A multi-dimensional gradient structure conductive reinforcing phase material and a preparation method thereof
Patent Information
- Application Number
- CN202611119683.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-27
- Publication Date
- 2026-11-20
AI Technical Summary
[0005]然而,Ti3ZnC2在制备及与金属基复合中仍存在以下应用瓶颈:其一,反应介质中ZnCl2的高粘度和强吸湿性导致熔盐传质效率低,反应物扩散受阻,A位置换反应动力学不可控,导致其物相、结构、尺寸和表面性质稳定性较差,难以满足复合材料对增强相的高要求;其二,产物仅为单一三维结构Ti3ZnC2,既缺乏界面功能化设计,导致与Ag、Cu、Sn基体复合时界面结合弱、润湿性差,易发生界面剥离与早期失效;也无法构建多维度(三维/二维/零维)梯度结构,致使材料内部在高导电所需的连续电子通道、抗机械冲击所需的柔性缓冲界面、以及抑制电弧热应力开裂所需的应力分散中心之间缺乏协同集成,因而导电性、力学强度与抗电弧侵蚀能力三者相互制约,难以实现综合性能的同步提升
Smart Images

Figure CN123132684A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electrical contact materials technology, specifically relating to a Ti3ZnC2 / Ti3C2T with a multidimensional gradient structure of "three-dimensional / two-dimensional / zero-dimensional". x @Zn y O z Conductivity-enhancing phase materials and their preparation methods. Background Technology
[0002] Electrical contact materials are core functional materials in power switchgear, directly determining the reliability of circuit switching, energy transmission efficiency, and equipment lifespan. They have irreplaceable strategic value in fields such as smart grids, microelectronic devices, high-voltage power transmission and distribution, and rail transportation. As power systems develop towards higher voltage, larger capacity, and higher frequency, electrical contact materials face increasingly stringent performance requirements: they not only need excellent conductivity to reduce contact resistance and Joule heat loss, but also high hardness, wear resistance, and resistance to arc erosion to withstand the mechanical and thermal shocks caused by frequent switching operations.
[0003] Traditional silver-based, copper-based, and tin-based electrical contact materials typically improve their mechanical properties and arc resistance by adding reinforcing phases such as oxides (e.g., CdO, SnO2) or metallic elements (e.g., Ni). However, significant differences in physicochemical properties exist between these reinforcing phases and the base metal (e.g., mismatch in thermal expansion coefficients, poor interfacial wettability), leading to low interfacial bonding strength and discontinuous conductive channels. Under arc erosion, these components are prone to interfacial delamination, material migration, and even welding failure, severely limiting the reliability and service life of electrical contact elements.
[0004] MAX phase materials (M n+1 AX nMAX phases (where M is a transition metal, A is a group IIIA or IVA element, and X is C or N) are a class of conductive ceramic materials with a hexagonal layered structure. Due to their unique chemical bonding mode, they combine the electrical and thermal conductivity of metals with the high hardness and high-temperature resistance of ceramics, and are considered ideal conductive reinforcing phases. In recent years, researchers have studied the substitution process of Al element in Ti3AlC2, a representative material of the family, through the A-position substitution strategy, and successfully developed novel functionalized MAX phase materials. Specifically, Huang Qing et al.'s team first studied and reported the successful preparation of a novel Ti3ZnC2 using a Lewis acid molten salt (such as ZnCl2) in a chemical substitution reaction with Ti3AlC2. After Zn substitution at the A site, Ti3ZnC2 exhibits significantly improved electrical conductivity compared to Ti3AlC2, along with enhanced Vickers hardness and flexural strength, and improved corrosion resistance. This makes Ti3ZnC2 more comprehensively advantageous than the traditional MAX phase in terms of electrical conductivity, mechanical properties, and corrosion resistance, meeting the multidimensional performance requirements of electrical contact materials for reinforcing phases. Therefore, it shows promising application prospects in Ag, Cu, and Sn-based electrical contact material composite systems, combining high conductivity, high resistance to arc erosion, and long service life.
[0005] However, Ti3ZnC2 still faces the following application bottlenecks in its preparation and composite with metal matrices: First, the high viscosity and strong hygroscopicity of ZnCl2 in the reaction medium lead to low molten salt mass transfer efficiency, hindered reactant diffusion, and uncontrollable A-position exchange reaction kinetics, resulting in poor stability of its phase, structure, size, and surface properties, making it difficult to meet the high requirements of composite materials for reinforcing phases; Second, the product is only a single three-dimensional Ti3ZnC2 structure, lacking interface functionalization design, resulting in weak interfacial bonding and poor wettability when composited with Ag, Cu, and Sn matrices, making it prone to interfacial delamination and early failure; It also cannot construct multi-dimensional (three-dimensional / two-dimensional / zero-dimensional) gradient structures, resulting in a lack of synergistic integration among the continuous electron channels required for high conductivity, the flexible buffer interface required for mechanical shock resistance, and the stress dispersion center required to suppress arc thermal stress cracking within the material. Therefore, conductivity, mechanical strength, and arc erosion resistance are mutually constrained, making it difficult to achieve simultaneous improvement in comprehensive performance. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the technical problem to be solved by this invention is to provide a multidimensional gradient structure conductive reinforced phase material and its preparation method. The invention innovatively designs a "three-dimensional / two-dimensional / zero-dimensional" gradient structure, which combines the stability of a three-dimensional structure, the high specific surface area of two-dimensional sheets, and the high surface activity of zero-dimensional nanoparticles. When combined with conductive metals such as silver, copper, and tin, it can significantly improve the interfacial bonding strength, while endowing the composite material with excellent electrical properties, mechanical properties, and resistance to arc erosion.
[0007] The present invention is achieved through the following technical solutions.
[0008] This invention provides a multidimensional gradient structure conductive enhancement phase material, which is Ti3ZnC2 / Ti3C2T x @Zn y O z It has a three-dimensional / two-dimensional / zero-dimensional gradient structure, with the innermost layer being a three-dimensional Ti3ZnC2 structure and the outermost layer being an in-situ constructed two-dimensional layered structure Ti3C2T. x Both have in-situ loaded zero-dimensional nanoparticle structures of Zn on their surfaces. y O z .
