Process for the treatment of manganese carbonate ores

By mixing manganese carbonate ore powder with ammonium sulfate in the liquid phase and then roasting at low temperature and rapidly cooling, the problem of selective leaching of manganese, iron, calcium and magnesium in low-grade manganese carbonate ore was solved, achieving efficient extraction of manganese and highly selective recovery of resources, while reducing purification costs.

CN123132610APending Publication Date: 2026-11-20CENT SOUTH UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611649356.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-23
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies are difficult to efficiently and selectively leach manganese from low-grade manganese carbonate ores, and there are also problems with unsatisfactory selectivity in the leaching of manganese, iron, calcium, and magnesium, resulting in low overall manganese recovery rate and high purification costs.

Method used

The process involves mixing manganese carbonate ore powder with ammonium sulfate in the liquid phase, followed by low-temperature roasting and rapid cooling, and then using a water leaching process. By utilizing the activation effect of ammonium bisulfate, selective leaching of manganese is achieved, and the catalytic leaching of iron, calcium, and magnesium is reduced through the synergistic catalysis of additives.

Benefits of technology

This method enables highly selective extraction of manganese from low-grade manganese carbonate ore, improves the manganese leaching rate, and reduces the accompanying leaching of iron, calcium, and magnesium, thus possessing industrialization value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123132610A_ABST
    Figure CN123132610A_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of mineral processing and manganese metallurgy, and particularly relates to a processing method of manganese carbonate ore, which comprises the following steps: mixing manganese carbonate ore powder and ammonium sulfate liquid phase, and then drying to obtain a composite material; roasting the composite material at a low temperature of 240-380 DEG C to obtain a roasted material; subjecting the roasted material to quenching treatment, and then water leaching treatment, and then performing solid-liquid separation to obtain a manganese sulfate water leaching liquid. The present application innovatively composites manganese carbonate ore powder and ammonium sulfate liquid phase, and then performs roasting treatment at the temperature, so that the high-activity ammonium bisulfate in-situ converted based on ammonium sulfate can activate and transform and decompose the structure of manganese carbonate ore, and then further combined with quenching and water leaching treatment, so that the manganese in the manganese carbonate ore can be selectively leached, and the accompanying leaching of iron, calcium and magnesium can be reduced, so that the high-selectivity extraction of manganese in the manganese carbonate ore can be realized at the front end.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of mineral processing and manganese metallurgy technology, specifically relating to a method for processing manganese carbonate ore. Technical Background

[0002] Manganese, as an important metal, is widely used in key fields such as iron and steel metallurgy, new energy batteries, electronic information, chemical catalysis, and aerospace. Among them, manganese sulfate and manganese carbonate are two core basic products that connect manganese ore resource development, deep processing, and the manufacture of high-end manganese-based materials, playing an irreplaceable role in the manganese industry chain. Manganese sulfate is an important raw material for preparing high-purity battery-grade manganese sources, widely used in high-nickel ternary materials, lithium manganese oxide, lithium manganese iron phosphate, and other new energy battery cathode materials; manganese carbonate is an important precursor for the production of high-purity manganese salts, electronic-grade materials, and various functional manganese-based compounds. With the continuous growth in demand for new energy manganese-based materials and the increasingly prominent strategic value of high-purity manganese sulfate and manganese carbonate, stable access to high-quality manganese resources has become crucial to ensuring the development of the industry chain. However, existing manganese ore resources generally exhibit a structural characteristic of "few rich ores and many poor ores," with low-grade manganese carbonate ores being the main component. These ores generally suffer from low manganese grade, numerous associated impurities, and high difficulty in beneficiation, resulting in long-term underutilization. With the increasing scarcity of high-quality manganese ore resources, low-grade manganese carbonate ore is gradually becoming an important resource source for the stable production of basic manganese salts such as manganese sulfate and manganese carbonate. Therefore, breakthroughs in the efficient utilization technology of low-grade manganese carbonate ore will not only help improve the comprehensive utilization rate of manganese resources and the added value of products, but also be of great significance for ensuring the security of manganese resource supply, enhancing the resilience of the new energy manganese materials industry chain, and promoting the green and sustainable development of the manganese industry.

