An isocyanate silane modified molybdenum disulfide interfacial anchoring type polyurea grease
By activating molybdenum disulfide nanosheets and modifying them with isocyanate silane, and embedding them into a polyurea thickened network, the problem of molybdenum disulfide agglomeration under high temperature conditions was solved, thereby improving the high-temperature stability and low-friction performance of the grease.
Patent Information
- Application Number
- CN202611429654.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-20
AI Technical Summary
In the prior art, the bonding between molybdenum disulfide and polyurea segments is weak, which makes it easy to agglomerate and settle under high temperature, long-term shear or heavy load conditions, affecting the colloidal stability, high-temperature viscosity retention and dropping point of the grease.
Molybdenum disulfide nanosheets were prepared by treating them with an activator to form isocyanate silane-modified molybdenum disulfide nanosheets. These nanosheets were then reacted with an isocyanate-based alkoxysilane coupling agent to form modified molybdenum disulfide nanosheets. Subsequently, these nanosheets were dispersed in situ in a polyurea thickened network to form an isocyanate silane bridging layer that forms an interface with the polyurea segments and is embedded in the thickened network.
It improves the bonding strength between molybdenum disulfide and the polyurea network, enhances dispersion stability, maintains the continuity of the thickened network, improves the dropping point and high-temperature viscosity retention of the grease, and reduces the coefficient of friction.
Smart Images

Figure CN123132071A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of lubricating materials, high-temperature greases and polyurea thickeners, specifically relating to an isocyanate silane-modified molybdenum disulfide interface anchoring polyurea composite thickener, a grease containing the composite thickener and its preparation method, which can be used in mechanical friction parts under high temperature, high load and long cycle operation. Background Technology
[0002] Polyurea greases possess good oxidation stability, thermal stability, mechanical stability, and service life, and are widely used in the lubrication of motor bearings, metallurgical machinery, aerospace, and high-end equipment. The performance of polyurea greases depends primarily on the type of base oil, the polyurea thickening network structure, and the dispersion state and interfacial interaction of the solid lubricating components within the thickened network.
[0003] Molybdenum disulfide (MoD) possesses a layered crystal structure and excellent solid lubrication properties, making it a commonly used extreme pressure anti-wear component in greases. Current technologies often incorporate MoD as an additive powder directly into the grease system, relying on its interlayer slippage to reduce friction and wear. While this method can improve friction performance, the relationship between MoD and polyurea segments is primarily one of weak adsorption or mechanical mixing, making it difficult to form a stable interface with the polyurea thickened network.
[0004] Under high temperature, prolonged shearing, or heavy load conditions, ordinary molybdenum disulfide is prone to agglomeration, sedimentation, or localized enrichment, resulting in a decrease in the continuity of the polyurea fiber network. This, in turn, affects the colloidal stability, high-temperature viscosity retention, and dropping point of the grease. Simply increasing the amount of molybdenum disulfide added cannot effectively solve this problem; excessive addition will actually weaken the integrity of the thickened network, leading to a decrease in the high-temperature stability of the grease. Summary of the Invention
[0005] In view of the defects or deficiencies of the prior art, the present invention provides an isocyanate silane modified molybdenum disulfide interface anchoring polyurea grease.
[0006] Therefore, the lubricating grease provided by the present invention is prepared by the following method steps: Step 1: Activate molybdenum disulfide nanosheets using an activating agent. Then, react the activated molybdenum disulfide nanosheets with an isocyanate-containing alkoxysilane coupling agent in an organic solvent under an inert atmosphere and at 60–90°C to prepare modified molybdenum disulfide nanosheets. The activating agent is selected from hydrogen peroxide solution, peracetic acid aqueous solution, ozone aqueous solution, or sodium hypochlorite solution. The isocyanate-containing alkoxysilane coupling agent is selected from γ-isocyanate propyltriethoxysilane, γ-isocyanate propyltrimethoxysilane, or a combination of the two. Step 2: Modified molybdenum disulfide nanosheets are dispersed in base oil, followed by the addition of 4,4′-diphenylmethane diisocyanate and amine compounds. The mixture is then subjected to a polyurea reaction at 100–140°C. After the reaction is complete, the system is heated to 150–200°C for refining. Subsequently, the mixture is cooled, functional additives are added, degassed, and homogenized to obtain a lubricating grease. The base oil is one or more of cycloalkyl mineral oil, polyalphaolefin, and synthetic ester oil. The amine compounds are a mixture of C8-C22 aliphatic monoamines and polyamines, and the polyamines include one or more of ethylenediamine, dodecylamine, and diethylenetriamine.