[0009] This invention also provides a method for preparing the above-mentioned conductive reinforcing phase material, specifically including the following steps:
[0010] S1: The precursor Ti3AlC2 was subjected to mechanical-plasma synergistic activation treatment to introduce Al vacancy defects on its surface, thus obtaining defective Ti3AlC2 powder.
[0011] S2: The powder obtained above is mixed with a pore-forming agent, and a columnar sample is formed by cold isostatic pressing using a molybdenum wire as the current collector, as a porous electrode sample.
[0012] S3: The above porous electrode sample, together with the counter electrode and the reference electrode, was placed in molten salt to carry out an electrochemical molten salt replacement reaction. After the reaction was completed, post-processing was performed to obtain the three-dimensional structure Ti3ZnC2.
[0013] S4: The powder obtained above is ultrasonically dispersed in a buffer solution containing hydroxycarboxylic acid, followed by photochemical etching and oxidation treatment, washing, and vacuum drying to obtain the Ti3ZnC2 / Ti3C2T. x @Zn y O z Conductivity-enhancing phase material.
[0014] Preferably, step S1 includes the following steps and parameters: First, Ti3AlC2 powder and anhydrous ethanol are mixed in a mortar and pestle mill at a mass ratio of 1:(0.5~1) at a speed of 30~80 rpm for a total mixing time of 0.5~2.5 h. Then, the mixture is vacuum dried and sieved to obtain pretreated powder with a particle size of 2~50 μm. Next, the pretreated powder is placed in an RF plasma chamber... Processing under a mixed atmosphere With a content of 5 vol.%~15 vol.%, a chamber pressure of 30~50 Pa, a radio frequency power of 50~150 W, and a processing time of 30~60 min, defect-type Ti3AlC2 powder with Al vacancies on the surface was obtained.
[0015] Preferably, step S2 includes the following steps and parameters: the pore-forming agent is one or more of NaCl, LiCl, and KCl, and the mass ratio of defective Ti3AlC2 powder to the pore-forming agent is (8~9): (1~2); the cold isostatic pressing pressure is 50~100 MPa, the holding time is 3~7 min, and the porosity of the porous electrode is 30%~40%.
[0016] Preferably, in step S3, the counter electrode is a high-purity zinc rod with a surface covered with a molybdenum mesh with a pore size of 0.2 mm, the reference electrode is a high-temperature resistant Ag / AgCl reference electrode for molten salt, and the molten salt is a ternary molten salt of LiCl-KCl-NaCl with a mass ratio of LiCl:NaCl:KCl=(40~45):(8~10):(50~55).
[0017] Preferably, in step S3, the electrochemical molten salt replacement reaction includes the following steps and parameters: The reaction is carried out in a vertical high-temperature molten salt reactor. First, the bottom ends of the three electrodes from step S3 are placed 3-6 cm above the molten salt surface. Then, under Ar atmosphere protection, the temperature is increased to 350-400℃ at a rate of 3-6℃ / min and held for 30-60 min to melt the molten salt. Next, the three electrodes are placed 1.5-2.5 cm below the molten salt surface (ensuring the bottom of the electrodes is >1 cm from the bottom of the crucible), and the temperature is further increased to 400-450℃ at a rate of 2-5℃ / min. Pulse potential control is used, with a high potential of +0.7-+0.9 V, a low potential of +0.1-+0.2 V, a pulse period of 10-20 s, and a total reaction time of 4-8 h.
[0018] Preferably, in step S3, the post-processing includes: first, dissolving the cooled reaction product in deionized water at 80-100℃ to remove the molten salt, then removing the supernatant after standing, repeating the operation 4-6 times; then centrifuging and washing at 6000-10000 rpm for 3-10 min, repeating the operation 3-5 times until the conductivity of the supernatant is <38 μS / cm; finally, performing vacuum freeze-drying on the product for 6-10 h, with a cold trap temperature of -50℃ and a vacuum degree <10 Pa, to obtain the three-dimensional structure Ti3ZnC2.
[0019] Preferably, in step S4, the specific process of ultrasonic dispersion is as follows: the three-dimensional structure Ti3ZnC2 obtained in step S3 is added to a buffer solution with a mass concentration of 15~25 mg / mL, and ultrasonically dispersed for 10~20 min at a power of 145~245 W and a frequency of 40 kHz to obtain a uniform suspension.
[0020] Preferably, in step S4, the photochemical etching oxidation treatment includes the following steps and parameters: a uniform suspension containing Ti3ZnC2 is reacted in an ice bath under the protection of an O2 / Ar mixed gas, wherein the O2 volume fraction is 0.5%~5%, the ultraviolet light wavelength is 365 nm, the irradiance is 50~150 mW / cm², and the reaction time is 2.5~3.5 h, ultimately obtaining a three-dimensional / two-dimensional / zero-dimensional gradient structure Ti3ZnC2 / Ti3C2T x @Zn y O z Reinforcing phase materials.
[0021] The innovativeness of this invention is as follows:
[0022] To address the two application bottlenecks mentioned in the background art regarding the preparation and composite with metal matrices of Ti3ZnC2, this invention innovatively proposes the following corresponding solutions: For bottleneck one, a mechanical activation pretreatment combined with a low-viscosity mixed molten salt system is used to replace the high-viscosity ZnCl2, improving molten salt mass transfer kinetics and achieving uniform and controllable A-site substitution reaction; For bottleneck two, a surface modification process is introduced after the substitution reaction to grow two-dimensional Ti3C2T on the Ti3ZnC2 surface in situ. x Layers and zero-dimensional ZnO nanoparticles construct a multi-dimensional gradient structure. Among them, three-dimensional Ti3ZnC2 provides a continuous conductive framework and load-bearing body, while two-dimensional Ti3C2T... x The lamellar structure provides flexible interfacial buffers and chemical bonding sites—enhancing the interfacial bonding strength with Ag, Cu, and Sn matrices while also providing internal flexibility. Zero-dimensional ZnO nanoparticles provide highly active interfaces and stress dispersion centers, suppressing arc-induced thermal stress cracking. These three elements work synergistically to address both weak interfacial bonding and the lack of internal multifunctional synergy, achieving simultaneous improvements in conductivity, mechanical strength, and arc erosion resistance. This meets the future demanding application requirements of electrical contact materials for high performance, high reliability, and long lifespan under demanding service conditions.
