines thin-film defect characterization, single-carrier transport testing, and joint verification of the J / CV of a complete device is crucial for achieving efficient charge balance.
[0004] Furthermore, the modulation of multilayer quantum light-emitting layers (EMLs) lacks systematic comparative studies. Existing perovskite thick-film studies have confirmed that multilayer stacking EMLs can broaden the carrier recombination range, dilute the interfacial exciton concentration, and suppress Auger quenching; however, layer stacking also introduces new interlayer interface traps, increasing carrier transport resistance. These two effects compete with each other, jointly determining the ultimate performance limit of the device. However, current research mostly discusses the monolayer light-emitting performance in hybrid or all-inorganic systems in isolation, lacking a systematic comparison of the photoelectric properties and capacitance evolution of quantum dot films in these two systems.
[0005] In summary, while all-inorganic perovskite QLEDs possess stability advantages, they still suffer from three major technical shortcomings: a lack of directional screening methods for defects in the inorganic hole transport layer; no quantitative matching standard between HTL / ETL carrier conduction and film thickness; and unclear modulation mechanisms of multilayer quantum dot emitting layers. These issues make it difficult for all-inorganic devices to simultaneously achieve uniform, high-brightness emission across the entire spectrum. Summary of the Invention
[0006] To address the aforementioned deficiencies in existing technologies, this invention aims to provide an all-inorganic QLED based on a zinc oxide quantum dot homojunction. The core of this approach lies in using core-shell CsPbBr3@ZnO quantum dots as the light-emitting layer and aminosilane-functionalized ZnO quantum dots (denoted as AP-ZnO quantum dots) modified with NaCl doping or ZnS sensitization as the carrier transport layer. Through homojunction structure design and process optimization, the device polarization capacitance is significantly reduced, and interface contact characteristics are improved, ultimately achieving uniform, high-brightness, and highly stable green electroluminescence across the entire device architecture.
[0007] To achieve the above objectives, the present invention adopts the following technical solution: This invention first constructs a process screening and optimization method for all-inorganic quantum dot light-emitting diodes, used to systematically determine the optimal fabrication process parameters and film thicknesses for each functional layer of the device, including the following steps: (1) Screening of hole transport layer film defects: The photoluminescence spectrum of hole transport layer film under different spin coating process conditions was tested. The intensity ratio of intrinsic bandgap emission peak to oxygen vacancy defect peak was used as the evaluation index. The higher the ratio, the lower the proportion of oxygen vacancy defects and the better the p-type conductivity of the film. The spin coating process of hole transport layer with low oxygen vacancy defect ratio and high crystal order was selected as candidate process conditions.
[0008] (2) Matching of single carrier transport capabilities: Single carrier devices with electron transport layer and single carrier devices with hole transport layer were prepared by space charge confinement current method and JV characteristic curves were tested. The intrinsic transport capabilities of holes and electrons were qualitatively compared under the same applied voltage. The matching criterion was that the current density of single carrier device with hole transport layer was similar to that of single carrier device with electron transport layer. The process combination of hole transport layer and electron transport layer with matching carrier conduction level was screened, and the film thickness matching range of hole transport layer and electron transport layer was preliminarily determined.
[0009] (3) Complete device electrical verification: Based on steps (1) and (2), complete QLED devices are prepared with different spin coating process parameters and JV test and CV test are performed respectively. The lowest leakage current in the low voltage range and the lowest peak capacitance of the CV curve are used as the judgment criteria (the peak capacitance of the CV curve is used to quantitatively characterize the total amount of excess carriers accumulated in the multi-layer functional interface of the device. The lower the peak capacitance, the smaller the non-radiative recombination loss of the interface). The optimal spin coating process parameters and film thickness of hole transport layer and electron transport layer are determined comprehensively.
[0010] (4) Optimization of the number of light-emitting layers: Based on the optimal HTL / ETL process parameters determined in step (3), QLED devices with different numbers of light-emitting layers are prepared. Through JVL test and CV test, the optimal number of light-emitting layers is determined by taking the lowest start-up voltage, the highest brightness, and the lowest peak capacitance of the CV curve as the comprehensive judgment criteria, so as to achieve the synergistic optimization of carrier balance and recombination range expansion.
[0011] Based on the optimal process parameters determined by the above process screening and optimization methods, the present invention further provides an all-inorganic quantum dot light-emitting diode based on a zinc oxide quantum dot homojunction, comprising a substrate, an anode, a hole transport layer, a light-emitting layer, an electron transport layer and a cathode stacked sequentially.