[0007] An optional feature is that the molybdenum disulfide nanosheets have an average sheet diameter of 50-500 nm, preferably 100-300 nm, and a sheet thickness of 1-30 nm, preferably 3-15 nm.
[0008] An alternative approach is that the mass ratio of the activated molybdenum disulfide nanosheets to the isocyanate-containing alkoxysilane coupling agent is 1:0.05-0.60.
[0009] An alternative is that, based on 100% of the total mass of the grease, the base oil is 70-91 wt%, the 4,4′-diphenylmethane diisocyanate and amine compounds together are 8-25 wt%, the modified molybdenum disulfide nanosheets are 0.5-2.5 wt%, the functional additives are 0.1-5 wt%, and the sum of the amounts of all components is 100 wt%.
[0010] An optional option is that the modified molybdenum disulfide nanosheets are 1.5-2.5 wt% based on the total mass of the grease, preferably 1.5 wt%.
[0011] Alternatively, the functional additive may include one or more of antioxidants, rust inhibitors, extreme pressure anti-wear agents, and metal passivators.
[0012] An alternative approach is to have a reaction time of 4-8 h in step S1; a polyurea reaction time of 30-90 min in step S3; and a refining time of 20-60 min.
[0013] The grease has a dropping point of not less than 310°C and an apparent viscosity retention rate of not less than 90% after being kept at 200°C for 60 minutes. Preferably, the grease has a dropping point of not less than 328°C and an apparent viscosity retention rate of not less than 94% after being kept at 200°C for 60 minutes.
[0014] Beneficial effects (1) In this invention, ordinary molybdenum disulfide is converted into isocyanate silane modified molybdenum disulfide, and further converted into interface anchoring layer nodes that participate in the construction of polyurea thickened network, thereby improving the bonding strength between molybdenum disulfide and polyurea network.
[0015] (2) The silane bridging layer on the surface of molybdenum disulfide modified by isocyanate silane can improve its dispersion stability in base oil and polyurea precursor system, reduce agglomeration and local enrichment under high temperature shear conditions, and help maintain the continuity of polyurea thickened network.
[0016] (3) The isocyanate silane-modified molybdenum disulfide and polyurea segments form a synergistic structure of "lamellae bearing - bridging anchoring - hydrogen bond network", which can improve the dropping point and high temperature viscosity retention of grease.
[0017] (4) An appropriate amount of molybdenum disulfide sheets can play a layered solid lubricating role during frictional contact and work together with a stable polyurea thickened network to reduce the coefficient of friction. When the content is too high, local aggregation will weaken the uniformity of the network. Therefore, the present invention limits the preferred content range.
[0018] (5) The innovation of this invention is focused on the interfacial anchoring structure between isocyanate silane modified molybdenum disulfide and polyurea thickener, rather than simply adding ordinary molybdenum disulfide as a conventional additive to grease, which has a clear structural difference and source of performance improvement. Attached Figure Description
[0019] Figure 1 This is a schematic diagram of the structure of the isocyanate silane-modified molybdenum disulfide interface-anchored polyurea composite thickener of the present invention. Figure 2 This is a scanning electron microscope image of the modified molybdenum disulfide nanosheets prepared in Example 1.
[0020] Figure 3 The graph shows the dropping point trends of greases with different molybdenum disulfide contents in the examples (modified molybdenum disulfide samples) and the comparative example (unmodified molybdenum disulfide samples).
[0021] Figure 4 The apparent viscosity change curves of 1.5 wt% unmodified molybdenum disulfide sample and 1.5 wt% isocyanate silane modified molybdenum disulfide sample at 200°C are shown for the examples and comparative examples.
[0022] Figure 5 This is a comparison chart of the friction coefficients of different grease samples with different molybdenum disulfide contents in the examples (modified molybdenum disulfide sample) and the comparative example (unmodified molybdenum disulfide sample). Detailed Implementation
[0023] Unless otherwise specified, the scientific and technical terms used in this article are intended for understanding by those skilled in the art.