[0023] Compared with the prior art, the present invention has the following technical effects:
[0024] 1. This invention uses Ti3AlC2 as a precursor and prepares a multi-dimensional gradient structure conductive enhancement phase material with "three-dimensional / two-dimensional / zero-dimensional" structures through "mechanical-plasma synergistic activation-electrochemical molten salt replacement-photochemical etching oxidation". The innermost layer is a three-dimensional Ti3ZnC2 structure, and the outermost layer is an in-situ constructed two-dimensional layered structure Ti3C2T x Both have in-situ loaded zero-dimensional nanoparticle structures of Zn on their surfaces. y O zWhen combined with conductive metals such as Ag, Cu, and Sn, this gradient structure achieves multi-level synergistic enhancement: the three-dimensional structure provides a continuous conductive path and mechanical support, the two-dimensional sheets strengthen the interface bonding and inhibit crack propagation with their high specific surface area, and the zero-dimensional particles enhance interface anchoring and disperse arc erosion energy with their high surface activity, thereby significantly improving the electrical and mechanical properties of the composite material, while also improving its resistance to arc erosion.
[0025] 2. The preparation process of the present invention is simple and energy-efficient, making it easy to industrialize. When this multi-dimensional gradient structure conductive reinforcing phase material is combined with conductive metals such as silver, copper, and tin, it is easy to form a strong interfacial bond and maintain a continuous conductive channel. At the same time, with the help of the flexible buffer of the two-dimensional sheets and the stress dispersion effect of the zero-dimensional particles, the mechanical properties and arc erosion resistance of the composite material are improved simultaneously.
[0026] 3. This invention boasts advanced technology, controllable cost, and promising engineering application prospects. Compared to composite materials prepared by combining the multidimensional gradient structure conductive reinforcing phase material of this invention with conductive metal powders such as Ag, Cu, and Sn, and metal-based electrical contact composite materials reinforced with the original MAX phase powder, as well as commercial metal-based electrical contact composite materials, the composite material using this "three-dimensional / two-dimensional / zero-dimensional" multidimensional gradient structure reinforcing phase with the Ag, Cu, and Sn matrix can significantly enhance interfacial bonding strength, electrical and thermal conductivity, and resistance to arc erosion. It has enormous potential to replace traditional electrical contact materials in fields such as power switchgear, electrical contact elements, new energy power transmission and distribution systems, and microelectronic devices. Attached Figure Description
[0027] Figure 1 The precursor A (Ti3AlC2), electrochemical molten salt substitution product B (Ti3ZnC2), and final product C (Ti3ZnC2 / Ti3C2T) in Example 3 of this invention are used. x XRD pattern of ZnO.
[0028] As shown in the figure, the diffraction peaks of precursor A completely match the characteristic diffraction peaks of Ti3AlC2 and there are no other impurity peaks, indicating that A is a high-purity Ti3AlC2. Meanwhile, the diffraction peaks of product B, obtained through electrochemical molten salt replacement, completely match the characteristic diffraction peaks of Ti3ZnC2 and there are no impurity peaks, indicating that Zn in the molten salt completely replaces Al in Ti3AlC2. The characteristic diffraction peaks of the final product C, prepared by photochemical etching oxidation, match both Ti3ZnC2 and Ti3C2T. x Characteristic diffraction peaks were observed, and a weak characteristic diffraction peak of ZnO was detected. Furthermore, no characteristic diffraction peaks of the precursor Ti3AlC2 or other impurity phases were detected in product C. Therefore, it was confirmed that the final phase obtained was Ti3ZnC2 / Ti3C2T. x @ZnO.
[0029] Figure 2 SEM image of the "three-dimensional / two-dimensional / zero-dimensional" multi-dimensional gradient structure conductive enhancement phase material prepared in Example 3 of the present invention.
[0030] As shown in the figure, the product maintains the macroscopic three-dimensional bulk skeleton structure, with the outer layer being a two-dimensional layered structure Ti3C2T. x Zero-dimensional ZnO nanoparticles were randomly loaded onto three-dimensional Ti3ZnC2 and two-dimensional Ti3C2T. x The surface forms a clear three-dimensional / two-dimensional / zero-dimensional multi-dimensional gradient structure.
[0031] Figure 3 TEM image of the "three-dimensional / two-dimensional / zero-dimensional" multi-gradient structure conductive enhancement phase material prepared in Example 3 of this invention; Figure 3 (a) Ti3ZnC2 / Ti3C2T under low magnification x TEM image of the overall structural features of ZnO; Figure 3 (b) is Figure 3 (a) Enlarged view; Figure 3 (c) is Figure 3 (b) Enlarged view.
[0032] As can be seen from the figure: Figure 3 (a) Demonstrates the final product Ti3ZnC2 / Ti3C2T prepared by the method of the present invention at low magnification. x The overall structural characteristics of @ZnO are that its size is approximately 2~3 μm. And... Figure 3 (b) Under medium to high magnification, a solid Ti3ZnC2 crystal was observed inside, with obvious two-dimensional Ti3C2T crystals visible on its surface. x Layered structure, and Ti3C2T x The outermost surface of the lamellar structure shows clearly visible ZnO nanoparticles. At even higher magnification... Figure 3 (c) shows that the Ti3ZnC2 surface Ti3C2T x The thickness of the layers is approximately 20~100 nm, while Ti3C2T x The ZnO nanoparticles distributed on the outermost surface of the lamellae have a diameter of approximately 20–50 nm.
[0033] Figure 4 Ti3ZnC2 / Ti3C2T prepared for embodiments of the present invention x @Zn y O z A schematic diagram of the structure of an electrical contact material formed by combining a multidimensional gradient structure conductive enhancement phase material with an Ag, Cu, and Sn matrix.
