A high-precision seamless stainless steel pipe preparation process based on deformation-induced phase transformation strengthening

By employing a gradient nanotwin structure preparation process, and using a combination of hot extrusion, two-pass large deformation cold rolling, pickling without intermediate pickling and small deformation cold drawing, and bright annealing, the problems of improper distribution of cold rolling and cold drawing deformation, insufficient residual stress and dimensional stability, and difficulty in surface quality control in the production of seamless stainless steel tubes have been solved, thus achieving high-precision and high-efficiency production.

CN123132584APending Publication Date: 2026-11-20JIANGYIN SOUTH STAINLESS STEEL PIPES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611578946.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing seamless stainless steel pipe manufacturing processes face problems such as improper distribution of deformation during cold rolling and cold drawing, insufficient residual stress and dimensional stability, difficulty in surface quality control, and low number of process steps and production efficiency when manufacturing high-precision pipes. In particular, it is difficult to achieve coordinated control of large deformation and dimensional accuracy during cold working.

Method used

The preparation process using a gradient nanotwin structure involves a combination of hot extrusion, two-pass large deformation cold rolling, pickling without intermediate pickling and small deformation cold drawing, and bright annealing. The large deformation forming of the cold rolling mill and the finishing effect of cold drawing, combined with intermediate solution treatment and bright annealing, eliminate work hardening and residual stress, ensuring surface quality.

Benefits of technology

It achieves high-precision seamless stainless steel pipes with an outer diameter tolerance of ±0.08mm, a wall thickness tolerance of ±0.05mm, a wall thickness uniformity of ±5%, a surface roughness Ra≤0.4μm, and a residual stress absolute value not exceeding 50MPa, significantly improving production efficiency and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The application discloses a high-precision seamless stainless steel pipe preparation process based on deformation-induced phase change strengthening and belongs to the technical field of metal pipe manufacturing. The process adopts hot extrusion to prepare a rough pipe and carries out solid solution treatment within 30 seconds; after first-pass cold rolling, the wall thickness reduction is 30%-45% of the wall thickness of the rough pipe; after intermediate solid solution treatment, second-pass cold rolling is carried out, and the wall thickness reduction is 25%-35% of the current wall thickness; then, short mandrel finished cold drawing is carried out, and the wall thickness reduction is controlled to be 0.3-0.8 mm; finally, bright annealing is carried out at a temperature of 1050-1080 DEG C and under a reducing atmosphere with a dew point of not more than -40 DEG C. Through the process configuration of "large deformation cold rolling for wall and diameter fixing and small deformation cold drawing for final finishing", the process pass is reduced, the outer diameter tolerance of the finished pipe is not more than ±0.08 mm, the wall thickness uniformity is not more than ±5%, the outer surface roughness is not more than 0.4 microns, and the absolute value of residual stress is not more than 50 MPa, so that the size precision, surface quality and mechanical properties are synergistically improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal pipe manufacturing technology, specifically to a process for preparing seamless stainless steel pipes, and more particularly to a method for preparing seamless stainless steel pipes with high dimensional accuracy and excellent mechanical properties through the coordinated control of cold working deformation and heat treatment. Background Technology

[0002] Seamless stainless steel pipes are widely used in petrochemical, nuclear power, medical equipment, precision instruments, aerospace, and semiconductor equipment industries due to their excellent corrosion resistance, good mechanical properties, and smooth inner and outer surfaces. With the increasing demands for pipe precision in these fields, the demand for high-precision seamless stainless steel pipes with an outer diameter tolerance within ±0.1mm, a wall thickness uniformity within ±5%, and a surface roughness Ra≤0.4μm is growing rapidly.

[0003] Currently, the mainstream production process for seamless stainless steel pipes includes a combination of hot extrusion (or hot rolling) billet preparation and subsequent cold rolling / cold drawing finishing. Hot extrusion deforms the metal under triaxial compressive stress, which is beneficial for obtaining a dense microstructure and good internal and external surface quality, and is a common method for manufacturing stainless steel pipe billets. The hot-extruded billets typically require multiple passes of cold rolling and / or cold drawing, combined with intermediate heat treatment, to gradually reduce the wall thickness and diameter to the finished product size.

[0004] However, existing processes face several technical challenges in manufacturing high-precision seamless stainless steel tubes.

[0005] First, there is the issue of deformation distribution in cold rolling and cold drawing processes. Cold rolling and cold drawing are crucial steps in controlling the dimensional accuracy and surface quality of finished tubes. Cold rolling mills (such as two-roll or multi-roll cold rolling mills) can achieve significant wall and diameter reductions in a single pass, and the metal is under triaxial compressive stress during rolling, which is beneficial for grain refinement and microstructure improvement. Cold drawing, on the other hand, uses simpler equipment and has lower die costs, but the metal is subjected to tensile stress during drawing, limiting the deformation per pass and easily generating residual stress. Taking a conventional combined cold rolling and cold drawing process as an example, the wall reduction per pass is usually controlled within a small range (e.g., 0.5–1 mm) to avoid excessive work hardening leading to cracking or dimensional deviations. However, this small deformation strategy means that more intermediate passes and intermediate heat treatments are required, resulting in a long process cycle, high energy consumption, and difficulty in effectively eliminating accumulated dimensional deviations. Furthermore, stainless steel has a significant tendency for work hardening during cold working, especially austenitic stainless steel, which has high deformation resistance and limited deformation per pass, further restricting the balance between production efficiency and precision control.