[0003] Currently, the existing technologies for preparing manganese sulfate and manganese carbonate from manganese carbonate ore mainly include two types of processes: direct wet leaching and roasting-enhanced leaching. For example, Chinese patent document CN117604244A discloses the leaching of low-grade manganese carbonate ore with an inorganic strong acid, and the preparation of a low-impurity manganese leaching solution using a weak acid adjustment process; Chinese patent document CN121109875A discloses the reduction roasting of rhodochrosite using an ammonium sulfate-oxalic acid composite flux under a nitrogen protective atmosphere, utilizing the reducing effect of oxalic acid to reduce a small amount of high-valence manganese in the ore to low-valence manganese, thereby improving the leaching and recovery efficiency of manganese in low-grade rhodochrosite. However, the direct wet leaching process has drawbacks such as high leaching agent consumption, high pressure for acidic waste liquid disposal, and high requirements for equipment corrosion resistance; the roasting-enhanced leaching process requires high-temperature roasting and the introduction of inert protective gas, leading to increased energy consumption and operating costs.

[0004] Therefore, developing efficient and low-consumption extraction technologies for manganese from low-grade manganese carbonate ores and constructing a collaborative recycling system for ammonium salts and tail gas resources are of great significance for improving the utilization efficiency of manganese resources, reducing environmental impact, and ensuring the security of manganese resource supply. Summary of the Invention

[0005] To address the aforementioned problems, the present invention aims to provide a method for processing manganese carbonate ore, with the goal of highly selectively recovering manganese from it.

[0006] Manganese carbonate ore is commonly found intercalated with iron, magnesium, and calcium, especially in low-grade manganese carbonate ore, where the intercalation of manganese, iron, calcium, and magnesium is even more concentrated, and the overall content of these components is relatively high. This further restricts the efficient leaching and selective separation of manganese. Existing processes mainly employ a post-leaching staged purification approach, which lacks effective control over the reaction and dissolution behavior of manganese, iron, calcium, and magnesium during the leaching process. This easily leads to acid consumption of non-target components and co-leaching of impurities, increasing the subsequent separation load and purification cost of manganese with iron, calcium, and magnesium. Furthermore, manganese loss may occur due to co-precipitation, adsorption, or entrainment, reducing the overall manganese recovery rate. To address this problem, this invention, through in-depth research, provides a front-end solution to improve the selective leaching of manganese, iron, calcium, and magnesium in manganese carbonate ore, as detailed below:

[0007] A method for processing manganese carbonate ore involves mixing manganese carbonate ore powder and ammonium sulfate in liquid phase and then drying the mixture to obtain a composite material; the amount of ammonium sulfate is more than 0.7 times the weight of the manganese carbonate ore.

[0008] The composite material is calcined at a low temperature of 240~380℃ to obtain the calcined material;

[0009] The roasted material was subjected to rapid cooling, followed by water immersion, and then solid-liquid separation to obtain manganese sulfate aqueous extract.

[0010] To address the issue of unsatisfactory selectivity in leaching manganese, iron, calcium, and magnesium from manganese carbonate ore, this invention innovatively combines manganese carbonate powder with ammonium sulfate in a liquid phase, followed by roasting at a specified temperature. This allows for the activation, transformation, and decomposition of the manganese carbonate ore structure based on the in-situ conversion of highly active ammonium bisulfate from ammonium sulfate. Further combined with rapid cooling and water leaching, this synergistic process achieves selective leaching of manganese from the manganese carbonate ore while reducing the accompanying leaching of iron, calcium, and magnesium. This enables highly selective extraction of manganese from the manganese carbonate ore at the upstream stage. Furthermore, this invention features a mild processing temperature and low reagent dosage, demonstrating excellent industrialization value.

[0011] In this invention, there are no special requirements for the grade of the manganese carbonate ore powder. In order to maximize the economic value of the technical solution of this invention, it can be medium- or low-grade manganese carbonate ore powder, for example, the grade of manganese is 8% to 20% (for example, it can be a low-grade ore of 8% to 12%); the grade of iron is 1% to 15%; the grade of calcium is 1% to 10%; and the grade of magnesium is 0.1% to 5%.

[0012] The particle size of the manganese carbonate ore powder is ≤5mm.