[0024] The key to this invention lies in the isocyanate silane modification and interface anchoring method of the molybdenum disulfide sheets. The modified molybdenum disulfide is pre-dispersed in the oil phase and the polyurea precursor system before the polyurea thickening network is formed in situ, so that it is embedded in the polyurea network during the reaction process, rather than being added as a regular powder after the grease is formed.
[0025] The modified molybdenum disulfide nanosheets of this invention are obtained by reacting molybdenum disulfide nanosheets, after hydroxylation or defect activation, with an isocyanate-containing alkoxysilane coupling agent. The isocyanate-containing alkoxysilane coupling agent forms a silane bridging layer on the surface of the molybdenum disulfide sheets, which can be coupled with the polyurea reaction system. This silane bridging layer forms an interface with amine compounds or polyurea segments during the subsequent in-situ polyurea reaction, allowing the modified molybdenum disulfide nanosheets to be embedded in the polyurea thickened network in the form of sheet nodes. See also... Figure 1 As shown, isocyanate silane-modified molybdenum disulfide sheets are embedded as interface nodes in the polyurea thickened network. The silane bridging layer improves the dispersibility of molybdenum disulfide in the oil phase and the polyurea precursor system, and enhances the interfacial coupling between molybdenum disulfide and the polyurea network through reactive bonding and hydrogen bonding.
[0026] In this invention, modified molybdenum disulfide nanosheets are pre-dispersed in base oil before the reaction of diisocyanate compounds and amine compounds to form a polyurea thickened network. This allows the modified molybdenum disulfide nanosheets to be anchored within the thickened network during the in-situ reaction of polyurea. Specifically, the surface of the modified molybdenum disulfide sheets is anchored to the polyurea segments at multiple points through isocyanate silane bridging layers, urea group connections, and hydrogen bonding, thus transforming molybdenum disulfide from a common added powder into sheet nodes within the polyurea network.
[0027] The polyurea thickened network of the present invention is formed by reacting 4,4′-diphenylmethane diisocyanate with amine compounds; the amine compounds include C8-C22 aliphatic monoamines and polyamine compounds, and the polyamine compounds include one or two of ethylenediamine and diethylenetriamine.
[0028] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. It should be noted that the following embodiments are only some examples of the present invention. Based on the technical concept of the present invention, those skilled in the art can optimize the process by adjusting the relevant reaction conditions. These relevant reaction conditions include, but are not limited to, the reaction temperature of each step, the organic solvent used and its amount, and the reactants and their proportions. In the following embodiments, unless specific conditions are specified, conventional conditions or conditions recommended by the manufacturer are followed. Raw materials, reagents, or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0029] In the following examples, hydrogen peroxide solution is used to selectively and mildly oxidize the edge defect sites of molybdenum disulfide nanosheets, introducing hydroxyl active sites on the powder surface to provide reaction sites for subsequent silane coupling grafting. This hydrogen peroxide solution can also be replaced with at least one of peracetic acid aqueous solution or ozone aqueous solution. Oxidation conditions should be controlled to avoid excessive oxidation of molybdenum disulfide by the oxidant, which could lead to the formation of molybdenum trioxide impurities and impair the solid lubrication properties of the modified powder. When a dilute sodium hypochlorite solution is used as the oxidant, thorough rinsing with water is necessary after oxidation to remove residual inorganic salt ions, preventing salt impurities from being introduced into the grease system and deteriorating the high-temperature and rust-preventive properties of the grease.
[0030] Example 1: Step 1, Preparation of modified molybdenum disulfide nanosheets Weigh 2.0 g of molybdenum disulfide nanosheets (average sheet diameter 200 nm, sheet thickness 3-15 nm), add them to 80 mL of ethanol / water mixed solvent (ethanol to water volume ratio 4:1), ultrasonically disperse for 30 min, add 1.0 mL of 30% hydrogen peroxide solution, stir and react at 60 °C for 2 h to obtain active sites at the edges and defect sites of the molybdenum disulfide sheets that can react with silane coupling agents. After the reaction is completed, wash with anhydrous ethanol and deionized water by centrifugation, and vacuum dry at 60 °C for 10 h to obtain activated molybdenum disulfide nanosheets. The activated molybdenum disulfide nanosheets were dispersed in 100 mL of anhydrous toluene and sonicated for 30 min under nitrogen protection. γ-isocyanate propyltriethoxysilane was added at a mass ratio of 1:0.20, and the mixture was refluxed at 80 °C for 6 h. After the reaction, the nanosheets were washed sequentially with anhydrous toluene and anhydrous ethanol, and then vacuum dried at 60 °C for 12 h to obtain modified molybdenum disulfide nanosheets M1. The obtained sample maintained the layered stacking morphology, and its scanning electron microscope image is shown below. Figure 2 , Figure 2 The modified molybdenum disulfide still maintains a layered stacked morphology, which is beneficial for it to play a layered solid lubricating role in high-load contact interfaces.
