A batch annealing heat treatment method for preparing dc04 cold-rolled substrate from sphd hot-rolled plate adapted only to dc03

By using heating austenitization and controlled slow cooling treatment in a bell-type annealing furnace, the microstructure and texture of SPHD hot-rolled sheet were improved, solving the problem that SPHD hot-rolled sheet could not be directly converted into DC04 cold-rolled substrate. This significantly improved deep-drawing performance and met the standards of DC04 cold-rolled substrate.

CN123132575APending Publication Date: 2026-11-20GUILIN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611601020.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-16
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies make it difficult to directly convert SPHD hot-rolled plates into substrates that meet the requirements of DC04 cold-rolled substrates through conventional hot rolling processes. In particular, without changing the smelting and hot rolling front-end processes, existing methods cannot effectively improve the microstructure and texture of the substrate, resulting in unstable deep-drawing performance.

Method used

A combined heat treatment process of heating austenitization, controlled slow cooling and medium-temperature holding in a bell-type annealing furnace is adopted to complete pearlite spheroidization through the full solid solution of coarse AlN and the precipitation of nano-sized AlN particles, thereby improving the texture strength of the substrate {111}//ND.

Benefits of technology

Without changing the smelting and hot rolling front-end processes, the deep drawing performance of the substrate is significantly improved, making it meet the performance requirements of DC04 cold-rolled substrate. The process is simple to operate, low in cost, and suitable for industrial-scale application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123132575A_ABST
    Figure CN123132575A_ABST
Patent Text Reader

Abstract

This invention provides a bell-type annealing heat treatment method for preparing DC04 cold-rolled substrates from SPHD hot-rolled sheets that are only compatible with DC03, belonging to the field of metal material heat treatment technology. This invention overcomes the problem of insufficient deep-drawing performance and difficulty in stably preparing DC04 cold-rolled substrates due to the high content of C and N interstitial elements in SPHD hot-rolled sheets that are only compatible with DC03, without modifying the smelting and hot-rolling front-end processes. This invention uses hot-rolled SPHD hot-rolled sheets with high C and N interstitial element content, which are originally only suitable as DC03 cold-rolled substrates, as raw materials. In the same bell-type annealing furnace, the process involves sequentially performing austenitization at 940–980℃ for 8–15 min, controlled slow cooling at 1–3℃ / s to 610–630℃ and holding at that temperature for 30–120 min, and finally, cooling to room temperature with the furnace under a sealed inner bell. By controlling AlN solid solution and precipitation, grain structure, and texture, the treated SPHD hot-rolled sheet meets the requirements for pre-substrate use in DC04 deep-drawing cold-rolled steel sheets.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of heat treatment technology for metallic materials, and in particular to a bell-type annealing heat treatment method for preparing DC04 cold-rolled substrates from SPHD hot-rolled plates that are only compatible with DC03. Background Technology

[0002] SPHD is an ultra-low carbon deep-drawing hot-rolled steel for household appliances. Hot-rolled SPHD sheets are often used as cold-rolled substrates. However, SPHD hot-rolled sheets produced using conventional hot-rolling processes are limited by hot-rolling process parameters and metallurgical process control levels. Their initial texture, grain size, and AlN precipitate state often fail to meet the raw material requirements for higher-grade cold-rolled deep-drawing steel sheets, typically only meeting the requirements for preparing DC03 cold-rolled substrates. If such hot-rolled sheets are directly used in the production of DC04 deep-drawing cold-rolled steel sheets, due to the substrate's... 90 With low values ​​and a high proportion of unfavorable textures, the deep-drawing performance indicators are difficult to consistently meet the DC04 requirements after subsequent cold rolling, finished product annealing and leveling, resulting in a low product yield.

[0003] Further research indicates that this type of SPHD hot-rolled sheet can only stably meet the requirements of DC03 cold-rolled substrate, which is closely related to its high content of interstitial elements such as C and N. DC04 deep-drawing cold-rolled steel sheet has strict requirements for the control of interstitial elements in the substrate, typically requiring the N content to be controlled below 0.0025%; when the N content is higher than or equal to 0.0025%, it falls into the category of high N content. When the C content is high, the volume fraction of pearlite in the steel increases, which is unfavorable for the development of texture during annealing, leading to r 90 The values ​​are too low; when the N content is too high and the Als / N mass ratio is insufficient, in addition to the formation of coarse AlN, a certain amount of dissolved N will remain in the steel. Dissolved N easily causes age hardening during subsequent cold rolling and annealing processes, and inhibits the development of the {111} / / ND texture, increasing the planar anisotropy index Δr and leading to a deterioration in deep drawing performance. Furthermore, high C and N content also causes uneven grain size in the hot-rolled state, further reducing the stability of the substrate's deep drawing performance. Therefore, for SPHD hot-rolled plates with high C and N content, it is difficult to reliably obtain the microstructure and texture conditions required for DC04 cold-rolled substrates using only conventional hot rolling processes.