[0013] In this invention, the concentration of ammonium sulfate in the liquid-phase mixing system is 0.30~0.95 g / mL, for example, it can be further 0.5~0.8 g / mL;

[0014] In this invention, considering both effectiveness and cost, the weight ratio of manganese carbonate ore powder to ammonium sulfate is 1:0.8~2, and can be further 1:1~1.5;

[0015] Preferably, the liquid-phase mixing process is carried out under ultrasonic-assisted immersion or negative pressure;

[0016] Preferably, the drying temperature is 80~200℃.

[0017] In this invention, additives are also added to the material before calcination;

[0018] The additives include at least one of hydrotalcite and calcium titanate;

[0019] Preferably, the divalent metal of hydrotalcite includes at least one of Mn, Mg, Fe, Ca, Zn, and Cu; the trivalent metal of hydrotalcite includes at least one of Al, Fe, Mn, and Cr.

[0020] This invention innovatively demonstrates that further use of additives during the roasting process can further synergistically enhance the in-situ catalytic reactivity of ammonium bisulfate on manganese carbonate ore, thereby improving the water leaching selectivity of manganese, iron, calcium, magnesium, and other elements in manganese carbonate ore.

[0021] Preferably, the amount of additive is 1 to 10% of the weight of manganese carbonate ore powder, and more preferably 4 to 6%.

[0022] In this invention, the atmosphere during the roasting process is an oxygen-containing atmosphere; preferably, the oxygen-containing atmosphere is air.

[0023] In this invention, the calcination temperature can be 280~360℃, and more specifically 300~350℃.

[0024] Preferably, the roasting time is 20-150 min, and more preferably 60-120 min.

[0025] In this invention, the roasted material is innovatively subjected to rapid cooling while hot, which helps to further enhance the water leaching selectivity of elements such as manganese, iron, calcium, and magnesium.

[0026] In this invention, considering cost, the cooling medium for rapid cooling is water;

[0027] Preferably, the initial temperature of the cooling medium is below 40°C, and more preferably it is 4~30°C;

[0028] Preferably, during the rapid cooling stage, the solid-liquid ratio of the calcining material and the cooling medium is 1:3~20, and more preferably 1:5~10.

[0029] In this invention, during the water immersion process, the solid-liquid ratio is 1:3~20, which can be further 1:5~10; the immersion temperature is 60~120℃, which can be further 65~85℃; the immersion time is 30~150min, which can be further 60~120min; and the stirring rate is 30~400r / min, which can be further 100~120r / min.

[0030] In this invention, valuable manganese metal can be recovered from manganese sulfate aqueous leaching solution using known processes. For example, as an optional approach, the manganese sulfate aqueous leaching solution is subjected to impurity removal treatment to obtain purified manganese sulfate solution, which is then subjected to crystallization treatment to separate solid and liquid phases to obtain manganese sulfate crystals and crystallization mother liquor.

[0031] In this invention, the mother liquor for crystallization is subjected to carbonation treatment, followed by solid-liquid separation to obtain manganese carbonate precipitate and carbonation mother liquor;

[0032] Preferably, the carbonation atmosphere is the exhaust gas from roasting;

[0033] Preferably, the carbonation mother liquor is subjected to oxalic acid precipitation, followed by solid-liquid separation and calcination to obtain the hydrotalcite.

[0034] Ammonium bicarbonate is prepared by absorbing and treating the carbonation atmosphere.

[0035] Beneficial effects:

[0036] (1) In this invention, manganese carbonate ore powder and ammonium sulfate are pre-composite and then roasted with controlled roasting temperature. This enables the physicochemical transformation of manganese carbonate based on the in-situ conversion of ammonium sulfate with highly active ammonium bisulfate, thus achieving selective leaching of manganese in manganese carbonate ore.

[0037] (2) This invention combines low-temperature roasting with liquid-phase rapid cooling to promote the conversion of manganese carbonate into water-soluble manganese salt, thereby achieving simultaneous rapid cooling and preliminary leaching. The salt phase dissolution forms pore channels, reducing leaching diffusion resistance, and the sensible heat of the roasted sand is used to heat the leaching process, thereby improving manganese extraction efficiency and heat utilization efficiency.