[0031] Step 2, Preparation of isocyanate silane-modified molybdenum disulfide interface-anchored polyurea grease Add 100 g of KN4016 naphthenic base oil to the reactor and heat to 80°C; under nitrogen protection, add 0.5 wt% of modified molybdenum disulfide nanosheets M1 at a total mass of 110 g of grease and stir mechanically for 30 min to uniformly disperse it in the base oil. 6.0 g of 4,4′-diphenylmethane diisocyanate was added to the above dispersion system and stirred at a constant temperature for 10 min. Then, 2.79 g of an amine compound composed of dodecylamine, ethylenediamine, and diethylenetriamine was slowly added, ensuring that the molar equivalent ratio of -NCO to -NH2 in the entire reaction system was 1.02 (the mass of 4,4′-diphenylmethane diisocyanate and the amine compound accounted for 8 wt% of the total mass of the grease). The reaction temperature was controlled at 130 °C and the reaction was carried out for 50 min, allowing the polyurea thickened network to form in situ and the modified molybdenum disulfide sheets to be anchored at the interface. After the reaction was completed, the system was heated to 175 °C and refined for 30 min, then cooled to 80 °C. 0.3 wt% of the antioxidant diphenylamine and 0.3 wt% of the rust inhibitor barium petroleum sulfonate were added, stirred evenly, degassed, and homogenized by three-roll milling to obtain the M-0.5 sample.
[0032] Examples 2-5: The difference between Examples 2-5 and Example 1 is that the amount of modified molybdenum disulfide nanosheets added in step 2 is different, namely 1.0 wt%, 1.5 wt%, 2.0 wt%, and 2.5 wt%, respectively. The rest of the operation is the same as in Example 1, and samples M-1.0, M-1.5, M-2.0, and M-2.5 are obtained.
[0033] It should be noted that in Examples 2-5, as the proportion of molybdenum disulfide nanosheets increases, the total amount of lubricating grease decreases. In the corresponding schemes, the total mass of isocyanate and amine compounds accounts for 7.95wt%, 7.91wt%, 7.87wt%, and 7.84wt% of the lubricant mass, respectively. In each example, the amounts of 4,4′-diphenylmethane diisocyanate and amine compounds are adjusted according to the corresponding molar ratios. The amounts of isocyanate are 5.43wt%, 5.40wt%, 5.37wt%, and 5.35wt%, respectively, and the amounts of amine compounds are 2.52wt%, 2.51wt%, 2.50wt%, and 2.49wt%, respectively.
[0034] Example 6: Interface-anchored polyurea grease in different base oil systems The difference between this example and Example 1 is that PAO 40 was used instead of KN4016 naphthenic base oil, and the content of modified molybdenum disulfide nanosheets M1 was 1.5 wt% (corresponding to 7.91 wt% of the mass of 4,4′-diphenylmethane diisocyanate and amine compounds, and 5.40 wt% and 2.51 wt% of the total mass of the grease, respectively). The remaining operations were the same as in Example 1, and sample M-PAO was obtained.
[0035] Example 7: The difference between this embodiment and Example 1 is that trimethylolpropane complex ester base oil was used instead of KN4016 naphthenic base oil, and the content of modified molybdenum disulfide nanosheets M1 was 1.5 wt% (the corresponding mass of 4,4′-diphenylmethane diisocyanate and amine compounds accounted for 7.91 wt% of the total mass of the grease). The remaining preparation steps were the same as in Example 1, and sample M-EST was obtained.
[0036] Examples 8-10: Interface-anchored polyurea greases of molybdenum disulfide nanosheets modified with isocyanate silane of different sheet sizes The difference between this embodiment and Example 1 is that molybdenum disulfide nanosheets with average sheet diameters of 80 nm, 200 nm and 450 nm were selected respectively, activated and modified with silane according to M1 in Example 1, and then 1.5 wt% interface anchoring polyurea grease was prepared according to the process of M-1.5 to obtain samples M-S80, M-S200 and M-S450.