[0004] Existing technologies include heat treatment processes for SPHD hot-rolled sheets, which improve the deep-drawing performance of SPHD sheets through austenitization, cooling, and heat preservation. However, these technologies do not address the original goal of obtaining DC04 cold-rolled substrate material conditions for SPHD hot-rolled sheets that were only suitable for DC03 substrates. Furthermore, existing solutions lack complete process adaptation schemes for bell-type annealing furnaces. In industrial sheet production, it is difficult to achieve a synergistic matching of austenitization, controlled slow cooling, and medium-temperature AlN precipitation on bell-type annealing equipment, making it impossible to directly convert DC03 grade SPHD hot-rolled sheets into DC04 cold-rolled substrates. Improving substrate quality through front-end process optimization such as smelting and hot rolling requires modifications to production line equipment, resulting in high costs and hindering industrial application.

[0005] Therefore, without changing the original smelting and hot rolling process of SPHD hot-rolled plates, a heat treatment method relying on bell-type annealing furnace equipment is provided to adjust the hot-rolled SPHD hot-rolled plates, which were originally only applicable to DC03 cold-rolled substrates, to meet the application conditions of DC04 cold-rolled substrates, which has important industrial value. Summary of the Invention

[0006] This invention addresses SPHD hot-rolled sheets with high C and N interstitial element content, originally only suitable for DC03. Through a combined heat treatment process involving austenitization in a bell-type annealing furnace, controlled slow cooling, medium-temperature holding, and furnace cooling, coarse AlN is fully dissolved and re-precipitated as 10-30 nm nanoparticles. Simultaneously, pearlite spheroidization is achieved, effectively improving the {111} / / ND texture strength of the substrate. Thus, without altering the smelting and hot-rolling front-end processes, the SPHD hot-rolled sheet, originally only suitable as a DC03 cold-rolled substrate, is transformed into a pre-substrate meeting the requirements for DC04 deep-drawing cold-rolled steel sheets. After cold rolling, finished product annealing, and leveling, the substrate, tested according to GB / T 5027, exhibits r90≥1.6, elongation≥38%, and Δr≤0.10, meeting the performance requirements of GB / T 5213-2019 for DC04 finished products. Furthermore, the process relies on existing bell-type annealing furnace equipment, is simple to operate, low in cost, and suitable for large-scale industrial applications.

[0007] To achieve the above-mentioned technical objectives of this invention, the following technical solution is adopted:

[0008] In one aspect, the present invention provides a bell-type annealing heat treatment method for preparing DC04 cold-rolled substrates from SPHD hot-rolled plates adapted only to DC03, comprising the following steps:

[0009] (1) Furnace heating austenitization: The hot-rolled SPHD plate is placed in a bell-type annealing furnace and heated under a protective atmosphere. The plate temperature measured by the temperature measuring device arranged at a representative position of the plate is used as the control basis. After each control measuring point reaches 940-980℃, it is held in this temperature range for 8-15 minutes to fully dissolve the original coarse AlN precipitates in the steel and completely austenitize the pearlite.

[0010] (2) Controlled cooling and medium-temperature heat preservation in the furnace: After the high-temperature heat preservation is completed, the heating furnace cover is lifted off, and the plate is slowly cooled to 610-630℃ by forced air cooling at a cooling rate of 1-3℃ / s. After reaching the medium temperature range, the heating cover is re-closed, and the heating power is adjusted to maintain the temperature in this range for 30-120 minutes. This process regulates the ferrite phase transformation, so that nano-sized AlN particles are re-precipitated in the steel and the pearlite spheroidization is completed.