[0034] As shown in the figure, this conductive reinforcing phase material maintains the macroscopic three-dimensional Ti3ZnC2 bulk framework structure, with its outer layer being a two-dimensional Ti3C2T.x Layered structure; zero-dimensional Zn y O z Nanoparticles are randomly loaded onto a three-dimensional Ti3ZnC2 framework and a two-dimensional Ti3C2T framework. x On the surface of the lamellar material, a clear three-dimensional / two-dimensional / zero-dimensional multi-dimensional gradient structure is formed. This multi-dimensional gradient structure, which enhances conductivity, is dispersed within the Ag, Cu, and Sn matrix to form a composite electrical contact material. Detailed Implementation
[0035] The present invention will now be described in more detail with reference to the accompanying drawings.
[0036] Example 1
[0037] Ti3AlC2 powder was mixed with anhydrous ethanol at a mass ratio of 1:0.5 and placed in a mortar and pestle mill at 30 rpm for a total mixing time of 2.5 h. The mixture was then vacuum dried and sieved to obtain a pretreated powder with a particle size of 50 μm. The pretreated powder was then placed in an RF plasma chamber... Mixed atmosphere ( A defective Ti3AlC2 powder with Al vacancies on its surface was obtained by treating the sample for 60 min at a concentration of 5 vol.%, chamber pressure of 30 Pa, and RF power of 50 W. The defective Ti3AlC2 powder was then mixed with NaCl at a mass ratio of 8:1. Using molybdenum wire as the current collector, the mixture was cold isostatically pressed at 50 MPa for 3 min to form a columnar sample, which served as a porous electrode sample. The porosity of the obtained porous electrode was 40%. An electrochemical molten salt replacement reaction was carried out in a vertical high-temperature molten salt reactor equipped with a three-electrode system. The reactor included a vertical quartz reaction tube, a surrounding heating furnace body, and a water-cooled sealing flange. The molten salt was a ternary molten salt of LiCl-KCl-NaCl (mass ratio LiCl:NaCl:KCl=40:10:50). The working electrode (porous electrode sample) and the counter electrode (surface coated with pores of 0.2 mm) were used. The high-purity zinc rod (mm molybdenum mesh) and reference electrode (high-temperature resistant Ag / AgCl reference electrode for molten salt) are inserted and fixed to the lifting mechanism through the electrode lead interface on the water-cooled flange, so that the lower end of the electrode is initially 3 cm above the molten salt surface. Under Ar atmosphere protection, the temperature is increased to 350℃ at a rate of 3℃ / min and held for 60 min to melt the molten salt. Then, the electrode is lowered to 1.5 cm below the molten salt surface through the lifting mechanism (ensuring that the lower end of the electrode is >1 cm from the bottom of the crucible). The temperature is then increased to 400℃ at a rate of 2℃ / min, using pulse potential control, with a high potential of +0.7 V and a low potential of +0.1 V, a pulse period of 10 s, and a total reaction time of 8 h. After the reaction is completed, the cooled reaction product is dissolved in 80℃ deionized water to remove the molten salt. After standing, the supernatant is removed. This operation is repeated 6 times, and then the product is centrifuged at 6000 rpm for 3 minutes. The process was repeated 5 times until the conductivity of the supernatant was <38 μS / cm. Finally, the product was freeze-dried under vacuum for 6 h (cold trap temperature -50℃, vacuum degree <10 Pa) to obtain a three-dimensional Ti3ZnC2 structure. The obtained three-dimensional Ti3ZnC2 structure was added to a buffer solution containing hydroxycarboxylic acid (citric acid, concentration 0.5 wt%) (containing the corresponding citrate, acid to salt molar ratio 1:0.3, pH 4.5), at a mass concentration of 15 mg / mL. The solution was ultrasonically dispersed for 10 min at a power of 145 W and a frequency of 40 kHz to obtain a homogeneous suspension. The Ti3ZnC2 homogeneous suspension was reacted in an ice bath under O2 / Ar mixed gas protection (O2 volume fraction 5%, UV wavelength 365 nm, irradiance 50 mW / cm²) for 3.5 h. After the reaction, the product was washed and vacuum-dried (temperature 50℃, vacuum degree <10 Pa, time 6 h). h) then the Ti3ZnC2 / Ti3C2T is obtained. x @Zn 0.8 O 1.3Conductivity-enhancing phase material, in which Zn 0.8 O 1.3 The nanoparticles have a particle size of 20 nm and a y / u ratio of 0.62. The prepared Ti3ZnC2 / Ti3C2T... x @Zn 0.8 O 1.3 The conductive reinforcing phase material and Ag powder were wet-mixed at a mass ratio of 1:9 for 40 min and dried for 12 h. The mixed powder was first placed into a mold and cold-pressed (850 MPa, 5 min), then heat-treated at 600℃ for 1.5 h in an Ar atmosphere, then cold-pressed again (850 MPa, 5 min), and then heat-treated at 300℃ for 6 h in an Ar atmosphere. Finally, it was re-pressed (950 MPa, 5 min) to obtain the Ag-based electrical contact composite material.