[0037] Examples 11-13: Interface-anchored polyurea greases under different process parameters Unlike Example 1, 1.5 wt% of modified molybdenum disulfide nanosheets M1 were added to KN4016 naphthenic base oil and dispersed for 30 min. 4,4′-diphenylmethane diisocyanate and an amine mixture composed of dodecylamine, ethylenediamine, and diethylenetriamine were added. The in-situ polyurea reaction temperature was controlled at 110°C, 120°C, and 140°C, and the reaction time was 40 min, respectively. The refining temperature was 160°C and the refining time was 45 min, yielding samples M-T110, M-T120, and M-T140.
[0038] Comparative Example 1: Polyurea-based grease without added molybdenum disulfide The difference between this comparative example and Example 1 is that, except for the absence of molybdenum disulfide, the types and amounts of other raw materials, the reaction sequence, and the preparation process are the same as step 2 of Example 1, resulting in a polyurea-based grease without added molybdenum disulfide, denoted as BG.
[0039] Comparative Example 2: Unmodified molybdenum disulfide / polyurea grease This comparative example differs from Example 1 in that, except for replacing the modified molybdenum disulfide nanosheets with 0.5 wt%, 1.0 wt%, 1.5 wt%, 2.0 wt%, and 2.5 wt% unmodified molybdenum disulfide nanosheets, the rest of the preparation process is the same as step 2 of Example 1, yielding U-0.5, U-1.0, U-1.5, U-2.0, and U-2.5, respectively. This group of samples is used to compare the effects of conventionally physically doped molybdenum disulfide and interface-anchored molybdenum disulfide.
[0040] Comparative Example 3: Non-interface anchoring molybdenum disulfide / polyurea grease The comparative example first prepared polyurea-based grease BG according to Comparative Example 1; after the grease formation and refining were completed, 1.5 wt% of modified molybdenum disulfide nanosheets M1 prepared in step 1 of Example 1 were added at 80°C, mechanically stirred for 30 min and homogenized by three-roll milling to obtain the sample PM-1.5.
[0041] Comparative Example 4: This comparative example uses γ-aminopropyltriethoxysilane to surface-treat activated molybdenum disulfide nanosheets (activation scheme of Example 1): Specifically, the activated molybdenum disulfide nanosheets were dispersed in 100 ml of anhydrous toluene and protected with nitrogen for 30 min; γ-aminopropyltriethoxysilane was added, with a mass ratio of γ-aminopropyltriethoxysilane to molybdenum disulfide of 0.2:1; the system was heated to 80 °C and refluxed for 6 h; after the reaction was completed, the mixture was centrifuged, washed with toluene to remove unreacted silane, and dried under vacuum at 60 °C for 12 h to obtain aminosilane-modified molybdenum disulfide nanosheets; Then, following the process in step 2 of Example 1, 1.5 wt% molybdenum disulfide / polyurea grease was prepared to obtain sample N-Si-1.5.
[0042] Comparative Example 5: In this comparative example, unactivated molybdenum disulfide nanosheets were directly reacted with γ-isocyanate propyltriethoxysilane in anhydrous toluene: 2.0 g of molybdenum disulfide nanosheets were directly dispersed in 100 ml of anhydrous toluene and protected with nitrogen for 30 min; γ-isocyanate propyltriethoxysilane was added, with a mass ratio of γ-isocyanate propyltriethoxysilane to molybdenum disulfide of 0.2:1; the system was heated to 80 °C and refluxed for 6 h; after the reaction was completed, the mixture was centrifuged, washed with toluene to remove unreacted silane, and dried under vacuum at 60 °C for 12 h to obtain aminosilane-modified molybdenum disulfide nanosheets; The obtained molybdenum disulfide was used to prepare polyurea grease according to the process in step 2 of Example 1, and sample D-Si-1.5 was obtained.
[0043] Comparative Example 6: The difference between this comparative example and Example 1 is that the amount of modified molybdenum disulfide nanosheets M1 added was adjusted to 3.5 wt% (corresponding to 7.76 wt% of the mass of 4,4′-diphenylmethane diisocyanate and amine compounds in total grease). The rest of the process was the same as in Example 2, and sample M-3.5 was obtained.