[0012] The hole transport layer is made of ZnS-sensitized aminosilane-functionalized ZnO quantum dots, specifically a composite system of ZnS nanoclusters and AP-ZnO quantum dots, wherein the mass ratio of ZnS nanoclusters to AP-ZnO quantum dots is 1:25 to 50; the electron transport layer is made of NaCl-doped AP-ZnO quantum dots, wherein the amount of NaCl doping is 2.5% to 5% based on the mass of AP-ZnO quantum dots.
[0013] The luminescent layer is made of core-shell perovskite quantum dots, comprising a perovskite quantum dot core and a ZnO shell covering the surface of the perovskite quantum dot core; preferably, the core-shell perovskite quantum dots are CsPbBr3@ZnO core-shell quantum dots. The ZnO shell not only fully preserves the exciton luminescence properties of the perovskite core, but also constructs a continuous high-mobility carrier transport channel, while physically blocking the translayer migration and diffusion of perovskite ions.
[0014] The hole transport layer has a thickness of 10–20 nm, and the electron transport layer has a thickness of 10–20 nm; preferably, when the hole transport layer has a thickness of 10 nm, the electron transport layer has a thickness of 13–20 nm; when the hole transport layer has a thickness of 20 nm, the electron transport layer has a thickness of 10–15 nm.
[0015] The surface of the light-emitting layer is treated with argon plasma. This argon plasma treatment can remove adsorbed impurities, loose particles, and surface oxide layers from the surface of the light-emitting layer, break the chemical bonds of hydrophobic functional groups on the quantum dot surface and generate active dangling bonds of zinc oxide, thereby improving the hydrophilicity of the film and suppressing the fluorescence quenching effect caused by the electron transport layer.
[0016] The light-emitting layer has a multi-layer stacked structure with 1 to 3 stacked layers.
[0017] Based on the above device structure, the present invention further provides a method for fabricating an all-inorganic quantum dot light-emitting diode, comprising the following steps: (1) Cleaning and ultraviolet ozone treatment of the substrate containing the anode (such as ITO transparent conductive glass substrate); (2) A hole transport layer material is spin-coated onto the substrate and annealed to form a hole transport layer. The precursor of the hole transport layer material is a composite system obtained by mixing ZnS nanocluster dispersion and AP-ZnO quantum dot aqueous solution at a volume ratio of 1:25-50 and stirring at room temperature for 24 hours. The concentrations of both ZnS quantum dot dispersion and AP-ZnO quantum dot aqueous solution are 20 mg / mL. The preferred spin-coating parameters for the hole transport layer are a rotation speed of 5000 rpm, an acceleration of 2000 rpm / s, a time of 30 s, an annealing temperature of 120℃-150℃, and an annealing time of 10-15 min.
[0018] (3) Spin-coating a core-shell perovskite quantum dot solution onto the hole transport layer and annealing it to form a light-emitting layer; the number of stacked light-emitting layers is 1 to 3, and the spin-coating parameters for each light-emitting layer are: rotation speed 1000 to 2000 rpm, acceleration 1000 rpm / s, time 30s, annealing temperature 60 to 80℃, and annealing time 10 to 15 min.
[0019] (4) The surface of the light-emitting layer is subjected to argon plasma treatment; the conditions for argon plasma treatment are: radio frequency power 50 W, argon flow rate 20 sccm, working pressure 2 Pa, and treatment time 30 s. (5) An electron transport layer material is spin-coated onto the plasma-treated luminescent layer and annealed to form an electron transport layer. The precursor of the electron transport layer material is a doped system formed by mixing AP-ZnO quantum dot aqueous solution and NaCl aqueous solution at a volume ratio of 100:(5-10). The concentration of AP-ZnO quantum dot aqueous solution is 20 mg / mL, and the concentration of NaCl aqueous solution is 10 mg / mL. The preferred spin-coating parameters for the electron transport layer are a rotation speed of 2000 rpm, an acceleration of 1000 rpm / s, a time of 30s, an annealing temperature of 60-80℃, and an annealing time of 10-15 min.
[0020] (6) A metal cathode is deposited on the electron transport layer.