[0038] (3) The present invention also shows that the innovative use of additives to assist in roasting helps to further enhance the in-situ activity of ammonium bisulfate and further enhance the leaching rate and selectivity of manganese in manganese carbonate ore. Attached Figure Description

[0039] Figure 1 This is a complete process flow diagram of the present invention;

[0040] Figure 2 The XRD pattern of raw manganese carbonate ore in Example 1;

[0041] Figure 3 The XRD pattern of the ammonium bicarbonate product in Example 1 is shown below.

[0042] Figure 4 The XRD pattern of the manganese sulfate product in Example 1 is shown below.

[0043] Figure 5 The XRD pattern of the manganese carbonate product in Example 1 is shown below.

[0044] Figure 6 XRD pattern of magnesium-manganese-aluminum hydrotalcite from Example 1 (a: uncalcined; b: calcined at 400℃; c: adsorbed F) - back); Detailed Implementation

[0045] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments, but the scope of protection of the present invention is not limited to the following embodiments.

[0046] The present invention provides an optional method for processing manganese carbonate ore, comprising the following steps:

[0047] Step (1): After crushing and grinding the manganese carbonate ore, mix it thoroughly with ammonium sulfate solution and optional additives in a predetermined ratio, and then dry it to constant weight;

[0048] Step (2): The uniformly mixed material is placed in a tube furnace for roasting. During the roasting process, air is continuously introduced through an air pump. The roasted sand is then rapidly cooled and leached with water and separated into solid and liquid to obtain leachate and leach residue.

[0049] Step (3): After purifying and removing impurities from the leachate, the purified liquid is concentrated, crystallized, and separated into solid and liquid to obtain manganese sulfate product and mother liquor A; the ammonia gas generated by roasting in step (2) and the added carbon dioxide are passed into mother liquor A for carbonization and manganese precipitation, and manganese carbonate precipitate and mother liquor B are obtained by solid-liquid separation. The manganese carbonate precipitate is washed and dried to obtain manganese carbonate product.

[0050] Step (4): Oxalic acid is added to the mother liquor B obtained in step (3) to precipitate the residual manganese, magnesium, aluminum and other ions with oxalic acid. After filtration, the filtrate and oxalic acid precipitate are obtained.

[0051] Step (5): Weigh Al2(SO4)3·18H2O according to a predetermined ratio, add it to the oxalic acid precipitate obtained in step (4), grind it for a predetermined time to mix it thoroughly; then add NaOH according to a predetermined ratio, continue grinding until it is evenly mixed, and after washing with water, filtering and drying, the resulting material is magnesium manganese aluminum hydrotalcite.

[0052] Further, in step (1), the manganese carbonate ore is dried at 80~200℃.

[0053] Further, the dried manganese carbonate ore in step (1) is crushed and ground into particles with a diameter ≤5mm.

[0054] Further, in step (1), the mass ratio of manganese carbonate ore to ammonium sulfate is 1:0.8~2.

[0055] Furthermore, in step (2), the calcination temperature is 240~380℃, the calcination time is 20~150min, and air is used as the carrier gas with a flow rate of 1~4m. 3 / h.

[0056] Furthermore, in step (2), the medium for rapid cooling is room temperature water, wherein the solid-liquid ratio of roasted ore sand to water is 1:3~20;

[0057] The system after rapid cooling is then subjected to leaching treatment, wherein the leaching temperature is 60~120℃, the leaching time is 30~150min, and the stirring rate is 30~400r / min.

[0058] Further, in step (2), the graded purification and impurity removal process of the leachate includes: adding hydrogen peroxide solution to the leachate and stirring thoroughly to allow Fe to be purified. 2+ Oxidized to Fe 3+ The pH of the solution was adjusted to 5-6 using dilute ammonia water, so that Fe... 3+ And Al 3+ The precipitates are formed as Fe(OH)3 and Al(OH)3 respectively, and the filtrate is obtained by solid-liquid separation. A sulfiding agent is added to the filtrate, the amount of which is 0.002 to 0.01 times the mass of the calcined sand. The sulfiding agent is selected from one or more of sodium formaldehyde sulfoxylate, MnS, Na2S and NaHS to precipitate and remove trace metal impurities such as copper, cobalt, nickel, zinc and lead. The filtrate is obtained by solid-liquid separation. Then a fluoridating agent is added to form insoluble fluoride precipitates of calcium and magnesium ions. The fluoridating agent is selected from one or two of NH4F and MnF2. After solid-liquid separation, magnesium manganese aluminum hydrotalcite is added to the filtrate to adsorb and remove residual copper ions and fluoride ions remaining from the calcium and magnesium removal process. Solid-liquid separation is performed again to obtain a purified liquid. The purified liquid is evaporated, crystallized and solid-liquid separated to obtain manganese sulfate product and crystallization mother liquor. Further, the washing liquid obtained in step (3) is collected and returned to the water quenching process for recycling as a water quenching medium for the calcined product.