[0044] The performance of the above-described embodiments and comparative examples was tested as follows: (1) Dropping point (test method refers to GB / T 3498), high-temperature isothermal viscosity change, and coefficient of friction were tested on the samples obtained in Examples 1-5 and Comparative Examples 1-2. The high-temperature viscosity change was evaluated by the apparent viscosity change under isothermal conditions of 200℃ for 60 min. The viscosity reduction rate was calculated based on the apparent viscosity change before and after isothermal conditions, and the apparent viscosity retention rate was calculated as 100% - viscosity reduction rate. The coefficient of friction was evaluated by a four-ball friction test with a test load of 392 N, a rotation speed of 1200 r / min, and a test time of 60 min. The results are listed in Table 1 and... Figures 3-5 .
[0045] Table 1. Effects of different molybdenum disulfide states and contents on the performance of polyurea grease.
[0046] From Table 1 and Figure 3 It is evident that unmodified molybdenum disulfide can reduce the coefficient of friction, but its improvement on dropping point and high-temperature structural retention is insufficient, and the dropping point decreases with increasing content. Isocyanate silane-modified molybdenum disulfide interface-anchored samples all showed increased dropping points and decreased high-temperature viscosity reduction rates within the range of 0.5-2.5 wt%. Among them, M-1.5 had a dropping point of 328℃, a viscosity reduction rate of 5.3% after being held at 200℃ for 60 min, and a coefficient of friction of 0.062. Figure 3 The results showed that the dropping point reached a relatively high level when the modified molybdenum disulfide content was 1.5 wt%. The dropping point decreased slightly after the content was further increased, indicating that an appropriate amount of interfacial anchoring sheets can enhance the polyurea network, while excessive sheets can lead to local aggregation.
[0047] Figure 4 The results showed that the viscosity decrease of the 1.5 wt% isocyanate silane-modified molybdenum disulfide sample under constant temperature of 200℃ was significantly less than that of the 1.5 wt% unmodified molybdenum disulfide sample, indicating that the interface anchoring structure is beneficial to maintaining the high-temperature stability of the polyurea thickened network.
[0048] Figure 5 The modified molybdenum disulfide sample showed a lower overall coefficient of friction than the unmodified molybdenum disulfide sample, and reached a better level around 1.5-2.0 wt%, indicating that isocyanate silane modified molybdenum disulfide has a synergistic effect in polyurea network reinforcement and layered solid lubrication.
[0049] (2) The effect of molybdenum disulfide introduction method on performance The samples obtained by different molybdenum disulfide introduction methods at a content of 1.5 wt% in Example 3 and Comparative Examples 1-6 were compared. The cone penetration (test method refers to GB / T 269) and stencil oil separation (test method refers to SH / T 0324) results are shown in Table 2.
[0050] Table 2. Effects of different molybdenum disulfide introduction methods on the performance of polyurea grease.
[0051] As shown in Table 2, the addition of modified molybdenum disulfide after lipid formation (PM-1.5 obtained in Comparative Example 3) can reduce the coefficient of friction, but its dropping point and high-temperature viscosity retention are lower than those of the in-situ interface anchoring sample (M-1.5). The performance of non-isocyanate silane modified (N-Si-1.5 obtained in Comparative Example 4) and unactivated direct silane treatment (D-Si-1.5 obtained in Comparative Example 5) are both lower than M-1.5, indicating that surface activation, isocyanate-containing silane bridging layer, and in-situ polyurea reaction jointly determine the interface anchoring effect. The performance of M-3.5 deteriorates, indicating that excessive lamellar layers can disrupt network uniformity. The colloidal stability effect is reflected by the oil separation rate of the steel mesh; the lower the oil separation rate, the better the colloidal stability. The in-situ anchored M-1.5 with modified molybdenum disulfide exhibits the best colloidal stability.
[0052] (3) The performance of the samples obtained in Examples 3 and 6-13 was tested, and the results are listed in Table 3.
[0053] Table 3. Effects of base oil, flake size, and process parameters on grease performance
[0054] As shown in Table 3, in the naphthenic mineral oil, PAO, and synthetic ester base oil systems, 1.5 wt% interface-anchored modified molybdenum disulfide can achieve high dropping points and low friction coefficients; modified molybdenum disulfide with an average flake diameter of 80-450 nm can form interface-anchored polyurea composite thickening structures; when the in-situ reaction temperature is adjusted within the range of 110-140℃, the samples still maintain good high-temperature viscosity retention and friction reduction properties.