[0011] (3) Furnace cooling: After the medium-temperature heat preservation is completed, the heating is stopped, the inner cover of the bell-type annealing furnace is kept closed and the protective atmosphere is maintained. The SPHD hot-rolled plate is naturally cooled to room temperature with the inner cover to obtain the SPHD cold-rolled substrate that can be used to prepare DC04 deep drawing cold-rolled steel plate.

[0012] Preferably, the chemical composition of the hot-rolled SPHD sheet, by mass percentage, is: C 0.004%~0.010%, Mn 0.10%~0.35%, Si≤0.03%, P≤0.025%, S≤0.015%, Als 0.030%~0.060%, N 0.0025%~0.0050%, with the balance being iron and unavoidable impurities; and the mass ratio of Als to N is ≥6.

[0013] Preferably, after cold rolling, finished product annealing and leveling, the hot-rolled SPHD hot-rolled sheet has a particle size of 1.3 ≤ r. 90 <1.6, 34%≤elongation<38%, Δr>0.10, can only stably meet the requirements of DC03 cold-rolled substrate.

[0014] Preferably, in the hot-rolled SPHD hot-rolled plate, the average particle size of the hot-rolled AlN precipitate is >100nm.

[0015] Preferably, the thickness of the hot-rolled SPHD sheet is 1mm to 3.5mm.

[0016] Preferably, before heat treatment in step (1), rust and oil stains on the surface of the hot-rolled SPHD plate are removed, and the plate is cleaned with anhydrous ethanol and then air-dried.

[0017] Preferably, after processing in steps (2) and (3), AlN nanoparticles with a particle size of 10nm to 30nm are precipitated in the SPHD substrate; the substrate {111} / / ND texture strength is higher than that of the original SPHD hot-rolled plate of the same batch, with the same chemical composition, and not subjected to the heat treatment of this method.

[0018] More preferably, the microstructure of the treated SPHD substrate consists of ferrite and a small amount of spheroidized pearlite, with an average grain size of 20 μm to 40 μm, and precipitated AlN nanoparticles with a particle size of 10 nm to 30 nm; the SPHD cold-rolled substrate, after cold rolling, finished product annealing and leveling, is tested according to GB / T 5027: r 90 ≥1.6, elongation ≥38%, Δr≤0.10, meeting the requirements of GB / T5213-2019 for DC04.

[0019] In another aspect, this invention provides an SPHD cold-rolled substrate for DC04 deep-drawing cold-rolled steel sheet. The microstructure of the SPHD cold-rolled substrate consists of ferrite and a small amount of spheroidized pearlite, with an average grain size of 20 μm to 40 μm. AlN nanoparticles with a particle size of 10 nm to 30 nm are precipitated. The substrate's {111} / / ND texture strength is higher than that of the original SPHD hot-rolled sheet from the same batch, with the same chemical composition, and not subjected to the heat treatment method described herein. After cold rolling, finished product annealing, and leveling, the SPHD cold-rolled substrate is tested according to GB / T 5027: r 90 With an elongation of ≥1.6, an elongation of ≥38%, and Δr ≤0.10, it can be used to prepare DC04 deep-drawing cold-rolled steel sheet. The chemical composition of the SPHD cold-rolled substrate, by mass percentage, is: C 0.004%~0.010%, Mn 0.10%~0.35%, Si≤0.03%, P≤0.025%, S≤0.015%, Als 0.030%~0.060%, N 0.0025%~0.0050%, with the balance being iron and unavoidable impurities; and the mass ratio of Als to N is ≥6.

[0020] Compared with the prior art, the present invention achieves the following technical effects:

[0021] (1) This invention proposes using SPHD hot-rolled plates, which are only compatible with DC03 cold-rolled substrates, as raw materials. Through a combination of heat treatment processes including austenitization in a bell-type annealing furnace, controlled slow cooling, medium-temperature holding, and furnace cooling, coarse AlN is fully dissolved and reprecipitated as 10-30 nm nanoparticles in the ferrite phase transformation range, without changing the smelting and hot rolling front-end processes. At the same time, pearlite spheroidization is completed. The fine AlN particles effectively pin the grain boundaries, inhibit the growth of unfavorable orientation grains, significantly improve the {111} / / ND texture strength of the substrate, and overcome the adverse effects of high C and N interstitial element content on deep drawing performance.