[0059] Further, the ammonia and carbon dioxide gas generated in step (1) are introduced into mother liquor A for carbonization reaction.

[0060] Furthermore, the filtrate obtained in step (4) is appropriately adjusted and added to step (1) to realize the recycling of ammonium sulfate.

[0061] Furthermore, the magnesium-manganese-aluminum hydrotalcite obtained in step (5) is added to step (1) as an additive to promote the deammoniation of ammonium sulfate to generate ammonium bisulfate during the subsequent roasting process; the magnesium-manganese-aluminum hydrotalcite can also be used in the purification process to adsorb and remove copper ions and fluoride ions.

[0062] In the following cases, the solid-liquid ratio for the quenching and leaching processes is expressed in g / mL.

[0063] The low-grade manganese carbonate ore used in the examples was provided by a manganese mine in Guizhou Province, and its total manganese (T) Mn The content of ore was 9.48%, and the main mineral was manganese carbonate (MnCO3). The XRF results of the ore are shown in Table 1.

[0064] Table 1. XRF Results Analysis of Low-Grade Manganese Carbonate Ore (wt.%)

[0065]

[0066] Example 1

[0067] Manganese carbonate ore was dried at 100℃ for 12 hours, cooled to room temperature, coarsely crushed using a jaw crusher, and then finely ground using a ball mill to obtain manganese carbonate ore powder with a particle size of less than 75μm. 30g of the ore sample was weighed for later use. 1.5g of magnesium-manganese-aluminum hydrotalcite (additive) was weighed and mixed evenly with the ore sample.

[0068] Weigh 30g of ammonium sulfate and add it to 50mL of water. Stir well and pour the mixture into the ammonium sulfate solution. Mix for 10min. Dry the well-mixed sample at 100℃ to constant weight.

[0069] Subsequently, the sample was placed in a tube furnace and calcined under a continuous air atmosphere, with the air flow rate controlled at 1.5 m³ / min during the calcination process. 3 The temperature is increased to 350℃ (roasting temperature) at a rate of 5℃ / min per hour and held for 120 minutes. During roasting, manganese carbonate ore undergoes a sulfation reaction with ammonium sulfate, and the manganese in the ore is gradually converted into water-soluble ammonium manganese sulfate double salt. At the same time, ammonium sulfate decomposes upon heating to produce ammonia-containing gas.

[0070] Immediately after the high-temperature roasted sand was removed from the furnace, it was added to 150g of deionized water with an initial temperature of 30°C, which was pre-placed in a leaching reactor, and rapidly cooled. Then, leaching was carried out at 70°C while maintaining the aforementioned liquid-to-solid ratio. The stirring speed during the leaching process was 100 r / min, and the leaching time was 120 min, allowing the manganese sulfate in the roasted sand to dissolve and enter the liquid phase. After leaching, solid-liquid separation was performed using vacuum filtration to obtain manganese sulfate leachate and leaching residue.

[0071] Further calculations of the leaching rates of metals such as manganese and iron showed that the leaching rate of manganese was 95.71%, the leaching rate of iron was only 20.47%, the leaching rate of calcium was 4.32%, and the leaching rate of magnesium was 59.34%.

[0072] Example 2

[0073] In this invention, known processes can be used to separate and purify manganese from the leachate of Example 1. For example, compared with Example 1, the only difference is that the manganese sulfate leachate is treated as follows:

[0074] The obtained manganese sulfate leaching solution was purified to remove impurities. First, 5% hydrogen peroxide solution was added to the leaching solution to prevent further precipitation. Ammonia water was slowly added to the leaching solution to adjust the pH to 6.0. After stirring for 120 min, the solution was filtered to remove impurities such as iron and aluminum. Then, 0.15 g of ammonium sulfide was added to the filtrate and reacted at room temperature for 60 min. After standing for 60 min, the solution was filtered to remove heavy metal impurities such as copper, lead, zinc, nickel, and cobalt. Next, 2 g of MnF was added to the filtrate and reacted at 90 °C for 120 min. After filtering, impurities such as calcium and magnesium were removed. Finally, 1 g of magnesium manganese aluminum hydrotalcite product was added to the filtrate, heated to 30 °C, and stirred for 120 min to remove residual copper and fluoride ions. The purified manganese sulfate solution was obtained by filtration.