[0021] The aforementioned process screening and optimization methods, along with device structure design and fabrication methods, constitute a fully integrated process system encompassing "plasma interface passivation—PL defect screening—SCLC carrier matching—JV / CV joint verification—synergistic control of the number of emitting layers." This system first improves the interfacial affinity between EML and ETL through argon plasma treatment, suppressing fluorescence quenching. Then, it quantitatively screens low-defect HTL spin-coating processes using PL spectroscopy based on the ratio of intrinsic bandgap emission peak to oxygen vacancy defect peak intensity. Next, it qualitatively matches the carrier conductivity of HTL and ETL using SCLC single-carrier JV curves, determining the film thickness matching range. Then, it comprehensively determines the optimal spin-coating parameters based on the complete device's JV and CV electrical characteristics and the quantitative results of luminescence uniformity measurement. Finally, based on HTL / ETL carrier matching, by controlling the number of EML stacked layers, the system utilizes the thick-film effect to broaden the carrier recombination range and disperse exciton concentration to suppress interfacial non-radiative recombination, while simultaneously offsetting the transport resistance losses introduced by multiple emitting layers, achieving a significant improvement in the brightness and luminescence uniformity of the all-inorganic QLED device.
[0022] Compared with existing technologies, this invention is the first to use zinc oxide quantum dots to construct homojunction QLED devices, wherein the light-emitting layer is a core-shell structure CsPbBr3@ZnO quantum dot, and the carrier transport layer is obtained by doping or sensitizing AP-ZnO. Based on this, a fully integrated and synergistically optimized process system is established, encompassing interface modification, transport layer fabrication, film thickness matching, and light-emitting layer stacking. Compared with existing technologies, this invention has the following significant advantages: 1. Advantages of the passivation process at the luminescent layer interface: This invention uses argon plasma to pretreat the surface of perovskite quantum dot films. Argon plasma can gently strip adsorbed impurities and the surface oxide layer, break hydrophobic chemical bonds on the surface, and generate a large number of active dangling bonds, thereby improving the interfacial affinity between the luminescent layer and the aqueous electron transport layer. Simultaneously, the interface modification effect can be quantified by the attenuation of the luminescent layer's plasma intensity (PL), fundamentally suppressing quantum dot fluorescence quenching caused by ETL contacts and fully preserving the intrinsic luminescent properties of the quantum dots.
[0023] 2. Advantages of Inorganic Hole Transport Layer Modification and Screening: This invention uses a ZnS and AP-ZnO (mass ratio 1:50) quantum dot composite system to prepare a composite hole transport film through a full reaction at room temperature. By using the intensity ratio of the intrinsic bandgap emission peak and the oxygen vacancy defect peak in the PL spectrum of the film, the defect density and p-type conductivity of the film are quantitatively evaluated. The HTL spin-coating process with low defects and high crystallinity order is quickly screened, solving the problem of insufficient hole injection and inability of the device to light up normally in traditional inorganic hole transport layer films.
[0024] 3. Quantitative Evaluation System for Carrier Co-matching: This invention establishes a multi-dimensional joint characterization standard. By qualitatively comparing the hole and electron transport magnitudes through the JV curve of a single carrier in SCLC, the thickness of each functional layer film is coordinated to balance the internal carrier transport of the device. Combined with the quantitative results of the complete device's JV and CV electrical characteristics and luminescence uniformity, the optimal spin-coating parameters are comprehensively determined to accurately match the hole and electron injection rates, significantly reduce the device's low-voltage leakage current and interface excess charge accumulation, and weaken the interface non-radiative recombination loss.
[0025] 4. Core-shell structure suppresses ion migration, while thick-film emitting layer synergistically enhances performance: The ZnO-coated CsPbBr3 core-shell quantum dots used in this invention retain the exciton luminescence characteristics of the perovskite core within their zinc oxide shell, while simultaneously constructing a continuous high-mobility carrier transport channel and physically blocking the cross-layer migration and diffusion of perovskite ions. Building upon this, and ensuring HTL / ETL carrier transport matching, this invention employs a thick-film stacked EML to widen the carrier recombination region, disperse exciton concentration to suppress interfacial nonradiative recombination, mitigate efficiency roll-off at high brightness, and offset the transport resistance losses introduced by the multilayer emitting layer. This results in a significant improvement in the brightness and luminous uniformity of the all-inorganic QLED device.
[0026] 5. Engineering value of the entire process: This invention uses zinc oxide quantum dots to construct homojunction QLED devices, forming a quantifiable and reproducible evaluation standard for the entire process. It standardizes the process parameters of interface treatment, transport layer film formation, film thickness matching, and multi-layer light-emitting layer control, reduces the device debugging threshold, effectively improves the dark spots and uneven light emission caused by traditional processes, and significantly improves the light emission uniformity, photoelectric conversion efficiency and long-term working stability of all-inorganic perovskite QLEDs. Attached Figure Description
[0027] Figure 1 Fourier transform infrared (FTIR) spectra of EML films before and after argon plasma treatment.