[0055] In summary, this invention transforms ordinary molybdenum disulfide from an additive solid lubricant into isocyanate-silane-modified molybdenum disulfide, which further serves as an interface-anchored functional layer capable of participating in the formation of a polyurea thickening network. Through surface activation and isocyanate-silane modification, molybdenum disulfide forms multi-point interfacial coupling with polyurea segments during the in-situ reaction of polyurea, thereby improving the grease dropping point, high-temperature viscosity retention, and tribological properties.
[0056] Under the optimized formulation, the modified molybdenum disulfide content of 1.5 wt% exhibits superior overall performance, achieving a dropping point of 328℃, a viscosity reduction rate of 5.3% after being held at 200℃ for 60 min, and a coefficient of friction of 0.062. Compared with polyurea-based grease without added molybdenum disulfide, unmodified molybdenum disulfide / polyurea grease, samples with added modified molybdenum disulfide after grease formation, and non-isocyanate silane modified samples, the sample of this invention simultaneously demonstrates a higher dropping point, a lower high-temperature viscosity reduction rate, and a lower coefficient of friction.
[0057] This invention, through five embodiments and three comparative examples, supports the technical features such as molybdenum disulfide surface activation, isocyanate-containing silane bridging, in-situ polyurea reaction anchoring, molybdenum disulfide content range, flake diameter range, base oil type, and process parameter range. This grease is suitable for high-temperature, high-load lubrication applications such as high-temperature bearings, metallurgical rolls, high-speed motors, and heavy-duty transmission components.
Claims
1. An isocyanate silane-modified molybdenum disulfide interface-anchored polyurea grease, characterized in that, The lubricating grease is prepared using the following method and steps: Step 1: Activate molybdenum disulfide nanosheets using an activating agent. Then, react the activated molybdenum disulfide nanosheets with an isocyanate-containing alkoxysilane coupling agent in an organic solvent under an inert atmosphere and at 60–90°C to prepare modified molybdenum disulfide nanosheets. The activating agent is selected from hydrogen peroxide solution, peracetic acid aqueous solution, ozone aqueous solution, or sodium hypochlorite solution. The isocyanate-containing alkoxysilane coupling agent is selected from γ-isocyanate propyltriethoxysilane, γ-isocyanate propyltrimethoxysilane, or a combination of the two. Step 2: Modified molybdenum disulfide nanosheets are dispersed in base oil, followed by the addition of 4,4′-diphenylmethane diisocyanate and amine compounds. The mixture is then subjected to a polyurea reaction at 100–140°C. After the reaction is complete, the system is heated to 150–200°C for refining. Subsequently, the mixture is cooled, functional additives are added, degassed, and homogenized to obtain a lubricating grease. The base oil is one or more of cycloalkyl mineral oil, polyalphaolefin, and synthetic ester oil. The amine compounds are a mixture of C8-C22 aliphatic monoamines and polyamines, and the polyamines include one or more of ethylenediamine, dodecylamine, and diethylenetriamine.
2. The lubricating grease according to claim 1, characterized in that, The molybdenum disulfide nanosheets have an average diameter of 50-500 nm and a thickness of 1-30 nm.
3. The lubricating grease according to claim 1, characterized in that, The mass ratio of the activated molybdenum disulfide nanosheets to the isocyanate-containing alkoxysilane coupling agent is 1:0.05-0.
60.
4. The lubricating grease according to claim 1, characterized in that, Based on 100% of the total mass of the grease, the base oil is 70-91 wt%, the 4,4′-diphenylmethane diisocyanate and amine compounds are 8-25 wt%, the modified molybdenum disulfide nanosheets are 0.5-2.5 wt%, the functional additives are 0.1-5 wt%, and the sum of the amounts of all components is 100 wt%.
5. The lubricating grease according to claim 1, characterized in that, The modified molybdenum disulfide nanosheets comprise 1.5-2.5 wt% of the total mass of the grease.
6. The lubricating grease according to claim 1, characterized in that, The functional additives include one or more of antioxidants, rust inhibitors, extreme pressure anti-wear agents, and metal passivators.
7. The lubricating grease according to claim 1, characterized in that, The reaction time in step 1 is 4-8 h; in step S3, the polyurea reaction time is 30-90 min; and the refining time is 20-60 min.
8. The lubricating grease according to claim 1, characterized in that, The grease has a dropping point of not less than 310°C and an apparent viscosity retention rate of not less than 90% after being kept at 200°C for 60 minutes.