[0038] Example 2
[0039] Ti3AlC2 powder was mixed with anhydrous ethanol at a mass ratio of 1:1 and placed in a mortar and pestle mill at 55 rpm for a total mixing time of 0.5 h. The mixture was then vacuum dried and sieved to obtain a pretreated powder with a particle size of 38 μm. The pretreated powder was then placed in an RF plasma chamber... Mixed atmosphere ( The Ti3AlC2 powder with Al vacancies on its surface was obtained by treating it for 30 min at a content of 15 vol.%, chamber pressure of 50 Pa, and radio frequency power of 150 W. The defective Ti3AlC2 powder was then mixed with pore-forming agent KCl at a mass ratio of 8:2. The mixture was then cold isostatically pressed at 100 MPa for 7 min using molybdenum wire as the current collector to form a columnar sample as a porous electrode sample. The porosity of the obtained porous electrode was 30%. The molten salt was a ternary molten salt of LiCl-KCl-NaCl (mass ratio LiCl:NaCl:KCl=45:8:55). The working electrode (porous electrode sample), the counter electrode (high-purity zinc rod with a surface covered with a 0.2 mm molybdenum mesh), and the reference electrode (high-temperature resistant Ag / AgCl reference electrode for molten salt) were inserted and fixed to the lifting mechanism through the electrode lead interface on the water-cooled flange, so that the initial position of the lower end of the electrode was 6 cm above the molten salt surface. Under Ar atmosphere protection, the sample was cold isostatically pressed at 100 MPa for 7 min to form a columnar sample as a porous electrode sample. The temperature was increased to 400℃ at a rate of ℃ / min and held for 30 min to melt the molten salt. Then, the electrode was lowered to 2.5 cm below the molten salt surface using the lifting mechanism (ensuring the lower end of the electrode was >1 cm from the bottom of the crucible). The temperature was then increased to 450℃ at a rate of 5 ℃ / min, using pulse potential control with a high potential of +0.9 V and a low potential of +0.2 V, a pulse period of 10 s, and a total reaction time of 4 h. After the reaction was complete, the cooled reaction product was dissolved in 100℃ deionized water to remove the molten salt. After standing, the supernatant was removed. This process was repeated 4 times. The product was then centrifuged at 10000 rpm for 3 min, and this process was repeated 3 times until the conductivity of the supernatant was <38 μS / cm. Finally, the product was freeze-dried under vacuum for 6 h (cold trap temperature -50℃, vacuum <10 Pa) to obtain a three-dimensional Ti3ZnC2 structure. The obtained Ti3ZnC2 powder was then subjected to a process containing hydroxycarboxylic acid (gluconic acid, concentration 2...). The Ti3ZnC2 was ultrasonically dispersed in a buffer solution (containing the corresponding gluconate, with an acid-to-salt molar ratio of 1:1 and a pH of 5.5) at a mass concentration of 25 mg / mL, under ultrasonic dispersion conditions of 245 W and 40 kHz for 20 min to obtain a homogeneous suspension. The Ti3ZnC2-containing homogeneous suspension was then reacted in an ice bath under O2 / Ar gas protection, with an O2 volume fraction of 0.5%, an ultraviolet wavelength of 365 nm, and an irradiance of 150 mW / cm² for 2.5 h. After the reaction, the mixture was washed and vacuum dried (temperature 50℃, vacuum degree <10 Pa, time 12 h) to obtain the Ti3ZnC2 / Ti3C2T. x @Zn 1.2 O 0.8 Conductivity-enhancing phase material, in which Zn 1.2 O 0.8The nanoparticles have a particle size of 50 nm and a y / u ratio of 1.5. The prepared Ti3ZnC2 / Ti3C2T... x @Zn 1.2 O 0.8 The conductive reinforcing phase material and Ag powder were wet-mixed at a mass ratio of 1:9 for 40 min and dried for 12 h. The mixed powder was first placed into a mold and cold-pressed (850 MPa, 5 min), then heat-treated at 600℃ for 1.5 h in an Ar atmosphere, then cold-pressed again (850 MPa, 5 min), and then heat-treated at 300℃ for 6 h in an Ar atmosphere. Finally, it was re-pressed (950 MPa, 5 min) to obtain the Ag-based electrical contact composite material.
[0040] Example 3
[0041] Ti3AlC2 powder was mixed with anhydrous ethanol at a mass ratio of 1:0.75 and placed in a mortar and pestle mill at 80 rpm for a total mixing time of 1.5 h. The mixture was then vacuum dried and sieved to obtain a pretreated powder with a particle size of 2 μm. The pretreated powder was then placed in an RF plasma chamber... Mixed atmosphere ( A defective Ti3AlC2 powder with Al vacancies on its surface was obtained by treating the sample for 45 min at a concentration of 10 vol.%, chamber pressure of 40 Pa, and radio frequency power of 100 W. The defective Ti3AlC2 powder was then mixed with a pore-forming agent mixture of NaCl and KCl at a mass ratio of 9:1. Using a molybdenum wire as the current collector, the mixture was cold isostatically pressed at 75 MPa for 5 min to form a columnar sample, which served as a porous electrode sample. The porosity of the obtained porous electrode was 45%. The molten salt was a ternary molten salt of LiCl-KCl-NaCl (mass ratio LiCl:NaCl:KCl=42:9:52). The working electrode (porous electrode sample), the counter electrode (high-purity zinc rod with a surface covered with a 0.2 mm molybdenum mesh), and the reference electrode (high-temperature resistant Ag / AgCl reference electrode for molten salt) were inserted into and fixed to the lifting mechanism through the electrode lead interface on the water-cooled flange, with the initial position of the lower end of the electrode 4.5 mm above the molten salt surface. Under Ar atmosphere protection, the temperature was increased to 375℃ at a rate of 4.5℃ / min and held for 45 min to melt the molten salt. Then, the electrode was lowered to 2.0 cm below the molten salt surface using the lifting mechanism (ensuring the lower end of the electrode is >1 cm from the bottom of the crucible). The temperature was then increased to 425℃ at a rate of 3.5℃ / min, using pulse potential control with a high potential of +0.8 V and a low potential of +0.15 V, a pulse period of 15 s, and a total reaction time of 6 h. After the reaction was complete, the cooled reaction product was dissolved in 90℃ deionized water to remove the molten salt. After standing, the supernatant was removed. This process was repeated 5 times, followed by centrifugation at 8000 rpm for 4 min, repeated 4 times until the conductivity of the supernatant was <38 μS / cm. Finally, the product was freeze-dried under vacuum for 8 h (cold trap temperature -50℃, vacuum <10). The three-dimensional structure Ti3ZnC2 was obtained by ultrasonic dispersion in a buffer solution containing hydroxycarboxylic acid (tartaric acid, concentration 1.25 wt%) (containing the corresponding tartrate, with an acid-to-salt molar ratio of 1:0.65 and a pH of 5.0) at a mass concentration of 20 mg / mL, a power of 195 W, and a frequency of 40 kHz for 15 min to obtain a homogeneous suspension. The homogeneous suspension containing Ti3ZnC2 was reacted in an ice bath under O2 / Ar mixed gas protection, where the O2 volume fraction was 2.75%, the ultraviolet wavelength was 365 nm, the irradiance was 100 mW / cm², and the reaction time was 3 h. After the reaction was completed, the mixture was washed and vacuum dried (temperature 50℃, vacuum degree <10 Pa, time 12 h) to obtain the Ti3ZnC2 / Ti3C2T. x The material is a ZnO conductive reinforcing phase material, wherein the ZnO nanoparticles have a particle size of 35 nm and y / u = 1.0. The prepared Ti3ZnC2 / Ti3C2T... x@ZnO conductive reinforcing phase material and Ag powder were wet-mixed at a mass ratio of 1:9 for 40 min and dried for 12 h. The mixed powder was first placed into a mold and cold-pressed (850 MPa, 5 min), then heat-treated at 600℃ for 1.5 h in an Ar atmosphere, then cold-pressed again (850 MPa, 5 min), and then heat-treated at 300℃ for 6 h in an Ar atmosphere. Finally, it was re-pressed (950 MPa, 5 min) to obtain Ag-based electrical contact composite material.