[0028] Figure 2 The images show the water contact angle of the EML film before and after argon plasma treatment, where (a) corresponds to before treatment and (b) corresponds to after treatment.
[0029] Figure 3 This is a comparison of the plasma intensity (PL) of different solvent systems ETLs spin-coated onto the surface of EML films treated with argon plasma.
[0030] Figure 4 Comparison of fluorescence intensity of bandgap emission peak and oxygen vacancy emission peak of HTL films prepared with different spin-coating process parameters.
[0031] Figure 5 JV characteristic curves of single-electron devices (TEOD) with electron transport layer AP-ZnO:Na and single-hole devices (HOD) with hole transport layer ZnS:AP-ZnO under different spin-coating parameters.
[0032] Figure 6 JV characteristic curves of a single-hole device without an emitting layer.
[0033] Figure 7 To optimize HTL spin coating parameters, the (a) JV and (b) CV curves of all-inorganic QLEDs obtained under different ETL spin coating parameters are shown.
[0034] Figure 8 JV curves for hybrid QLEDs (a) and all-inorganic QLEDs (b) with 1 to 3 light-emitting layers.
[0035] Figure 9 The LV curves are for a hybrid QLED (a) with 1 to 3 light-emitting layers and an all-inorganic QLED (b).
[0036] Figure 10 The CV curves are for a hybrid QLED (a) with 1 to 3 light-emitting layers and an all-inorganic QLED (b). Detailed Implementation
[0037] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described clearly and completely below with reference to the accompanying drawings and embodiments. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0038] Example 1: Interface modification and carrier balance regulation of homojunction devices 1.1 Fabrication of QLED Devices This embodiment prepares the QLED device according to the following steps: 1. Substrate Treatment: The patterned indium tin oxide (ITO) glass (16mm × 16mm, 1.1mm thick) was ultrasonically treated for 20 minutes in a beaker containing a mixture of ITO cleaning solution and deionized water at a volume ratio of 1:20. Then, it was sequentially immersed in ethanol and deionized water, followed by ultrasonic treatment for 20 minutes each. Finally, it was rinsed with deionized water to remove residual impurities. After drying with nitrogen, it was annealed on a 120℃ hot plate and then treated with ultraviolet ozone (UV-Zone) for 15 minutes.
[0039] 2. Preparation of the hole transport layer: Referring to the method in Example 1 of patent CN 118598180 A, a monodisperse ZnS nanocluster dispersion with a concentration of 20 mg / mL was prepared. Referring to the method in Example 1 of patent CN 117623369 A, an aqueous solution of aminosilane-functionalized ZnO nanocrystals (AP-ZnO) with a concentration of 20 mg / mL was prepared. The ZnS nanocluster dispersion was added to the AP-ZnO aqueous solution (volume ratio 1:50), and stirred at room temperature for 24 h to obtain a ZnS-sensitized AP-ZnO dispersion (denoted as ZnS:AP-ZnO). After filtration through a 0.45 μm aqueous filter, it was spin-coated onto an ITO glass substrate with the following spin-coating parameters: rotation speed 5000 rpm, acceleration 2000 rpm / s, and time 30 s. After spin-coating, it was annealed at 120 °C for 15 min to obtain the hole transport layer (HTL).
[0040] 3. Preparation of the luminescent layer: Following the method described in Example 2 of patent CN 115975631 B, CsPbBr3@ZnO quantum dots were prepared. A CsPbBr3@ZnO quantum dot dispersion with a concentration of 15 mg / mL was prepared using a mixed solvent of n-octane and n-hexane at a volume ratio of 3:2. After filtration through a 0.45 μm organic filter, the dispersion was spin-coated onto the hole transport layer. The spin-coating parameters were: rotation speed 2000 rpm, acceleration 1000 rpm / s, and time 30 s. After spin-coating, the dispersion was annealed at 70 °C for 15 min to obtain the luminescent layer (EML).
[0041] 4. Plasma treatment of the luminescent layer: The CsPbBr3@ZnO quantum dot film, which serves as the luminescent layer, was treated with argon plasma under the following conditions: RF power 50W, argon flow rate 20sccm, working pressure 2Pa, and treatment time 30s.
[0042] 5. Preparation of the electron transport layer: Referring to the method in Example 1 of patent CN 117623369 A, an AP-ZnO aqueous solution with a concentration of 20 mg / mL was prepared; a NaCl aqueous solution with a concentration of 10 mg / mL was also prepared. The AP-ZnO aqueous solution and the NaCl aqueous solution were mixed at a volume ratio of 100:5 to form an AP-ZnO:5% Na-doped system. After filtering through a 0.45 μm aqueous filter, the mixture was spin-coated onto a plasma-treated EML. The spin-coating parameters were: rotation speed 2000 rpm, acceleration 1000 rpm / s, and time 30 s. After spin-coating, the mixture was annealed at 70 °C for 15 min to obtain the electron transport layer (ETL).