[0075] The purified manganese sulfate solution was slowly heated to evaporate the water until the solution was concentrated to saturation. The concentrate was then cooled to room temperature, causing crystals to precipitate. After filtration and drying, pure manganese sulfate monohydrate and the remaining mother liquor were obtained. The manganese content and impurity ion content in the product were analyzed using single-element analysis. The filtered mother liquor was added to a carbonization reactor.

[0076] During the roasting process, ammonia-containing gas from a tubular furnace is directly introduced into the mother liquor along with carbon dioxide through a corrosion-resistant gas inlet pipe to carry out a carbonization reaction. Carbonization and precipitation are completed under mechanical stirring conditions. The carbonization reaction temperature is controlled at 40℃, and the reaction time is 60 minutes. As the reaction proceeds, a light pink manganese carbonate precipitate gradually forms in the system. Solid-liquid separation is performed using vacuum filtration. The obtained precipitate is washed with deionized water to remove entrained soluble salt impurities. The washed manganese carbonate precipitate is dried to constant weight in an oven at 105℃ to obtain industrial-grade manganese carbonate product. Finally, the remaining tail gas is fractionally absorbed, and after crystallization and drying, ammonium bicarbonate product is obtained.

[0077] 3g of oxalic acid was added to the filtrate after carbonization reaction to precipitate oxalic acid. The precipitate and filtrate were obtained by filtration. The main component of the filtrate was ammonium sulfate. The recovered filtrate was replenished and adjusted to the predetermined composition and then reused in the raw material mixing and roasting process to realize the closed-loop recycling of roasting additives, thereby constructing a recycling system of "ammonium sulfate roasting-carbonizing agent-carbonization conversion-ammonium sulfate regeneration". The obtained precipitate was ground and mixed with 10g of Al2(SO4)3·18H2O and NaOH. The mixture was then washed and filtered with water and finally dried to obtain magnesium manganese aluminum hydrotalcite. Finally, the obtained magnesium manganese aluminum hydrotalcite was roasted at 400℃ for 120min to obtain magnesium manganese aluminum hydrotalcite product.

[0078] This invention demonstrates that it enables the selective and efficient extraction of manganese resources and the recycling of ammonia from low-grade manganese carbonate ore through a roasting and leaching process.

[0079] Example 3

[0080] Compared with Example 1, the only difference is that the amount of ammonium sulfate was adjusted to 45g, the concentration of ammonium sulfate during the treatment process was 0.6g / mL, and the auxiliary agent was 6% of the weight of manganese carbonate ore. All other operations and parameters were the same as in Example 1. The final result was:

[0081] The leaching rates were 98.31% for manganese, 28.21% for iron, 6.33% for calcium, and 65.39% for magnesium.

[0082] Example 4

[0083] Compared to Example 1, the only difference is that the grinding (ball mill grinding) time is adjusted to maintain the mineral particle size at 1mm~2mm. All other operations and parameters are the same as in Example 1. The final result is:

[0084] The leaching rates were 89.37% for manganese, 21.89% for iron, 2.45% for calcium, and 49.23% for magnesium.

[0085] Example 5

[0086] Compared with Example 1, the only difference is that the calcination temperature was adjusted to 300℃ for constant temperature calcination. All other operations and parameters are the same as in Example 1. The final result is:

[0087] The leaching rates were 91.22% for manganese, 20.67% for iron, 4.10% for calcium, and 58.21% for magnesium.

[0088] Example 6

[0089] Compared with Example 1, the only difference is that the calcination time was adjusted to 60 minutes; all other operations and parameters are the same as in Example 1. The final result is:

[0090] The leaching rates were 91.04% for manganese, 20.50% for iron, 3.75% for calcium, and 53.84% for magnesium.