[0042] Example 4
[0043] Ti3AlC2 powder was mixed with anhydrous ethanol at a mass ratio of 1:0.6 and placed in a mortar and pestle mill at 40 rpm for a total mixing time of 2.0 h. The mixture was then vacuum dried and sieved to obtain a pretreated powder with a particle size of 45 μm. The pretreated powder was then placed in an RF plasma chamber... Mixed atmosphere ( The Ti3AlC2 powder with Al vacancies on its surface was obtained by treating it for 40 min at a content of 8 vol.%, a chamber pressure of 35 Pa, and a radio frequency power of 75 W. The defective Ti3AlC2 powder was then mixed with NaCl at a mass ratio of 9:2. Using molybdenum wire as the current collector, it was cold isostatically pressed at 60 MPa for 6 min to form a columnar sample as a porous electrode sample. The porosity of the obtained porous electrode was 35%. The molten salt was a ternary molten salt of LiCl-KCl-NaCl (mass ratio LiCl:NaCl:KCl=41:9:50). The working electrode (porous electrode sample), the counter electrode (high-purity zinc rod with a surface covered with a 0.2 mm molybdenum mesh), and the reference electrode (high-temperature resistant Ag / AgCl reference electrode for molten salt) were inserted into and fixed on the lifting mechanism through the electrode lead interface on the water-cooled flange, so that the initial position of the lower end of the electrode was 4.0 cm above the molten salt surface. Under Ar atmosphere protection, the electrode was pressed at 4.0 cm. The temperature was increased to 360℃ at a rate of ℃ / min and held for 55 min to melt the molten salt. Then, the electrode was lowered to 1.8 cm below the molten salt surface using the lifting mechanism (ensuring the lower end of the electrode was >1 cm from the bottom of the crucible). The temperature was then increased to 420℃ at a rate of 3.0 ℃ / min, using pulse potential control with a high potential of +0.75 V and a low potential of +0.12 V, a pulse period of 12 s, and a total reaction time of 7 h. After the reaction, the cooled reaction product was dissolved in 85℃ deionized water to remove the molten salt. After standing, the supernatant was removed. This process was repeated 4 times. The product was then centrifuged at 7000 rpm for 4 min, and this process was repeated 4 times until the conductivity of the supernatant was <38 μS / cm. Finally, the product was freeze-dried under vacuum for 7 h (cold trap temperature -50℃, vacuum <10 Pa) to obtain a three-dimensional Ti3ZnC2 structure. The obtained Ti3ZnC2 powder was then subjected to a process containing hydroxycarboxylic acid (malic acid, concentration 0.8%). The Ti3ZnC2 was ultrasonically dispersed in a buffer solution (containing the corresponding malate, with an acid-to-salt molar ratio of 1:0.4 and a pH of 4.7) at a mass concentration of 17 mg / mL, under ultrasonic dispersion conditions of 165 W and 40 kHz for 12 min to obtain a homogeneous suspension. The Ti3ZnC2-containing homogeneous suspension was then reacted in an ice bath under O2 / Ar gas protection (1% O2 volume fraction), with an ultraviolet wavelength of 365 nm and an irradiance of 75 mW / cm² for 3.5 h. After the reaction, the mixture was washed and vacuum dried (50℃, <10 Pa, 7 h) to obtain the Ti3ZnC2 / Ti3C2T. x @Zn 0.9 O 1.1 Conductivity-enhancing phase material, in which Zn 0.9 O 1.1The nanoparticles have a particle size of 25 nm and a y / u ratio of 0.82. The prepared Ti3ZnC2 / Ti3C2T... x @Zn 0.9 O 1.1 The conductive reinforcing phase material and Cu powder were wet-mixed at a mass ratio of 1:9 for 40 min and dried for 12 h. The mixed powder was first placed into a mold and cold-pressed (850 MPa, 5 min), then heat-treated at 600℃ for 1.5 h in an Ar atmosphere, then cold-pressed again (850 MPa, 5 min), and then heat-treated at 300℃ for 6 h in an Ar atmosphere. Finally, it was re-pressed (950 MPa, 5 min) to obtain the Cu-based electrical contact composite material.