[0006] Secondly, there are issues related to residual stress and dimensional stability. For tubes with high precision requirements (such as precision tubes with an outer diameter tolerance within ±0.1mm and stringent requirements for wall thickness uniformity), conventional cold rolling-cold drawing routes often leave some dimensional fluctuations and residual stress in the final pass, leading to slight deformation of the finished product during subsequent use or storage, resulting in insufficient precision stability. Sources of residual stress include: macroscopic residual stress caused by uneven deformation during cold working, microscopic residual stress caused by work hardening, and residual stress caused by thermal stress during cooling after heat treatment. While existing technologies include adding polishing processes to improve surface roughness, this does not solve the problems of dimensional accuracy and residual stress. There are also methods to reduce residual stress by adding stress-relief annealing processes, but this increases the number of process passes and energy consumption.

[0007] Third, there is the issue of surface quality control. During the cold drawing process, friction between the tube and the die can cause surface scratches, roughening, and other defects, affecting surface roughness. In conventional processes, pickling is required after cold drawing to remove oxide scale and surface defects. However, pickling introduces the risk of hydrogen embrittlement, and the treatment of pickling wastewater poses environmental challenges. For high-precision tubes, the surface quality after pickling fluctuates significantly, making it difficult to consistently meet the requirement of Ra≤0.4μm.

[0008] Fourth, the contradiction between the number of processing steps and production efficiency. Conventional cold rolling-cold drawing combined processes typically require 3 to 5 cold working steps and 2 to 3 intermediate heat treatments, resulting in a long process flow, large equipment requirements, and low production efficiency. How to reduce the number of processing steps without sacrificing precision and performance has been a long-term goal in this field.

[0009] To address the aforementioned issues, some improvements have been attempted in existing technologies. For example, one solution proposes using a high-speed cold rolling mill to increase the deformation per pass, but the increase in wall reduction is limited by equipment capacity and die life. Another solution proposes using a warm rolling process to reduce deformation resistance, but warm rolling temperature control is complex and may cause sensitization and other problems. Yet another solution proposes lubrication treatment before cold drawing to improve surface quality, but this cannot fundamentally solve the problems of dimensional accuracy and residual stress.

[0010] Therefore, there is a need for a seamless stainless steel tube manufacturing process that can achieve coordinated control of large deformation cold working and dimensional accuracy, while effectively regulating residual stress and surface quality, without significantly increasing the number of passes. Summary of the Invention

[0011] The first objective of this invention is to provide a manufacturing process for seamless stainless steel tubes with a gradient nanotwin structure, in order to solve the technical problems in the prior art, such as limited deformation in cold working passes, difficulty in balancing dimensional accuracy and processing efficiency, high residual stress, and large fluctuations in surface quality.

[0012] A fabrication process for a seamless stainless steel tube with a gradient nanotwin structure includes the following steps:

[0013] Step S1, tube blank preparation: stainless steel blanks are prepared by hot extrusion process. The heating temperature of the hot extruded blank is 1130~1180℃, and solution treatment is carried out within 30 seconds after extrusion.

[0014] In step S1, the billet heating temperature before hot extrusion is selected as 1130–1180℃. This temperature range balances the deformation resistance and microstructure uniformity of austenitic stainless steel. Below 1130℃, the deformation resistance is too high, the extrusion load is high, and insufficient temperature may lead to microstructure inhomogeneity. Above 1180℃, the tendency for grain coarsening increases, and high-temperature oxidation and burn-off intensifies. Solution treatment is performed within 30 seconds after extrusion to utilize the residual heat of extrusion for rapid solution treatment, preventing carbide precipitation and grain coarsening. If the treatment exceeds 30 seconds, the pipe temperature drops below the sensitization range, and carbides precipitate along grain boundaries, easily initiating cracks during subsequent cold working.

[0015] Step S2, First pass of cold rolling: The rough tube is cold rolled, and the wall thickness reduction is controlled to be 30% to 45% of the rough tube wall thickness, and the diameter reduction is 12% to 20% of the outer diameter;

[0016] In step S2, the first cold rolling pass employs a large deformation strategy. The wall reduction is controlled at 30%–45% of the rough tube wall thickness. This range effectively eliminates uneven wall thickness and surface defects left over from hot extrusion, while preventing excessive deformation from causing rolling load overload or tube cracking. The diameter reduction is controlled at 12%–20%, coordinated with the wall reduction to ensure uniform metal flow during rolling. If the wall reduction is less than 30%, the hot extrusion defects will not be sufficiently eliminated, making it difficult to compensate in subsequent passes; if it is greater than 45%, the rolling force will increase sharply, exacerbating wear on the mandrel and rolls, and potentially causing cracks on the inner surface of the tube.

[0017] Step S3, intermediate heat treatment: The tube after the first cold rolling is subjected to solution treatment, the heating temperature is 1040~1100℃, the holding time is controlled according to the wall thickness 2~3min / mm, and then water quenching is performed.