[0091] Example 7

[0092] Compared with Example 1, the only difference is that during the rapid cooling process, the solid-liquid ratio is 1:10 (g / mL), the leaching temperature is adjusted to 80℃, and the leaching time is 100 min. All other operations and parameters are the same as in Example 1. The final result is:

[0093] The leaching rates were 96.13% for manganese, 21.44% for iron, 3.94% for calcium, and 57.23% for magnesium.

[0094] Example 8

[0095] Compared with Example 1, the only difference is that no additives were added; all other operations and parameters are the same as in Example 1.

[0096] The leaching rates were as follows: manganese 92.38%, iron 24.43%, calcium 4.42%, and magnesium 4.42%.

[0097] 60.95%.

[0098] Example 9

[0099] Compared to Example 4, the only difference is that the temperature of the medium during the rapid cooling stage is adjusted to 10°C deionized water. All other operations and parameters are the same as in Example 4. The final result is:

[0100] The leaching rates were 92.72% for manganese, 23.27% for iron, 4.01% for calcium, and 59.79% for magnesium.

[0101] Example 10

[0102] Compared to Example 1, the only difference is that the liquid-phase mixing process is carried out under negative pressure (0.1 atmospheres). All other operations and parameters are the same as in Example 1. The final result is:

[0103] The leaching rates were 97.03% for manganese, 21.57% for iron, 4.55% for calcium, and 61.24% for magnesium.

[0104] Example 11

[0105] Compared with Example 1, the only difference is that 1.5g of calcium titanate was added as an additive during the calcination process. All other operations and parameters are the same as in Example 1. The final result is:

[0106] The leaching rates were 94.21% for manganese, 25.34% for iron, 5.19% for calcium, and 69.24% for magnesium.

[0107] As can be seen from Examples 1 and 11, using hydrotalcite as an additive helps to further optimize the leaching effect of manganese.

[0108] Comparative Example 1

[0109] Low-grade manganese carbonate ore (same as in Example 1) was dried at 100°C for 12 hours, cooled to room temperature, coarsely crushed using a jaw crusher, then finely ground using a ball mill, and passed through a 200-mesh sieve to obtain manganese carbonate ore powder with a particle size of less than 75 μm. 30 g of ore sample was weighed for later use.

[0110] Measure 15 mL of 98% concentrated sulfuric acid and 147 mL of distilled water. Slowly add the concentrated sulfuric acid to the distilled water and mix thoroughly in the leaching reactor. Add the manganese carbonate ore to the leaching reactor, control the leaching temperature at 30℃, the stirring speed at 400 r / min, and leach for 60 min. During the leaching process, manganese carbonate gradually converts to manganese sulfate and dissolves into the liquid phase. After leaching, vacuum filtration is used for liquid-solid separation to obtain manganese sulfate leachate and leaching residue.

[0111] Further calculations of the leaching rates of metals such as manganese and iron showed that the leaching rate of manganese was 96.60%, the leaching rate of iron was 38.70%, the leaching rate of calcium was 9.93%, and the leaching rate of magnesium was 82.10%.

[0112] Comparative Example 2

[0113] Compared with Example 1, the only difference is that the calcination temperature is adjusted to 200°C. All other operations and parameters are the same as in Example 1. The final result is:

[0114] The leaching rates were 51.27% for manganese, 8.34% for iron, 1.98% for calcium, and 49.31% for magnesium.

[0115] Comparative Example 3

[0116] Compared with Example 1, the only difference is that the amount of ammonium sulfate used was adjusted to 15g. All other operations and parameters are the same as in Example 1. The final result is:

[0117] The leaching rates were 78.78% for manganese, 14.23% for iron, 2.15% for calcium, and 52.77% for magnesium.

[0118] Comparative Example 4:

[0119] Compared with Example 1, the only difference is that rapid cooling is not performed; that is, after calcination, the furnace is cooled first, followed by water immersion treatment. All other operations and parameters are the same as in Example 1. The final result is:

[0120] The leaching rates were 79.23% for manganese, 15.41% for iron, 2.07% for calcium, and 50.00% for magnesium.

[0121] Comparative Example 5:

[0122] Compared with Example 1, the only difference is that ammonium sulfate and manganese carbonate ore were mixed in a solid phase and then roasted. All other operations and parameters were the same as in Example 1. The final result was:

[0123] The leaching rates were 82.39% for manganese, 17.84% for iron, 2.54% for calcium, and 56.37% for magnesium.