[0044] Example 5
[0045] Ti3AlC2 powder was mixed with anhydrous ethanol at a mass ratio of 1:0.9 and placed in a mortar and pestle mill at 70 rpm for a total mixing time of 1 h. The mixture was then vacuum dried and sieved to obtain a pretreated powder with a particle size of 15 μm. The pretreated powder was then placed in an RF plasma chamber and... Mixed atmosphere ( A defective Ti3AlC2 powder with Al vacancies on its surface was obtained by treating the sample for 50 min at a content of 12 vol.%, chamber pressure of 45 Pa, and radio frequency power of 125 W. The defective Ti3AlC2 powder was then mixed with pore-forming agent KCl at a mass ratio of 8:2. Using molybdenum wire as the current collector, the mixture was cold isostatically pressed at 85 MPa for 4 min to form a columnar sample, which served as a porous electrode sample. The porosity of the obtained porous electrode was 45%. The molten salt was a ternary molten salt of LiCl-KCl-NaCl (mass ratio LiCl:NaCl:KCl=44:8:48). The working electrode (porous electrode sample), the counter electrode (high-purity zinc rod with a surface covered with a 0.2 mm molybdenum mesh), and the reference electrode (high-temperature resistant Ag / AgCl reference electrode for molten salt) were inserted into and fixed on the lifting mechanism through the electrode lead interface on the water-cooled flange, so that the initial position of the lower end of the electrode was 5.5 cm above the molten salt surface. Under Ar atmosphere protection, the sample was heated to a height of 5.5 cm. The temperature was increased to 385℃ at a rate of ℃ / min and held for 45 min to melt the molten salt. Then, the electrode was lowered to 2.3 cm below the molten salt surface using the lifting mechanism (ensuring the lower end of the electrode was >1 cm from the bottom of the crucible). The temperature was then increased to 435℃ at a rate of 4.5 ℃ / min, using pulse potential control with a high potential of +0.85 V and a low potential of +0.18 V, a pulse period of 18 s, and a total reaction time of 5 h. After the reaction, the cooled reaction product was dissolved in 95℃ deionized water to remove the molten salt, and the supernatant was removed by standing. This process was repeated 5 times. The product was then centrifuged at 9000 rpm for 8 min, and this process was repeated 4 times until the conductivity of the supernatant was <38 μS / cm. Finally, the product was freeze-dried under vacuum for 9 h (cold trap temperature -50℃, vacuum <10 Pa) to obtain a three-dimensional Ti3ZnC2 structure. The obtained Ti3ZnC2 powder was then subjected to a process containing hydroxycarboxylic acid (a mixture of citric acid and gluconic acid, with a total concentration of 1.5%). The Ti3ZnC2 was ultrasonically dispersed in a buffer solution (containing the corresponding carboxylate, with an acid-to-salt molar ratio of 1:0.8 and a pH of 5.2) at a mass concentration of 23 g / L, a power of 220 W, and a frequency of 40 kHz for 18 min to obtain a homogeneous suspension. The Ti3ZnC2-containing homogeneous suspension was then reacted in an ice bath under O2 / Ar gas protection (4% O2 volume fraction), with an ultraviolet wavelength of 365 nm and an irradiance of 130 mW / cm² for 3.5 h. After the reaction, the mixture was washed and vacuum dried (50℃, vacuum <10 Pa, time 7 h) to obtain the Ti3ZnC2 / Ti3C2T. x @Zn 1.1 O 0.9 Conductivity-enhancing phase material, in which Zn 1.1 O 0.9The nanoparticles have a particle size of 42 nm and y / u = 1.22. The prepared Ti3ZnC2 / Ti3C2T... x @Zn 1.1 O 0.9 The conductive reinforcing phase material and Ag powder were wet-mixed at a mass ratio of 1:9 for 40 min and dried for 12 h. The mixed powder was first placed into a mold and cold-pressed (850 MPa, 5 min). Then, it was heat-treated at 600℃ for 1.5 h in an Ar atmosphere, cold-pressed again (850 MPa, 5 min), and then heat-treated at 300℃ for 6 h in an Ar atmosphere. Finally, it was re-pressed (950 MPa, 5 min) to obtain the Ag-based electrical contact composite material.
[0046] Example 6
[0047] Ti3AlC2 powder was mixed with anhydrous ethanol at a mass ratio of 1:0.75 and placed in a mortar and pestle mill at 80 rpm for a total mixing time of 1.5 h. The mixture was then vacuum dried and sieved to obtain a pretreated powder with a particle size of 2 μm. The pretreated powder was then placed in an RF plasma chamber... Mixed atmosphere ( A defective Ti3AlC2 powder with Al vacancies on its surface was obtained by treating the sample for 45 min at a concentration of 10 vol.%, chamber pressure of 40 Pa, and radio frequency power of 100 W. The defective Ti3AlC2 powder was then mixed with a pore-forming agent mixture of NaCl and KCl at a mass ratio of 9:1. Using a molybdenum wire as the current collector, the mixture was cold isostatically pressed at 75 MPa for 5 min to form a columnar sample, which served as a porous electrode sample. The porosity of the obtained porous electrode was 45%. The molten salt was a ternary molten salt of LiCl-KCl-NaCl (mass ratio LiCl:NaCl:KCl=42:9:52). The working electrode (porous electrode sample), the counter electrode (high-purity zinc rod with a surface covered with a 0.2 mm molybdenum mesh), and the reference electrode (high-temperature resistant Ag / AgCl reference electrode for molten salt) were inserted into and fixed to the lifting mechanism through the electrode lead interface on the water-cooled flange, with the initial position of the lower end of the electrode 4.5 mm above the molten salt surface. Under Ar atmosphere protection, the temperature was increased to 375℃ at a rate of 4.5℃ / min and held for 45 min to melt the molten salt. Then, the electrode was lowered to 2.0 cm below the molten salt surface using the lifting mechanism (ensuring the lower end of the electrode is >1 cm from the bottom of the crucible). The temperature was then increased to 425℃ at a rate of 3.5℃ / min, using pulse potential control with a high potential of +0.8 V and a low potential of +0.15 V, a pulse period of 15 s, and a total reaction time of 6 h. After the reaction was complete, the cooled reaction product was dissolved in 90℃ deionized water to remove the molten salt. After standing, the supernatant was removed. This process was repeated 5 times, followed by centrifugation at 8000 rpm for 4 min. This process was repeated 4 times until the conductivity of the supernatant was <38 μS / cm. Finally, the product was freeze-dried under vacuum for 8 h (cold trap temperature -50℃, vacuum <10). The three-dimensional structure Ti3ZnC2 was obtained by ultrasonic dispersion in a buffer solution containing hydroxycarboxylic acid (tartaric acid, concentration 1.25 wt%) (containing the corresponding tartrate, with an acid-to-salt molar ratio of 1:0.65 and a pH of 5.0) at a mass concentration of 20 mg / mL, a power of 195 W, and a frequency of 40 kHz for 15 min to obtain a homogeneous suspension. The homogeneous suspension containing Ti3ZnC2 was reacted in an ice bath under O2 / Ar mixed gas protection, where the O2 volume fraction was 2.75%, the ultraviolet wavelength was 365 nm, the irradiance was 100 mW / cm², and the reaction time was 3 h. After the reaction was completed, the mixture was washed and vacuum dried (temperature 50℃, vacuum degree <10 Pa, time 12 h) to obtain the Ti3ZnC2 / Ti3C2T. x The material is a ZnO conductive reinforcing phase material, wherein the ZnO nanoparticles have a particle size of 35 nm and y / u = 1.0. The prepared Ti3ZnC2 / Ti3C2T... x@ZnO conductive reinforcing phase material and Sn powder were wet-mixed at a mass ratio of 1:9 for 40 min and dried for 12 h. The mixed powder was first placed into a mold and cold-pressed (850 MPa, 5 min), then heat-treated at 600℃ for 1.5 h in an Ar atmosphere, then cold-pressed again (850 MPa, 5 min), and then heat-treated at 300℃ for 6 h in an Ar atmosphere. Finally, it was re-pressed (950 MPa, 5 min) to obtain Sn-based electrical contact composite material.