[0022] (2) The SPHD cold-rolled substrate treated by the method of the present invention has a microstructure consisting of ferrite and a small amount of spheroidized pearlite, with an average grain size of 20 μm to 40 μm, and the AlN precipitates are refined to 10 to 30 nm; after cold rolling, finished product annealing and leveling, the substrate is tested according to GB / T 5027, r 90 With a tensile strength ≥1.6, elongation ≥38%, and Δr ≤0.10, it fully meets the performance requirements of GB / T 5213-2019 for DC04 deep-drawing cold-rolled steel sheet. Compared with untreated raw materials, r 90 The elongation increased from 1.345 to 1.638–1.696, the elongation increased from 36.82%–37.65% to 41.86%–44.52%, and the Δr decreased from >0.10 to 0.058–0.072, resulting in a significant improvement in deep-drawing performance.

[0023] (3) The method of the present invention can be realized by relying on the existing bell-type annealing furnace equipment, without the need to modify the smelting and hot rolling production line. The process is simple to operate, the production cycle is short and the cost is low, making it suitable for large-scale industrial application. Attached Figure Description

[0024] For ease of explanation, the present invention will be described in detail below with reference to specific embodiments and accompanying drawings.

[0025] Figure 1 This is a temperature-time curve of the heat treatment process of the present invention;

[0026] Figure 2 Metallographic diagram of the original SPHD hot-rolled plate that is only compatible with DC03 substrate;

[0027] Figure 3 This is a metallographic image of the SPHD substrate after heat treatment in Embodiment 1 of the present invention;

[0028] Figure 4 This is a metallographic image of the SPHD substrate after heat treatment in Embodiment 2 of the present invention;

[0029] Figure 5 This is a metallographic image of the SPHD substrate after heat treatment in Embodiment 3 of the present invention.

[0030] Figure 6 This is a flowchart of the SPHD hot-rolled plate cover-type annealing process of the present invention. Detailed Implementation

[0031] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention. However, the present invention is not limited to these embodiments. In the following description, specific details such as specific configurations are provided only to help to fully understand the embodiments of the present invention.

[0032] Example 1

[0033] This embodiment provides a bell-type annealing heat treatment method for preparing DC04 cold-rolled substrates from SPHD hot-rolled plates that are only compatible with DC03, specifically including the following steps:

[0034] (a) Raw material preparation

[0035] The raw material is selected as a hot-rolled SPHD sheet with a thickness of 3.5 mm. This material has a high C and N content and a limited Al / N mass ratio; without the processing described in this invention, it can only be used as a DC03 cold-rolled substrate.

[0036] The chemical composition by mass percentage is as follows: C 0.006%, Mn 0.19%, Si 0.005%, P 0.009%, Ni 0.003%, Cr 0.008%, Als 0.047%, N 0.0035%, TO 0.0015%, with the balance being iron and unavoidable impurities; the Als / N mass ratio is 13.4.

[0037] The original hot-rolled microstructure consists of ferrite and a small amount of pearlite, with an average AlN precipitate particle size of approximately 180 nm.

[0038] Original untreated properties: After cold rolling, finished product annealing and leveling, the original SPHD hot-rolled sheet can be tested according to GB / T 5027 to obtain r 90 =1.345, elongation 36.82%~37.65%, Δr>0.10, only meets the requirements of DC03 finished product.

[0039] (ii) Surface pretreatment

[0040] Hot-rolled SPHD samples were cleaned by mechanical grinding or pickling to remove surface rust, then by alkaline degreasing agent to remove surface oil, followed by cleaning with anhydrous ethanol and air drying for later use. This ensured uniform heating of the plate surface during the heat treatment process and prevented surface defects from affecting the microstructure evolution.

[0041] (iii) Furnace heating austenitization

[0042] The hot-rolled plate is placed in a bell-type annealing furnace and heated to 960℃ under a protective atmosphere, then held for 8 minutes. This allows the original coarse AlN precipitates in the steel to be fully dissolved, and the pearlite to be completely austenitized. The holding time should not be too long to avoid excessive coarsening of the austenite grains.

[0043] (iv) Controlled slow cooling and medium-temperature heat preservation inside the furnace

[0044] After the heat preservation is completed, the heating furnace cover is lifted off the plate. The plate is then slowly cooled to 620°C by forced air cooling at a cooling rate of 1.5°C / s. After reaching 620°C, the heating cover is re-fastened, the heating power is adjusted, and the plate is kept at this temperature for 60 minutes to allow the ferrite phase transformation to proceed fully. Nanoscale AlN particles are then re-precipitated in the ferrite phase transformation range, while pearlite spheroidization is completed.