[0124] Comparative Example 6:

[0125] Compared with Example 1, the only difference is that the calcination temperature was adjusted to 500°C. All other operations and parameters are the same as in Example 1. The final result is:

[0126] The leaching rates were 71.18% for manganese, 16.69% for iron, 2.19% for calcium, and 52.44% for magnesium.

[0127] The above description is only a preferred embodiment of the present invention. Any modifications, substitutions or variations made by those skilled in the art without departing from the spirit and essence of the present invention shall fall within the protection scope defined by the claims of the present invention.

Claims

1. A method for processing manganese carbonate ore, characterized in that, Manganese carbonate ore powder and ammonium sulfate were mixed in liquid phase and then dried to obtain a composite material; the amount of ammonium sulfate was more than 0.7 times the weight of manganese carbonate ore. The composite material is calcined at a low temperature of 240~380℃ to obtain the calcined material; The roasted material was subjected to rapid cooling, followed by water immersion, and then solid-liquid separation to obtain manganese sulfate aqueous extract.

2. The method for processing manganese carbonate ore as described in claim 1, characterized in that, The manganese carbonate ore powder mentioned is a medium-to-low grade manganese carbonate ore powder; The particle size of the manganese carbonate ore powder is ≤5mm.

3. The method for processing manganese carbonate ore as described in claim 1, characterized in that, In the liquid-phase mixing system, the concentration of ammonium sulfate is 0.30~0.95 g / mL, preferably a saturated ammonium sulfate solution; The weight ratio of manganese carbonate ore powder to ammonium sulfate is 1:0.8~2; Preferably, the liquid-phase mixing process is carried out under ultrasonic assistance or negative pressure; Preferably, the drying temperature is 80~200℃.

4. The method for processing manganese carbonate ore as described in claim 1, characterized in that, Additives are also added to the material before roasting; The additives include at least one of hydrotalcite and calcium titanate; Preferably, the divalent metal of hydrotalcite includes at least one of Mn, Mg, Fe, Ca, Zn, and Cu; the trivalent metal of hydrotalcite includes at least one of Al, Fe, Mn, and Cr.

5. The method for processing manganese carbonate ore as described in claim 4, characterized in that, The dosage of the additive is 1 to 10% of the weight of the manganese carbonate ore powder.

6. The method for processing manganese carbonate ore as described in claim 1, characterized in that, The atmosphere during the roasting process is an oxygen-containing atmosphere; preferably, air. Preferably, the roasting time is 20-150 min.

7. The method for processing manganese carbonate ore as described in claim 1, characterized in that, The cooling medium for rapid cooling is water; Preferably, the initial temperature of the cooling medium is below 40°C; Preferably, during the rapid cooling stage, the solid-liquid ratio of the calcining material and the cooling medium is 1:3~20.

8. The method for processing manganese carbonate ore as described in claim 1, characterized in that, During the water immersion process, the solid-liquid ratio is 1:3~20, the immersion temperature is 60~120℃, the immersion time is 30~150min, and the stirring rate is 30~400r / min.

9. The method for processing manganese carbonate ore as described in any one of claims 1 to 8, characterized in that, The manganese sulfate aqueous leaching solution was subjected to impurity removal treatment to obtain a purified manganese sulfate solution. Subsequently, the purified solution was subjected to crystallization treatment, and solid-liquid separation was performed to obtain manganese sulfate crystals and crystallization mother liquor.

10. The method for processing manganese carbonate ore as described in claim 9, characterized in that, The mother liquor from crystallization was subjected to carbonation treatment, followed by solid-liquid separation to obtain manganese carbonate precipitate and carbonation mother liquor; Preferably, the carbonation atmosphere is the exhaust gas from roasting; Preferably, the carbonation mother liquor is subjected to oxalic acid precipitation, followed by solid-liquid separation and calcination to obtain the hydrotalcite. Ammonium bicarbonate is prepared by absorbing and treating the carbonation atmosphere.

Citation Information

Patent Citations

  • Method for preparing manganese immersion liquid with low impurity content by utilizing low-grade manganese carbonate ore

    CN117604244A

  • Heat-treatment-free Nb-Ti composite microalloyed Q420qD steel plate and preparation method thereof

    CN121109875A