[0043] 6. Cathode preparation: A shadow mask is used in a high vacuum (<5×10⁻⁶) environment. -6 All-inorganic QLED devices were fabricated by vapor deposition of Ag cathode in Torr.
[0044] 1.2 Characterization of the effect of plasma interface modification Fourier transform infrared (FTIR) spectra of CsPbBr3@ZnO quantum dot films before and after argon plasma (Plasma) treatment are as follows: Figure 1 As shown in the figure, before treatment, the film surface exhibited hydrophobic CO stretching vibration peaks, oleic acid accessory vibration peaks, and characteristic peaks of Si-O-Si bonds formed by the condensation of silanol groups. After argon plasma treatment, the intensities of the above-mentioned hydrophobic characteristic peaks were significantly reduced, indicating that the hydrophobic functional groups on the surface were effectively removed.
[0045] like Figure 2 As shown, plasma treatment reduced the water contact angle on the thin film surface from 73° before treatment. Figure 2 (a) significantly decreased to 54° after treatment. Figure 2(b) The hydrophilicity of the film is significantly improved, which provides favorable conditions for the uniform coating of the subsequent aqueous ETL.
[0046] To further evaluate the energy level matching and interface compatibility between ETL and EML after plasma treatment, this experiment spin-coated ethanol-based ZnMgO and aqueous AP-ZnO:5%Na electron transport layers onto the surface of the plasma-treated quantum dot luminescent layer, respectively. Blank control groups were also added using pure ethanol and pure water solvents. The relevant results are as follows: Figure 3 As shown.
[0047] The results showed that the fluorescence intensity of all solvent-based blank groups decreased significantly, with the fluorescence intensity of the ethanol solvent system being higher than that of the pure water system. After spin-coating ethanol-based ZnMgO ETL, the composite film experienced near-complete fluorescence quenching, mainly due to the intense nonradiative recombination caused by numerous interface defects. The defect energy levels acted as recombination centers, rapidly dissipating photoexcitons and leading to a sharp decrease in fluorescence signal. In contrast, after spin-coating aqueous AP-ZnO:Na ETL, the fluorescence intensity of the composite film showed almost no significant decrease compared to the plasma-treated emitting layer, indicating that AP-ZnO:Na significantly suppressed the nonradiative recombination loss dominated by interface defects, achieving better energy level matching with the emitting layer. Combined with the solvent control results, the interference of pure solvent on quantum dot fluorescence can be ruled out, further confirming that AP-ZnO:Na and the quantum dot emitting layer possess excellent interfacial compatibility and energy level matching characteristics under plasma regulation.
[0048] 1.3 Hole transport layer defect screening Defect screening was performed on the hole transport layer. Multiple sets of spin-coating process parameters were used to prepare HTL films on pretreated ITO substrates, and defects in each HTL film were characterized by photoluminescence (PL) spectroscopy. The PL spectra of the films included the intrinsic bandgap characteristic emission peak and the oxygen vacancy-induced defect emission peak. The ratio of the intrinsic bandgap emission peak intensity to the oxygen vacancy defect peak intensity was used as the evaluation index; a higher ratio indicates a lower proportion of oxygen vacancy defects and superior p-type conductivity.
[0049] After comparing multiple sets of spin coating parameters ( Figure 4 Two optimal ZnS:AP-ZnO HTL spin-coating processes were selected: 3000 rpm, 1000 rpm / s; and 5000 rpm, 2000 rpm / s. The HTL film prepared at (3000 rpm, 1000 rpm / s) exhibited limited crystal orientation coverage and insufficient surface crystal uniformity, resulting in only localized illumination (approximately 50% of the area emitting green light) in subsequent device experiments. In contrast, the HTL film prepared at (5000 rpm, 2000 rpm / s) showed significantly improved crystal orientation in the central region and markedly enhanced film order.
[0050] However, the device prepared using this preferred HTL process (5000 rpm, 2000 rpm / s) combined with ETL spin coating at (5000 rpm, 1000 rpm / s) failed to light up initially, and the JV curve ( Figure 7 The black curve (a) shows that the device current is significantly higher than expected. Therefore, further analysis of the carrier transport characteristics of HTL and ETL is needed through single-carrier device testing.