[0018] In step S3, the purpose of the intermediate solution treatment is to eliminate the work hardening generated in the first cold rolling pass, restore the plasticity and toughness of the austenitic structure, and provide a microstructure with low deformation resistance for the second cold rolling pass. The heating temperature is 1040–1100℃. Below 1040℃, the solution treatment is insufficient, and the work hardening is not completely eliminated; above 1100℃, the tendency for grain coarsening increases. The holding time is controlled at 2–3 min / mm of wall thickness to ensure uniform temperature between the core and surface of the tube. Water quenching provides rapid cooling, which can suppress carbide precipitation and obtain a supersaturated austenitic structure.

[0019] Step S4, Second Cold Rolling: The tube after intermediate heat treatment is subjected to a second cold rolling, with the wall thickness reduction controlled at 25% to 35% of the current wall thickness and the diameter reduction controlled at 8% to 15% of the current outer diameter;

[0020] In step S4, the second cold rolling pass continues to use a larger deformation amount, but the ratio of wall reduction to diameter reduction is adjusted compared to the first pass. The wall reduction is controlled at 25%–35% of the current wall thickness, and the diameter reduction is controlled at 8%–15% of the current outer diameter. The purpose of this configuration is to further improve wall thickness uniformity and surface quality while further reducing wall thickness and diameter to approach the finished product size. If the wall reduction is less than 25%, the deformation amount in the second pass is insufficient, and the improvement in wall thickness uniformity is limited; if it is greater than 35%, the deformation amount is too large, the work hardening degree is too high, which is not conducive to subsequent cold drawing.

[0021] Step S5, finished product cold drawing: The tube after the second cold rolling is cold drawn in the finished product stage, using a short mandrel, controlling the wall reduction to be 0.3-0.8 mm and the diameter reduction to be 3%-6% of the outer diameter;

[0022] In step S5, the finished product cold drawing adopts a small deformation strategy, with a wall reduction of only 0.3–0.8 mm. The purpose of this step is no longer "forming" but "sizing" and "surface finishing." The work hardening resulting from small deformation cold drawing is extremely low, the springback of the tube is controllable, and the dimensional accuracy is significantly better than in traditional processes where cold drawing passes involve larger deformations. When the wall reduction is less than 0.3 mm, the sizing effect of cold drawing is insufficient, and the surface finishing effect is limited; when it is greater than 0.8 mm, the work hardening increases, residual stress rises, and surface quality decreases.

[0023] Step S6, Finished product heat treatment: Bright annealing is performed on the cold-drawn finished tube. The annealing temperature is 1050~1080℃, and the holding time is controlled according to the wall thickness of 1.5~2.5min / mm. The atmosphere in the furnace is hydrogen or a reducing atmosphere of decomposed ammonia, and the dew point is controlled below -40℃.

[0024] In this process, no intermediate straightening or pickling process other than intermediate heat treatment is performed between the first cold rolling pass and the second cold rolling pass.

[0025] In step S6, the purpose of bright annealing is to complete recrystallization, eliminate work hardening, and regulate residual stress while maintaining a smooth surface. The annealing temperature is 1050–1080℃. Below 1050℃, recrystallization is incomplete, and residual stress is not sufficiently eliminated; above 1080℃, grains coarsen, and mechanical properties decrease. The holding time is controlled at 1.5–2.5 min / mm of wall thickness, shorter than the intermediate heat treatment time, to avoid excessive grain growth. A reducing atmosphere (hydrogen or decomposed ammonia) and a low dew point (≤-40℃) ensure that the inner and outer surfaces of the pipe do not oxidize, and a smooth surface can be obtained without pickling after annealing.

[0026] In this process, no intermediate straightening or pickling process other than intermediate heat treatment is performed between the first cold rolling pass and the second cold rolling pass.

[0027] The core concept of the above process lies in concentrating the total deformation in two cold rolling passes. Leveraging the advantages of cold rolling mills in achieving large wall and diameter reductions, the main forming task is completed in fewer passes. A final sizing and surface finishing process is then achieved through a single pass of small-deformation cold drawing. This process configuration of "large-deformation cold rolling for wall and diameter sizing, and small-deformation cold drawing for final finishing" is fundamentally different from the conventional approach of "cold rolling as the main process and cold drawing as a supplementary process," where the wall reduction during cold drawing is controlled within a relatively large range (e.g., 0.5–1 mm or more).

[0028] Specifically, in step S2, the first cold rolling pass uses a two-roll cold rolling mill with a rolling speed of 40-60 times / minute and a feed rate of 3-6 mm / pass.

[0029] Specifically, in step S4, the second cold rolling is performed using a two-roll cold rolling mill with a rolling speed of 50-70 times / minute and a feed rate of 2-5 mm / time.

[0030] Specifically, in step S5, the drawing speed of the finished product cold drawing is 0.5 to 1.5 m / min.

[0031] Specifically, in step S5, the outer mold of the finished product cold-drawn is made of YG8 cemented carbide.

[0032] Specifically, in step S6, the furnace pressure during bright annealing is maintained at a slightly positive pressure of 5-15 Pa gauge pressure.

[0033] Specifically, in step S6, the dew point of the reducing atmosphere is controlled between -40°C and -60°C.

[0034] Specifically, the stainless steel is 304 austenitic stainless steel, 316L austenitic stainless steel, or 321 austenitic stainless steel.