[0045] (v) Furnace cooling

[0046] After the heat preservation is completed, heating is stopped, and the inner cover of the bell-type annealing furnace is kept closed. The SPHD hot-rolled plate is naturally cooled to room temperature with the inner cover, and an SPHD cold-rolled substrate that can be used to prepare DC04 deep-drawing cold-rolled steel plate is obtained.

[0047] (vi) Performance testing

[0048] Microstructural observation of the treated SPHD substrate and mechanical property testing of the cold-rolled finished product were performed. The results are as follows: the microstructure consists of ferrite + a small amount of spheroidized pearlite, with an average grain size of 35 μm; the precipitated AlN particles have a diameter of 10–30 nm; after cold rolling, annealing, and leveling, the treated SPHD substrate can be tested according to GB / T 5027 to obtain r 90 =1.638; elongation 41.86%~42.74%; Δr=0.072. This substrate can be used as a pre-mount substrate for DC04 deep-drawing cold-rolled steel sheets.

[0049] Example 2

[0050] This embodiment provides a bell-type annealing heat treatment method for preparing DC04 cold-rolled substrates from SPHD hot-rolled plates that are only compatible with DC03, specifically including the following steps:

[0051] (a) Raw material preparation

[0052] The raw material is the same as in Example 1, which is a hot-rolled SPHD sheet with a thickness of 3.5 mm and a relatively high C and N content. It was originally only suitable for DC03 cold-rolled substrate. The chemical composition is the same as in Example 1: C 0.006%, N 0.0035%, Als 0.047%, and the Als / N mass ratio is 13.4. The original hot-rolled microstructure is ferrite and a small amount of pearlite, and the average particle size of the AlN precipitate is about 180 nm.

[0053] (ii) Surface pretreatment

[0054] Same as in Example 1, remove surface rust and oil, clean with anhydrous ethanol and air dry.

[0055] (iii) Furnace heating austenitization

[0056] The hot-rolled plate was placed in a bell-type annealing furnace and heated to 940°C under a protective atmosphere. It was held for 8 minutes to complete austenitization and fully dissolve coarse AlN.

[0057] (iv) Controlled slow cooling and medium-temperature heat preservation inside the furnace

[0058] The plate is lifted off the heating furnace cover and slowly cooled to 620°C by forced air cooling at a rate of 1.5°C / s. After reaching 620°C, the heating cover is reattached, the heating power is adjusted, and the plate is held at this temperature for 60 minutes to complete the ferrite phase transformation, AlN nanoparticle re-precipitation, and pearlite spheroidization.

[0059] (v) Furnace cooling

[0060] Stop heating, keep the inner cover closed, and let the SPHD hot-rolled plate cool to room temperature with the furnace to obtain the SPHD cold-rolled substrate for DC04.

[0061] (vi) Performance testing

[0062] The microstructure consists of ferrite with a small amount of spheroidized pearlite, with an average grain size of 20 μm; the precipitated AlN particles have a diameter of 10–30 nm; after cold rolling, final annealing, and leveling, the treated SPHD substrate can be tested according to GB / T 5027 to obtain r 90 =1.696; elongation 43.58%~44.52%; Δr=0.058. The substrate obtained in this embodiment has the best texture and mechanical properties, and fully meets the raw material conditions for the DC04 deep-drawing cold-rolled steel sheet pre-substrate.

[0063] Example 3

[0064] This embodiment provides a bell-type annealing heat treatment method for preparing DC04 cold-rolled substrates from SPHD hot-rolled plates that are only compatible with DC03, specifically including the following steps:

[0065] (a) Raw material preparation

[0066] The raw material is the same as in Example 1, a hot-rolled SPHD sheet with a thickness of 3.5 mm and a relatively high C and N content. It was originally only suitable for DC03 cold-rolled substrate. The chemical composition is the same as in Example 1: C 0.006%, N 0.0035%, Als 0.047%, Als / N mass ratio 13.4; the original hot-rolled microstructure is ferrite and a small amount of pearlite, and the average particle size of the AlN precipitates is about 180 nm.

[0067] (ii) Surface pretreatment

[0068] Same as in Example 1, remove surface rust and oil, clean with anhydrous ethanol and air dry.