[0051] 1.4 Single-carrier transmission capability matching The single-carrier transport characteristics of HTL and ETL under different process conditions were characterized using the space charge-confined current (SCLC) method. The complete device structures were: TEOD: ITO / ZnO / EML / AP-ZnO:Na / Ag; HOD: ITO / ZnS:AP-ZnO / EML / MoO3 / Al. The test results are as follows: Figure 5 As shown.
[0052] For the electron transport layer TEOD:AP-ZnO:Na, as the spin coating speed increases, the current density gradually increases under the same applied voltage, and the electron transport capability is continuously enhanced.
[0053] For the hole transport layer HOD:ZnS:AP-ZnO, the hole conduction capacity of the sample prepared at 3000 rpm is significantly higher than that of the sample prepared at 5000 rpm.
[0054] Given that the semiconductor layer is not unique and is quite complex, the test curves do not show a clearly defined trap-filled (TFL) region. This study only uses the JV curves to make a qualitative comparison of carrier transport capabilities, and does not use the simplified Mott-Gurney model to quantitatively extract mobility and trap density.
[0055] Comparing the current densities of each group of curves, it can be seen that the single-hole device (HTL is ZnS:AP-ZnO, 5000 rpm, 2000 rpm / s) and the single-electron device (ETL is AP-ZnO:Na, 2000 rpm, 1000 rpm / s) have the closest carrier conduction levels. This combination is beneficial for achieving a balance between the injection of holes and electrons inside the QLED device.
[0056] To further refine the single-carrier SCLC characterization of the device, a single-hole device without an emitting layer was used, and the results are shown in Figure 6. The device exhibits complete transport characteristics in the three segments of S=1, S>2, and S=2. The device meets the applicability premise of the Mott-Gurney model, and the hole carrier mobility can be quantitatively calculated and analyzed using the high-voltage range of S=2 combined with the Mott-Gurney formula.
[0057] 1.5 Joint verification of complete device via JV / CV Three groups of all-inorganic QLEDs with different ETL spin coating processes (rotation speeds of 2000 rpm, 3000 rpm, and 5000 rpm, with an acceleration of 1000 rpm / s) were characterized by combined JV and CV electrical characterization. The results are as follows: Figure 7 As shown.
[0058] As the ETL spin coating speed increases, the electron transport capability continues to improve, and the current density of the device at the same voltage increases sequentially: At 5000 rpm, the ETL exhibits significantly stronger electron transport capability than the HTL, indicating an excess of electron injection. Electrically, this manifests as a higher initial leakage current in the low-voltage range and a peak capacitance of 3.4 nF on the CV curve, suggesting a large amount of excess accumulated electrons at the emitting layer interface, inducing non-radiative recombination losses.
[0059] 3000 rpm ETL: exhibits a similar but milder carrier imbalance.
[0060] 2000 rpm ETL: The electron transport rate is optimally matched with the hole transport rate of the HTL. The device has the lowest initiation current in the low-voltage range, and unwanted leakage current is suppressed; the CV peak capacitance is the lowest among the three groups (2.3 nF), indicating that the excess carrier accumulation effect at the emissive layer interface is the weakest, and holes and electrons can more fully undergo radiative recombination in the emissive layer, ultimately achieving the optimal optoelectronic performance of the device.
[0061] When the HTL spin coating speed is 5000 rpm, the corresponding film thickness is about 10 nm, and the matching ETL thickness range is 13-20 nm, with the optimal film thickness being 15 nm; when the HTL spin coating speed is 3000 rpm, the corresponding film thickness is about 20 nm, and the matching ETL thickness range is 10-15 nm, with the optimal film thickness being 10 nm.
[0062] Example 2: Synergistic Regulation of Core-Shell Quantum Dot Emissive Layer Thickness and Suppression of Ion Migration Based on the HTL / ETL matching process determined in Example 1, this example further studies the stacking layer number control of the CsPbBr3@ZnO core-shell structure quantum dot luminescent layer.
[0063] Previous studies have shown that multilayer stacking to construct thick EMLs can broaden the carrier recombination region and reduce the local carrier concentration at the interface. However, excessive film thickness increases carrier transport resistance and disrupts the hole-electron injection balance. Meanwhile, perovskite quantum dots intrinsically exhibit field-induced ion migration. Migrating halide and lead ions accumulate at the functional layer interface, further exacerbating interfacial charge accumulation. This behavior can be observed through JV and CV electrical characterization.