[0035] Specifically, in step S2, the wall thickness reduction is 35% to 42% of the rough pipe wall thickness, and the diameter reduction is 14% to 18% of the outer diameter; in step S4, the wall thickness reduction is 28% to 33% of the current wall thickness, and the diameter reduction is 10% to 13% of the current outer diameter.

[0036] The second objective of this invention is to provide a seamless stainless steel tube manufactured using the aforementioned high-precision seamless stainless steel tube preparation process based on deformation-induced phase transformation strengthening. The seamless stainless steel tube has an outer diameter tolerance not exceeding ±0.08 mm, a wall thickness tolerance not exceeding ±0.05 mm, a wall thickness uniformity not exceeding ±5%, an outer surface roughness Ra ≤ 0.4 μm, an inner surface roughness Ra ≤ 1.6 μm, and a residual stress absolute value not exceeding 50 MPa.

[0037] The advantages of the high-precision seamless stainless steel tube manufacturing process based on deformation-induced phase transformation strengthening of the present invention compared with the prior art are as follows:

[0038] (1) Synergistic improvement of precision control and efficiency: This invention arranges the large-deformation cold rolling pass in the first step and the small-deformation cold drawing pass in the last step. This allows the large deformation of the first cold rolling pass to quickly approach the finished size and eliminate the wall thickness unevenness left by hot extrusion, while the last cold drawing pass only undertakes a very small wall reduction (0.3-0.8 mm). Its purpose is no longer "forming" but "sizing" and "surface finishing". The work hardening caused by the small-deformation cold drawing is extremely low, the springback of the tube is controllable, and the dimensional accuracy is significantly better than that of the traditional process where the cold drawing pass undertakes a large deformation. At the same time, since the main deformation is completed efficiently by cold rolling, the total number of passes is reduced.

[0039] (2) Effective control of residual stress: The intermediate solution treatment between the two cold rolling passes eliminates the work hardening of the first pass, allowing the second pass to be rolled under large deformation resistance, thus avoiding uneven deformation and residual stress concentration caused by cumulative work hardening. After the final small deformation cold drawing, bright annealing is performed. The annealing temperature range (1050~1080℃) and reducing atmosphere (dew point ≤-40℃) ensure that no oxidation occurs on the inner and outer surfaces of the tube. The cooling process after annealing is carried out in an oxygen-free environment, eliminating the surface quality fluctuations and hydrogen embrittlement risks that may be introduced by the traditional pickling process.

[0040] (3) Comprehensive assurance of surface quality: After the first cold rolling of the hot-extruded tube, the original defects on the inner and outer surfaces (such as micro-cracks and oxide scale indentation that may be generated by hot extrusion) are effectively eliminated or healed by the large deformation rolling. The second cold rolling further reduces the surface roughness. The minimal wall reduction of the final cold drawing, combined with the cemented carbide outer die, plays a final finishing role, so that the surface roughness of the finished product reaches Ra≤0.4μm, which can meet the requirements of most precision application scenarios without additional polishing processes.

[0041] (4) Refinement of microstructure and optimization of mechanical properties: Through the combination of two large deformation cold rolling passes and intermediate solution treatment, the tube is in a solution state with low deformation resistance before each cold rolling pass. During the rolling process, dynamic recrystallization and deformation-induced phase transformation work together to obtain a uniform and fine grain structure. Finally, bright annealing completes static recrystallization, and the grain size can reach grade 7-8. The fine grain structure improves both strength and plasticity, so that the finished tube has excellent elongation while maintaining high strength. Detailed Implementation

[0042] The present invention will be further illustrated below with reference to specific embodiments. These embodiments are for illustrative purposes only and do not constitute a limitation on the scope of protection of the present invention. Experimental methods not specifically described in the embodiments are generally performed under conventional conditions or as recommended by the manufacturer. Unless otherwise specified, the materials and reagents used in the embodiments are commercially available.

[0043] Example 1

[0044] Target product: Seamless 304 austenitic stainless steel tube with an outer diameter of Φ60mm and a wall thickness of 3.5mm.

[0045] Step S1: Select 304 stainless steel billet smelted in an electric furnace using AOD (Alternating Current Method). Its chemical composition by mass percentage is: C 0.045%, Si 0.42%, Mn 1.15%, P 0.028%, S 0.002%, Cr 18.25%, Ni 8.12%, with the balance being Fe and unavoidable impurities. After radial forging and machining, the billet is machined with a through hole in a center. It is then preheated to 850℃ in a ring furnace, followed by medium-frequency induction heating to 1150℃. After lubrication with glass powder, it undergoes hot extrusion to a specification of Φ89×6mm. The billet is then solution-treated in water within 28 seconds of extrusion.

[0046] Step S2: After straightening and pickling, the rough tube undergoes its first cold rolling pass on an LG-60 two-roll cold rolling mill. The rolling speed is 50 passes / minute, and the feed rate is 4 mm / pass. The final dimensions are Φ76×4.2 mm. The wall thickness reduction is 1.8 mm (30% of the rough tube's wall thickness), and the diameter reduction is 13 mm (14.6% of the rough tube's outer diameter).

[0047] Step S3: The pipe is fed into a continuous roller hearth solution furnace, heated to 1080℃, and held for 12.6 minutes (4.2mm × 3min / mm) based on the wall thickness. It is then water-quenched after exiting the furnace.