[0069] (iii) Furnace heating austenitization

[0070] The hot-rolled plate is placed in a bell-type annealing furnace and heated to 940°C under a protective atmosphere. It is held for 10 minutes to complete austenitization and fully dissolve coarse AlN.

[0071] (iv) Controlled slow cooling and medium-temperature heat preservation inside the furnace

[0072] The plate is lifted off the heating furnace cover and slowly cooled to 620°C by forced air cooling at a cooling rate of 1.5°C / s. After reaching 620°C, the heating cover is reattached, the heating power is adjusted, and the plate is held at this temperature for 60 minutes to complete the ferrite phase transformation, AlN nanoparticle re-precipitation, and pearlite spheroidization.

[0073] (v) Furnace cooling

[0074] Stop heating, keep the inner cover closed, and let the SPHD hot-rolled plate cool to room temperature with the furnace to obtain the SPHD cold-rolled substrate for DC04.

[0075] (vi) Performance testing

[0076] The microstructure consists of ferrite with a small amount of spheroidized pearlite, with an average grain size of 24 μm; the precipitated AlN particles have a diameter of 10–30 nm; after cold rolling, final annealing, and leveling, the treated SPHD substrate can be tested according to GB / T 5027 to obtain r 90 =1.662; elongation 43.12%~43.86%; Δr=0.064. The substrate obtained in this embodiment meets the raw material conditions of DC04 cold-rolled substrate.

[0077] Comparative Example

[0078] The same hot-rolled SPHD sheet as in Example 1 was used directly as a cold-rolled substrate without undergoing the heat treatment of this invention. The raw material had a C content of 0.006%, a N content of 0.0035%, an Als / N mass ratio of 13.4, and the original hot-rolled microstructure consisted of ferrite and a small amount of pearlite, with an average AlN precipitate particle size of approximately 180 nm.

[0079] Performance testing: After cold rolling, finished product annealing and leveling, the original SPHD hot-rolled sheet can be tested according to GB / T 5027 to obtain r. 90 =1.345, elongation 36.82%~37.65%, Δr>0.10; untreated SPHD hot-rolled plates can only be used as DC03 cold-rolled substrates. When used directly in the production of DC04 cold-rolled plates, the performance of the finished products after subsequent cold rolling and annealing cannot stably meet the requirements of DC04.

[0080] Comparative Analysis of Examples and Comparative Cases

[0081] As can be seen from the comparison of Examples 1-3 and the comparative examples, this invention, through a bell-type annealing furnace and associated heat treatment process, transforms the original hot-rolled SPHD sheet, which is only compatible with DC03, into a DC04 cold-rolled substrate. After cold rolling, finished product annealing, and leveling, the substrate is tested according to GB / T 5027 to obtain r. 90 The value increased from 1.345 to 1.638–1.696, the elongation increased from 36.82%–37.65% to 41.86%–44.52%, Δr decreased from >0.10 to 0.058–0.072, the {111} / / ND texture strength was significantly improved, the AlN nanoparticles changed from a coarse precipitate phase of about 180 nm in the hot-rolled state to a dispersed precipitate of 10–30 nm, the microstructure became more homogenized, and the pearlite was spheroidized.

[0082] This invention addresses the issue of high C and N interstitial element content and limited Als / N mass ratio in SPHD hot-rolled sheets. It utilizes furnace heating for austenitization to fully dissolve coarse AlN, followed by controlled slow cooling and medium-temperature holding in the furnace to allow AlN to re-precipitate as 10-30 nm nanoparticles, simultaneously achieving pearlite spheroidization. This effectively overcomes the adverse effects of high C and N content on the {111} / / ND texture. After cold rolling, final annealing, and leveling, the treated SPHD substrate can be tested according to GB / T 5027 to obtain r 90 With an elongation of ≥1.6 and an elongation of ≥38%, it meets the performance requirements of DC04 finished products in GB / T 5213-2019 and Δr≤0.10, enabling the SPHD hot-rolled plate, which was originally only compatible with DC03, to be used as a pre-cold-rolled substrate for DC04 deep-drawing cold-rolled steel plates.

[0083] Those skilled in the art to which this application pertains may modify or supplement the specific embodiments described or use similar methods to replace them, but without departing from the inventive concept of this application or exceeding the scope defined by the appended claims.