[0064] Hybrid QLEDs (ITO / PEDOT:PSS / PTAA / EML(nL) / AP-ZnO:5% Na / Ag) and all-inorganic QLEDs (ITO / ZnS:AP-ZnO / EML(nL) / AP-ZnO:5% Na / Ag) were prepared respectively. EMLs were prepared with 1 layer (1L), 2 layers (2L), and 3 layers (3L) gradients. The effects of EML thickness on carrier transport, interfacial charge accumulation, and ion migration-induced interfacial degradation behavior were studied by JVL and CV electrical characterization.
[0065] 2.1 JVL Feature Analysis JVL test results are as follows Figure 8 (JV curve) and Figure 9 As shown in the LV curve.
[0066] Hybrid devices ( Figure 8 a, Figure 9 a) As the number of EML layers increases, the current density at the same voltage gradually decreases. PTAA has a strong hole injection capability. While thickening the EML extends the carrier transport path and reduces the local carrier concentration at the interface, excessive film thickness further increases transport resistance, disrupts the hole-electron injection balance, and leads to a significant decrease in device performance. The device brightness increases from a single-layer EML with a turn-on voltage of 2.5 V to a maximum brightness of 2332 cd / m². 2 The starting voltage of the dual-layer EML drops to 3.0 V, and the maximum brightness is 2221 cd / m². 2 The three-layer EML device can hardly be lit.
[0067] All inorganic devices ( Figure 8 b、 Figure 9(b) The current density ranking is 3L EML > 1L EML > 2L EML, with the 2-layer EML device exhibiting the lowest low-voltage leakage current. A single-layer EML has a limited thickness, resulting in a narrow carrier recombination region and exciton concentration near the EML-ETL interface. The high local electric field at the interface easily induces defect-induced nonradiative recombination and drives perovskite ions to migrate and accumulate at the transport layer interface. With a 2-layer EML, additional interlayer interface traps are formed, hindering effective electron-hole exchange. A large number of carriers are captured by the internal interface. Although the excess charge accumulation at the interface is reduced, the radiative recombination efficiency is significantly degraded. The newly added interlayer interface also becomes a site for ion migration and accumulation. When stacked to a 3-layer EML, the ZnO core-shell shell physically blocks the diffusion of perovskite ions across the shell. The multilayer film structure extends the ion migration and diffusion path, weakening the migration and enrichment of ions towards the transport layer interface under an electric field. The sufficiently thick luminescent layer constructs a broad and continuous carrier recombination region, which can disperse exciton concentration, reduce the local electric field at the interface, and suppress Auger quenching. The expanded recombination space effectively offsets the transport resistance loss caused by the increased film thickness. The device brightness increased from 150 cd / m². 2 Rising to 295 cd / m 2 The start-up voltage dropped from 3.6 V to 3.3 V.
[0068] 2.2 CV Characteristic Analysis Based on studies related to impedance spectroscopy and CV characterization, the peak capacitance of the QLED capacitance-voltage curve can quantitatively characterize the total amount of excess carriers accumulated at the multilayer functional interfaces of the device: the higher the peak capacitance, the more unradiative recombination charge is trapped at the interface, and the more severe the nonradiative loss. Perovskite migrating ions act as space charges at the interface, further increasing the CV peak capacitance, exacerbating the interface polarization effect, and degrading the device's photoelectric performance; the peak voltage reflects the height of the carrier injection barrier, and the rate of capacitance decrease after the peak can characterize the exciton radiative recombination efficiency.
[0069] CV test results as follows Figure 10 As shown.
[0070] Hybrid QLED ( Figure 10 a) Employing a high-mobility organic hole transport layer results in a natural excess of hole injection. Increasing the number of EML layers continuously introduces new charge accumulation interfaces, while more interfaces provide sites for perovskite ion migration and enrichment. The peak capacitance monotonically increases from 1.74 nF in a single-layer EML to 3.54 nF in a three-layer EML. Therefore, a single-layer EML results in the least interface charge accumulation and optimal device performance.
[0071] All-inorganic QLED ( Figure 10(b) In an all-inorganic system where HTL / ETL carrier transport matching is pre-completed, the three-layer CsPbBr3@ZnO core-shell luminescent layer, on the one hand, relies on the physical constraint of the ZnO shell on the migration of perovskite ions, and on the other hand, reduces the local electric field at the interface and suppresses ion aggregation at the interface through the thick film effect. This balances the film transport resistance and the recombination range widening effect, minimizing the accumulation of excess carriers at the interface. The polarization capacitance is 2.09 nF at 3L EML, lower than 2.3 nF at 1L EML and 3.5 nF at 2L EML.
[0072] The experimental patterns described above are highly consistent with the JV leakage current characteristics and CV impedance characterization theories, establishing an optimization strategy for all-inorganic QLEDs that combines "transport layer matching + synergistic control of light-emitting layer thickness" to achieve carrier balance and suppress perovskite ion migration.