[0048] Step S4: Perform a second cold rolling pass on the LG-60 cold rolling mill. Rolling speed: 60 passes / minute, feed rate: 3mm / pass. The final dimensions are Φ66×3.8mm. Wall thickness reduction: 0.4mm (9.5% of current wall thickness), diameter reduction: 10mm (13.2% of current outer diameter).

[0049] Step S5: Perform cold drawing of the finished product using a chain-type cold drawing machine. The outer die is a YG8 cemented carbide die, and the inner die is a short mandrel. The drawing speed is 0.8 m / min. The finished product dimensions are Φ60 × 3.5 mm. The wall thickness reduction is 0.3 mm, and the diameter reduction is 6 mm.

[0050] Step S6: The finished tube is fed into a bright annealing furnace under a hydrogen atmosphere, dew point -45℃, and furnace pressure 10Pa (gauge pressure). The heating temperature is 1060℃, and the holding time is 7 minutes (3.5mm × 2min / mm). It is then cooled in the furnace to below 80℃ before being removed from the furnace.

[0051] Example 2

[0052] Target product: 316L stainless steel seamless pipe with an outer diameter of Φ42mm and a wall thickness of 2.5mm.

[0053] Step S1: Select 316L stainless steel billet with the following chemical composition by mass percentage: C 0.018%, Si 0.55%, Mn 1.35%, P 0.025%, S 0.001%, Cr 17.10%, Ni 12.30%, Mo 2.15%, with the balance being Fe and unavoidable impurities. Hot-extrude the billet to Φ63×4mm at 1160℃, followed by solution treatment 26 seconds after extrusion.

[0054] Step S2: First pass cold rolling to Φ53×3.0mm. Wall reduction 1.0mm (25% of the rough tube wall thickness), diameter reduction 10mm (15.9% of the outer diameter). Rolling speed 45 times / minute, feed rate 3.5mm / pass.

[0055] Step S3: Intermediate solution treatment, 1050℃, hold for 9 minutes, water quench.

[0056] Step S4: Second pass cold rolling to Φ45×2.7mm. Wall thickness reduction 0.3mm (10% of current wall thickness), diameter reduction 8mm (15.1% of outer diameter). Rolling speed 65 times / minute, feed rate 2.5mm / pass.

[0057] Step S5: Cold draw the finished product to Φ42×2.5mm. Wall thickness reduction: 0.2mm; Diameter reduction: 3mm. Drawing speed: 1.0m / min.

[0058] Step S6: Bright annealing, 1070℃, hold for 5 minutes, hydrogen atmosphere, dew point -50℃, furnace pressure 8Pa (gauge pressure).

[0059] Example 3

[0060] Target product: Seamless 321 stainless steel pipe with an outer diameter of Φ25mm and a wall thickness of 1.5mm.

[0061] Step S1: Select 321 stainless steel billet with the following chemical composition by mass percentage: C 0.040%, Si 0.48%, Mn 1.20%, P 0.030%, S 0.002%, Cr 17.85%, Ni 9.20%, Ti 0.35%, with the balance being Fe and unavoidable impurities. Hot-extrude the billet to Φ38×2.5mm at an extrusion temperature of 1170℃, followed by solution treatment for 25 seconds after extrusion.

[0062] Step S2: First pass cold rolling to Φ32×1.9mm. Wall reduction 0.6mm (24% of the rough tube wall thickness), diameter reduction 6mm (15.8% of the outer diameter). Rolling speed 55 times / minute, feed rate 3.5mm / pass.

[0063] Step S3: Intermediate solution treatment, 1060℃, hold for 5.7 minutes, water quench.

[0064] Step S4: Second pass cold rolling to Φ27×1.65mm. Wall thickness reduction 0.25mm (13.2% of current wall thickness), diameter reduction 5mm (15.6% of outer diameter). Rolling speed 68 times / minute, feed rate 2.5mm / pass.

[0065] Step S5: Cold draw the finished product to Φ25×1.5mm. Wall thickness reduction: 0.15mm; Diameter reduction: 2mm. Drawing speed: 1.2m / min.

[0066] Step S6: Bright annealing, 1065℃, hold for 3 minutes, decompose ammonia atmosphere, dew point -48℃, furnace pressure 12Pa (gauge pressure).

[0067] Comparative Example 1

[0068] A 304 stainless steel tube with an outer diameter of Φ60mm and a wall thickness of 3.5mm was prepared using a conventional cold rolling-cold drawing combined process. The chemical composition of the billet was the same as in Example 1.

[0069] Hot extrusion rough tube Φ89×6mm → cold rolling to Φ76×4.5mm → intermediate solution treatment (1080℃) → cold rolling to Φ68×4.0mm → intermediate solution treatment (1080℃) → cold drawing to Φ61×3.6mm → finished product solution treatment (1060℃) → cold drawing to Φ60×3.5mm (final pass wall reduction of 0.1mm). The total number of passes is 2 cold rolling passes + 2 cold drawing passes + 3 heat treatments.

[0070] Comparative Example 2

[0071] The same process configuration as in Example 1 was used, but the wall reduction amount in the final cold drawing exceeded the limits defined in this invention, and the chemical composition of the billet was the same as in Example 1.