Claims

1. A bell-type annealing heat treatment method for preparing DC04 cold-rolled substrates from SPHD hot-rolled plates adapted only to DC03, characterized in that, Includes the following steps: (1) Furnace heating austenitization: The hot-rolled SPHD plate is placed in a bell-type annealing furnace and heated under a protective atmosphere. The plate temperature measured by the temperature measuring device arranged at a representative position of the plate is used as the control basis. After each control measuring point reaches 940-980℃, it is held in this temperature range for 8-15 minutes to fully dissolve the original coarse AlN precipitates in the steel and completely austenitize the pearlite. (2) Controlled cooling and medium-temperature heat preservation in the furnace: After the high-temperature heat preservation is completed, the heating furnace cover is lifted off, and the plate is slowly cooled to 610-630℃ by forced air cooling at a cooling rate of 1-3℃ / s. After reaching the medium temperature range, the heating cover is re-closed, and the heating power is adjusted to maintain the temperature in this range for 30-120 minutes. This process regulates the ferrite phase transformation, so that nano-sized AlN particles are re-precipitated in the steel and the pearlite spheroidization is completed. (3) Furnace cooling: After the medium-temperature heat preservation is completed, the heating is stopped, the inner cover of the bell-type annealing furnace is kept closed and the protective atmosphere is maintained. The SPHD hot-rolled plate is naturally cooled to room temperature with the inner cover to obtain the SPHD cold-rolled substrate that can be used to prepare DC04 deep drawing cold-rolled steel plate.

2. The method according to claim 1, characterized in that, The chemical composition of the hot-rolled SPHD sheet, by mass percentage, is as follows: C 0.004%~0.010%, Mn 0.10%~0.35%, Si≤0.03%, P≤0.025%, S≤0.015%, Als0.030%~0.060%, N 0.0025%~0.0050%, with the balance being iron and unavoidable impurities; and the mass ratio of Als to N is ≥6.

3. The method according to claim 1, characterized in that, After cold rolling, finishing annealing, and leveling, the hot-rolled SPHD sheet has a yield of 1.3 ≤ r. 90 <1.6, 34%≤elongation<38%, Δr>0.10, can only stably meet the requirements of DC03 cold-rolled substrate.

4. The method according to claim 1, characterized in that, In the hot-rolled SPHD hot-rolled plate, the average particle size of the hot-rolled AlN precipitate is >100nm.

5. The method according to claim 1, characterized in that, The thickness of the hot-rolled SPHD sheet is 1mm to 3.5mm.

6. The method according to claim 1, characterized in that, Step (1) Before heat treatment, remove rust and oil stains from the surface of hot-rolled SPHD hot-rolled plate, clean with anhydrous ethanol and air dry.

7. The method according to claim 1, characterized in that, After processing in steps (2) and (3), AlN nanoparticles with a particle size of 10nm to 30nm are precipitated in the SPHD substrate; the substrate {111} / / ND texture strength is higher than that of the original SPHD hot-rolled plate of the same batch, with the same chemical composition, and not subjected to this heat treatment method.

8. The method according to claim 1, characterized in that, The microstructure of the SPHD substrate after treatment consists of ferrite and a small amount of spheroidized pearlite, with an average grain size of 20 μm to 40 μm and AlN nanoparticles with a particle size of 10 nm to 30 nm precipitated.

9. An SPHD cold-rolled substrate for DC04 deep-drawing cold-rolled steel sheet, characterized in that, The SPHD cold-rolled substrate is prepared by any one of claims 1 to 8; the microstructure of the SPHD cold-rolled substrate consists of ferrite and a small amount of spheroidized pearlite, with an average grain size of 20 μm to 40 μm, and AlN nanoparticles with a particle size of 10 nm to 30 nm are precipitated. The substrate {111} / / ND texture strength is higher than that of the original SPHD hot-rolled plate of the same batch, with the same chemical composition, and not subjected to the heat treatment of this method.

10. The SPHD cold-rolled substrate according to claim 9, characterized in that, The chemical composition of the SPHD cold-rolled substrate, by mass percentage, is as follows: C 0.004%~0.010%, Mn 0.10%~0.35%, Si≤0.03%, P≤0.025%, S≤0.015%, Als 0.030%~0.060%, N 0.0025%~0.0050%, with the balance being iron and unavoidable impurities; and the mass ratio of Als to N is ≥6.