[0073] The all-inorganic QLED device constructed in this invention effectively solves the core technical problems of high interface polarization capacitance, HTL / ETL carrier transport imbalance, high defect density of inorganic hole transport layer and poor light emission uniformity in traditional heterojunction structures. It achieves a significant reduction in device polarization capacitance and an effective balance in carrier injection, and obtains green electroluminescence with uniformity and high brightness across the entire domain under the all-inorganic device architecture.
[0074] The above description is merely an exemplary embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A fully inorganic quantum dot light-emitting diode based on a zinc oxide quantum dot homojunction, characterized in that, It includes a substrate, an anode, a hole transport layer, an electron transport layer, and a cathode, which are stacked sequentially. The material of the light-emitting layer is a core-shell perovskite quantum dot, which includes a perovskite quantum dot core and a ZnO shell covering the surface of the perovskite quantum dot core. The hole transport layer is made of ZnS-sensitized aminosilane-functionalized ZnO quantum dots; the electron transport layer is made of NaCl-doped aminosilane-functionalized ZnO quantum dots.
2. The all-inorganic quantum dot light-emitting diode according to claim 1, characterized in that, The core-shell perovskite quantum dots are CsPbBr3@ZnO core-shell quantum dots.
3. The all-inorganic quantum dot light-emitting diode according to claim 1, characterized in that, The ZnS-sensitized aminosilane-functionalized ZnO quantum dots are a composite system of ZnS nanoclusters and aminosilane-functionalized ZnO quantum dots, wherein the mass ratio of ZnS nanoclusters to aminosilane-functionalized ZnO quantum dots is 1:25-50.
4. The all-inorganic quantum dot light-emitting diode according to claim 1, characterized in that, In the NaCl-doped aminosilane-functionalized ZnO quantum dots, the amount of NaCl doping is 2.5% to 5% based on the mass of the aminosilane-functionalized ZnO quantum dots.
5. The all-inorganic quantum dot light-emitting diode according to claim 1, characterized in that, The hole transport layer has a thickness of 10–20 nm, and the electron transport layer has a thickness of 10–20 nm.
6. The all-inorganic quantum dot light-emitting diode according to claim 1, characterized in that, The light-emitting layer has a multi-layer stacked structure with 1 to 3 stacked layers.
7. The all-inorganic quantum dot light-emitting diode according to claim 1, characterized in that, The surface of the light-emitting layer is treated with argon plasma.
8. A method for fabricating an all-inorganic quantum dot light-emitting diode as described in any one of claims 1 to 7, characterized in that, Includes the following steps: (1) The substrate containing the anode is cleaned and treated with ultraviolet ozone; (2) A hole transport layer material is spin-coated onto the substrate and annealed to form a hole transport layer; (3) Spin-coating a core-shell perovskite quantum dot solution onto the hole transport layer and annealing it to form a light-emitting layer; (4) The surface of the light-emitting layer is subjected to argon plasma treatment; (5) Spin-coating an electron transport layer material onto the luminescent layer after argon plasma treatment, followed by annealing to form an electron transport layer; (6) A metal cathode is deposited on the electron transport layer.
9. The preparation method according to claim 8, characterized in that, The precursor of the hole transport layer material in step (2) is a composite system obtained by mixing ZnS nanocluster dispersion and aminosilane-functionalized ZnO quantum dot aqueous solution and stirring at room temperature for 24 h; the precursor of the electron transport layer material in step (5) is a doped system formed by mixing aminosilane-functionalized ZnO quantum dot aqueous solution and NaCl aqueous solution.
10. The preparation method according to claim 8, characterized in that: In step (2), the spin coating parameters for the hole transport layer are 5000 rpm rotation speed, 2000 rpm / s acceleration, and 30s time, with an annealing temperature of 120℃~150℃ and an annealing time of 10~15min; in step (3), the number of stacked light-emitting layers is 1~3 layers, and the spin coating parameters for each light-emitting layer are 1000~2000 rpm rotation speed, 1000 rpm / s acceleration, and 30s time, with an annealing temperature of 60~80℃ and an annealing time of 10~15min; in step (4), the conditions for argon plasma treatment are: 50W RF power, 20sccm argon flow rate, 2Pa working pressure, and 30s treatment time; in step (5), the spin coating parameters for the electron transport layer are 2000 rpm rotation speed, 1000 rpm / s acceleration, and 30s time, with an annealing temperature of 60~80℃ and an annealing time of 10~15min.