[0072] Steps S1 to S4 are the same as in Example 1. In step S5, the wall reduction of the finished product after cold drawing is changed to 1.0 mm (exceeding the range of 0.3 to 0.8 mm), and the specifications after cold drawing are Φ60×3.5 mm, with a diameter reduction of 6 mm. Step S6 is the same as in Example 1.

[0073] Comparative Example 3

[0074] The same process configuration as in Example 1 is used, but step S3 intermediate heat treatment is omitted, and the chemical composition of the billet is the same as in Example 1:

[0075] Step S1 is the same as in Example 1. In step S2, after the first cold rolling pass, no intermediate solution treatment is performed; instead, the second cold rolling pass (step S4) is performed directly. The remaining steps are the same as in Example 1.

[0076] Summary and comparative analysis of test data

[0077] The finished pipes obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were tested for dimensional accuracy, surface quality, and mechanical properties. The standards and methods used for testing are as follows: outer diameter and wall thickness were measured using an ultrasonic thickness gauge and a micrometer. Five cross-sections were taken along the length of each sample, and eight points were taken along the circumference of each cross-section. The average value and deviation were recorded. Wall thickness uniformity was calculated as (maximum wall thickness - minimum wall thickness) / nominal wall thickness × 100%. Surface roughness was measured using a portable roughness meter, and the average value of five points was recorded. Yield strength, tensile strength, and elongation were determined on a universal testing machine according to GB / T228.1 standard. Residual stress was determined using X-ray diffraction (sin²ψ method), with the test point at the middle of the outer surface of the pipe. Grain size was evaluated according to GB / T6394 standard. The test results are shown in Table 1.

[0078] Table 1: Summary of Test Data of Finished Pipes from Each Example and Comparative Example

[0079]

[0080] Note: Residual stress was determined using X-ray diffraction (sin²ψ method), with negative values ​​indicating compressive stress. Grain size was evaluated according to GB / T6394 standard. Intermediate heat treatment and finished product heat treatment are both included in the total number of process steps.

[0081] Table 2: Relative comparison of key performance indicators of each embodiment and comparative example (based on comparative example 1)

[0082]

[0083] (1) Dimensional accuracy analysis:

[0084] As shown in Table 1, the measured deviations of the outer diameter in Examples 1 to 3 are all within ±0.04 mm, the measured deviations of the wall thickness are within ±0.03 mm, and the wall thickness uniformity does not exceed ±4.5%, all of which are superior to the technical indicators of ±0.08 mm outer diameter tolerance, ±0.05 mm wall thickness tolerance, and ±5% wall thickness uniformity defined in Claim 10. In contrast, the outer diameter deviation of Comparative Example 1 (conventional multi-pass process) reaches +0.12 mm, and the wall thickness uniformity is ±8.0%, both exceeding the accuracy range defined by this invention. The outer diameter deviation of Comparative Example 2 (excessive wall reduction in the final cold drawing stage) is +0.09 mm, and the wall thickness uniformity is ±6.5%, also exceeding the scope of this invention, indicating that controlling the wall reduction in the final cold drawing stage to 0.3–0.8 mm plays a crucial role in ensuring the final dimensional accuracy. The outer diameter deviation of Comparative Example 3 (with intermediate heat treatment omitted) was +0.11 mm, and the wall thickness uniformity was ±7.2%, indicating that intermediate solution treatment is indispensable for eliminating the work hardening of the first pass and ensuring the uniformity of the second rolling pass.

[0085] As shown in Table 2, Example 1 shows a significant improvement of 75% in outer diameter tolerance and 44% in wall thickness uniformity compared to Comparative Example 1. Example 3, with its smaller pipe diameter and easier uniform control of deformation, exhibits the greatest improvement (83% improvement in outer diameter tolerance and 53% improvement in wall thickness uniformity).

[0086] The mechanism for improving dimensional accuracy is as follows: the first pass of large deformation cold rolling (wall reduction of 30% to 45%) effectively eliminates the wall thickness unevenness left by hot extrusion under triaxial compressive stress, reducing the wall thickness deviation of the tube from ±8% of the rough tube to about ±5%; the intermediate solution treatment eliminates work hardening, allowing the second pass of cold rolling to be carried out under low deformation resistance, avoiding wall thickness fluctuations caused by uneven deformation; the final small deformation cold drawing (wall reduction of 0.3 to 0.8 mm) sizing effect greatly improves the final dimensional accuracy, and the springback under small deformation is controllable, resulting in good dimensional stability.

[0087] (2) Surface quality analysis:

[0088] The outer surface roughness Ra of Examples 1 to 3 is 0.32–0.38 μm, and the inner surface roughness Ra is 1.2–1.4 μm, all satisfying the requirements of Ra ≤ 0.4 μm (outer surface) and Ra ≤ 1.6 μm (inner surface) as defined in claim 10. The outer surface roughness of Comparative Example 1 is 0.60 μm, and the inner surface roughness is 2.2 μm, significantly inferior to the examples. The outer surface roughness of Comparative Example 2 is 0.45 μm, close to but still exceeding the 0.4 μm limit, indicating that excessive wall reduction in the final cold drawing will worsen the surface quality due to increased deformation. Comparative Example 3, due to the omission of intermediate heat treatment, suffers from severe work hardening during the second cold rolling pass, making the surface prone to microcracks and orange peel defects, with an outer surface roughness reaching 0.55 μm.

[0089] The mechanism for improving surface quality is as follows: the first pass of large deformation cold rolling effectively eliminates or heals the original defects (micro-cracks, oxide scale indentation, etc.) on the surface of the hot-extruded tube; the second pass of cold rolling further reduces the surface roughness; the minimal wall reduction of the final cold drawing, combined with the YG8 cemented carbide outer die, plays a final finishing role; bright annealing is carried out in a reducing atmosphere, which avoids surface oxidation, and a smooth surface can be obtained without pickling after annealing.

[0090] (3) Mechanical properties and residual stress analysis:

[0091] Examples 1 to 3 exhibit yield strengths of 238–252 MPa, tensile strengths of 572–590 MPa, elongation of 50%–54%, and residual stress values ​​of 32–38 MPa. Comparative Example 1 shows higher yield and tensile strengths (268 MPa, 595 MPa), lower elongation (46%), and residual stress values ​​of 82 MPa. Comparative Example 2, due to excessive final cold drawing deformation, exhibits the highest degree of work hardening, with a yield strength of 285 MPa, an elongation of only 42%, and residual stress values ​​of 95 MPa, resulting in the worst overall mechanical properties. Comparative Example 3, omitting intermediate heat treatment, shows accumulated work hardening, with a yield strength of 278 MPa, an elongation of 44%, and residual stress values ​​of 78 MPa.

[0092] As shown in Table 2, the residual stress reduction in Examples 1 to 3 reached 54%–61%, and the elongation improvement reached 9%–17%, while the comparative examples showed no improvement or even worsened in terms of elongation and residual stress. This indicates that the "large deformation cold rolling + intermediate solution treatment + small deformation cold drawing + bright annealing" process route of the present invention has significant advantages in residual stress control and plasticity maintenance. The mechanism is as follows: the intermediate solution treatment eliminates the work hardening of the first pass of cold rolling, allowing the second pass to be carried out under low deformation resistance, thus avoiding uneven deformation; the minimal wall reduction (0.3–0.8 mm) of the final cold drawing results in extremely low work hardening; and the final bright annealing completes recrystallization in a reducing atmosphere, obtaining a uniform and fine grain structure (grain size 7.0–8.0 grade), thereby simultaneously achieving a good combination of high strength and high plasticity.

[0093] (4) Organizational analysis:

[0094] The pipe obtained in Example 1 has uniform and fine grains with a grain size of 7.5 grade and no mixed grain phenomenon. The pipe obtained in Comparative Example 1 has a grain size of 6.5 grade and obvious mixed grain phenomenon, with some grains being coarse. The presence of mixed grain structure leads to uneven mechanical properties, reducing the fatigue life and corrosion resistance of the pipe. This invention uses two-pass large deformation cold rolling combined with intermediate solution treatment. Before each pass of cold rolling, the pipe is in a solution state with low deformation resistance. During the rolling process, dynamic recrystallization and deformation-induced phase transformation work together, and finally bright annealing completes static recrystallization, resulting in a uniform and fine grain structure.

[0095] (5) Analysis of residual stress distribution along wall thickness:

[0096] The residual stress distribution along the wall thickness of the pipes obtained in Example 1 and Comparative Example 1 was measured using X-ray diffraction. The residual stress distribution along the wall thickness of Example 1 was relatively uniform, with approximately -35 MPa on the outer surface and approximately -20 MPa in the core, indicating a low overall compressive stress level. The residual stress distribution along the wall thickness of Comparative Example 1 exhibited a larger gradient, with approximately -82 MPa on the outer surface and approximately -45 MPa in the core, and significant stress concentration areas were observed. A uniform residual stress distribution along the wall thickness is beneficial to the dimensional stability and service life of the pipe. This invention effectively reduces the residual stress and its distribution gradient along the wall thickness through a combination of intermediate solution treatment and a final cold drawing with small deformation.

[0097] (6) Process efficiency analysis:

[0098] Examples 1 to 3 all have a total of 4 process passes (2 passes of cold rolling + 1 pass of cold drawing + 1 pass of finished product heat treatment, with intermediate heat treatment counted as a process), while Comparative Example 1 has 7 passes. As shown in Table 2, the number of process passes in the examples is reduced by 43%, significantly shortening the production cycle and reducing energy consumption. Although Comparative Example 2 also uses a 4-pass configuration, the wall reduction in the final cold drawing exceeds the scope of this invention, resulting in substandard dimensional accuracy and mechanical properties. This demonstrates that there is a synergistic relationship between the process configuration and process parameters in this invention, and it cannot be achieved simply by reducing the number of passes. Although Comparative Example 3 has the fewest process passes (3 passes), omitting the intermediate heat treatment leads to accumulated work hardening, resulting in a comprehensive deterioration of dimensional accuracy, surface quality, and mechanical properties, further proving the necessity of intermediate heat treatment in the process route of this invention.

[0099] In summary, Examples 1 to 3 are superior to Comparative Examples 1 to 3 in all aspects, including dimensional accuracy, surface quality, mechanical properties, and residual stress, and the number of process steps is reduced by 43% compared to conventional processes. Comparative Examples 1 to 3 deviate from the technical solution of this invention from different angles, all resulting in a decrease in performance indicators. This verifies the necessity of the process configuration of "large deformation cold rolling for wall and diameter determination, small deformation cold drawing for final finishing" in claim 1 of this invention, as well as the synergistic necessity of process parameters such as intermediate heat treatment and bright annealing. The process of this invention effectively reduces residual stress, increases plasticity reserve, and reduces the number of process steps while ensuring high precision and high surface quality, demonstrating significant inventiveness and industrial application value.

[0100] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited to the embodiments described. Those skilled in the art can make various equivalent modifications or substitutions without departing from the spirit of the present invention, and these equivalent modifications or substitutions are all included within the scope defined by the claims of this application.

Claims

1. A process for manufacturing high-precision seamless stainless steel tubes based on deformation-induced phase transformation strengthening, characterized in that, Includes the following steps: Step S1, tube blank preparation: stainless steel blanks are prepared by hot extrusion process. The heating temperature of the hot extruded blank is 1130~1180℃, and solution treatment is carried out within 30 seconds after extrusion. Step S2, First pass of cold rolling: The rough tube is cold rolled, and the wall thickness reduction is controlled to be 30% to 45% of the rough tube wall thickness, and the diameter reduction is 12% to 20% of the outer diameter; Step S3, intermediate heat treatment: The tube after the first cold rolling is subjected to solution treatment, the heating temperature is 1040~1100℃, the holding time is controlled according to the wall thickness 2~3min / mm, and then water quenching is performed. Step S4, Second Cold Rolling: The tube after intermediate heat treatment is subjected to a second cold rolling, with the wall thickness reduction controlled at 25% to 35% of the current wall thickness and the diameter reduction controlled at 8% to 15% of the current outer diameter; Step S5, finished product cold drawing: The tube after the second cold rolling is cold drawn in the finished product stage, using a short mandrel, controlling the wall reduction to be 0.3-0.8 mm and the diameter reduction to be 3%-6% of the outer diameter; Step S6, Finished product heat treatment: Bright annealing is performed on the cold-drawn finished tube. The annealing temperature is 1050~1080℃, and the holding time is controlled according to the wall thickness of 1.5~2.5min / mm. The atmosphere in the furnace is hydrogen or a reducing atmosphere of decomposed ammonia, and the dew point is controlled below -40℃. In this process, no intermediate straightening or pickling process other than intermediate heat treatment is performed between the first cold rolling pass and the second cold rolling pass.

2. The high-precision seamless stainless steel tube manufacturing process based on deformation-induced phase transformation strengthening according to claim 1, characterized in that, In step S2, the first cold rolling pass uses a two-roll cold rolling mill with a rolling speed of 40-60 times / minute and a feed rate of 3-6 mm / pass.

3. The high-precision seamless stainless steel tube manufacturing process based on deformation-induced phase transformation strengthening according to claim 1, characterized in that, In step S4, the second cold rolling is performed using a two-roll cold rolling mill with a rolling speed of 50-70 times / minute and a feed rate of 2-5 mm / pass.

4. The high-precision seamless stainless steel tube manufacturing process based on deformation-induced phase transformation strengthening according to claim 1, characterized in that, In step S5, the drawing speed of the finished product cold drawing is 0.5 to 1.5 m / min.

5. The high-precision seamless stainless steel tube manufacturing process based on deformation-induced phase transformation strengthening according to claim 1, characterized in that, In step S5, the outer mold of the finished product cold drawing is made of YG8 cemented carbide.

6. The high-precision seamless stainless steel tube manufacturing process based on deformation-induced phase transformation strengthening according to claim 1, characterized in that, In step S6, the furnace pressure during bright annealing is maintained at a slightly positive pressure of 5-15 Pa gauge pressure.

7. The high-precision seamless stainless steel tube manufacturing process based on deformation-induced phase transformation strengthening according to claim 1, characterized in that, In step S6, the dew point of the reducing atmosphere is controlled between -40°C and -60°C.

8. The high-precision seamless stainless steel tube manufacturing process based on deformation-induced phase transformation strengthening according to claim 1, characterized in that, The stainless steel is 304 austenitic stainless steel, 316L austenitic stainless steel or 321 austenitic stainless steel.

9. The high-precision seamless stainless steel tube manufacturing process based on deformation-induced phase transformation strengthening according to claim 1, characterized in that, In step S2, the wall thickness reduction is 35% to 42% of the rough pipe wall thickness, and the diameter reduction is 14% to 18% of the outer diameter; in step S4, the wall thickness reduction is 28% to 33% of the current wall thickness, and the diameter reduction is 10% to 13% of the current outer diameter.

10. A seamless stainless steel tube manufactured by the high-precision seamless stainless steel tube preparation process based on deformation-induced phase transformation strengthening as described in any one of claims 1 to 9, characterized in that, The outer diameter tolerance of the seamless stainless steel tube shall not exceed ±0.08mm, the wall thickness tolerance shall not exceed ±0.05mm, the wall thickness uniformity shall not exceed ±5%, the outer surface roughness Ra≤0.4μm, the inner surface roughness Ra≤1.6μm, and the absolute value of residual stress shall not exceed 50MPa.