[0048] Comparative Example 1
[0049] Ti3ZnC2 powder and Ag powder were wet-mixed at a mass ratio of 1:9 for 40 min and dried for 12 h. The mixed powder was first placed into a mold and cold-pressed (850 MPa, 5 min), then heat-treated at 600℃ for 1.5 h in an Ar atmosphere, then cold-pressed again (850 MPa, 5 min), and then heat-treated at 300℃ for 6 h in an Ar atmosphere. Finally, it was re-pressed (950 MPa, 5 min) to obtain the Ag-based electrical contact composite material.
[0050] Comparative Example 2
[0051] Ti3ZnC2 powder and Cu powder were wet-mixed at a mass ratio of 1:9 for 40 min and dried for 12 h. The mixed powder was first cold-pressed into a mold (850 MPa, 5 min), then heat-treated at 600℃ for 1.5 h in an Ar atmosphere, then cold-pressed again (850 MPa, 5 min), and then heat-treated at 300℃ for 6 h in an Ar atmosphere. Finally, the mixture was re-pressed (950 MPa, 5 min) to obtain the Cu-based electrical contact composite material.
[0052] Comparative Example 3
[0053] Ti3ZnC2 powder and Sn powder were wet-mixed at a mass ratio of 1:9 for 40 min and dried for 12 h. The mixed powder was first cold-pressed into a mold (850 MPa, 5 min), then heat-treated at 600℃ for 1.5 h in an Ar atmosphere, then cold-pressed again (850 MPa, 5 min), and then heat-treated at 300℃ for 6 h in an Ar atmosphere. Finally, the Sn-based electrical contact composite material was obtained by re-pressing (950 MPa, 5 min).
[0054] Comparative Example 4
[0055] ZnO powder and Sn powder were wet-mixed at a mass ratio of 1:9 for 40 min and dried for 12 h. The mixed powder was first cold-pressed into a mold (850 MPa, 5 min), then heat-treated at 600℃ for 1.5 h in an Ar atmosphere, then cold-pressed again (850 MPa, 5 min), and then heat-treated at 300℃ for 6 h in an Ar atmosphere. Finally, the Sn-based electrical contact composite material was obtained by re-pressing (950 MPa, 5 min).
[0056] Comparative Example 5
[0057] ZnO powder and Ag powder were wet-mixed at a mass ratio of 1:9 for 40 min and dried for 12 h. The mixed powder was first placed into a mold and cold-pressed (850 MPa, 5 min), then heat-treated at 600℃ for 1.5 h in an Ar atmosphere, then cold-pressed again (850 MPa, 5 min), and then heat-treated at 300℃ for 6 h in an Ar atmosphere. Finally, it was re-pressed (950 MPa, 5 min) to obtain the Ag-based electrical contact composite material.
[0058] Comparative Example 6
[0059] ZnO powder and Cu powder were wet-mixed at a mass ratio of 1:9 for 40 min and dried for 12 h. The mixed powder was first placed into a mold and cold-pressed (850 MPa, 5 min). Then, it was heat-treated at 600℃ for 1.5 h in an Ar atmosphere, cold-pressed again (850 MPa, 5 min), and then heat-treated at 300℃ for 6 h in an Ar atmosphere. Finally, it was re-pressed (950 MPa, 5 min) to obtain Cu-based electrical contact composite material.
[0060] The performance of the prepared electrical contact composite material was tested according to GB / T 5586-2016 Basic Performance Test Method for Electrical Contact Materials, and compared with the comparative example and commercial electrical contact materials. The performance data are shown in Table 1.
[0061] Table 1. Performance comparison of the electrical contact composite materials prepared in the embodiments of the present invention with those of comparative examples and commercial materials.
[0062] <![CDATA[Conductivity (×10 7 S / m)]]> Hardness (HV) Tensile strength (MPa) Elongation (%) Contact resistance (μΩ) Quality loss (%) Example 1 4.86 129.6 301.2 19.7 35.14 4.2 Example 2 4.79 135.4 305.6 20.8 37.65 4.5 Example 3 4.91 136.7 309.3 21.4 34.42 3.8 Example 4 4.63 149.5 316.4 18.5 42.13 3.9 Example 5 4.82 132.5 303.1 19.2 36.26 4.1 Example 6 2.95 98.1 195.2 15.3 74.62 8.3 Comparative Example 1 4.27 142.9 215.2 14.5 46.52 5.8 Comparative Example 2 4.09 160.3 257.1 12.5 51.22 6.1 Comparative Example 3 2.38 109.4 180.4 10.8 82.56 9.2 Comparative Example 4 2.12 84.2 162.6 9.8 88.68 8.9 Comparative Example 5 4.53 107.8 288.2 16.1 49.72 6.3 Comparative Example 6 4.08 118.4 298.3 14.5 56.46 7.1 Commercial Ag / 10wt%CdO 4.51 80.2 250.8 25.5 35.58 5.2 <![CDATA[Commercial Ag / 10wt%SnO2]]> 4.65 85.5 230.1 24.6 48.32 5.5 Commercial Ag / 10wt%ZnO 4.45 85.1 285.4 15.2 45.14 6.4
[0063] Table 1 shows that the multidimensional gradient structure Ti3ZnC2 / Ti3C2T prepared in this invention... x @Zn y O z The composite materials prepared by combining the reinforcing phase material with Ag, Cu, and Sn matrices exhibit significantly improved overall performance compared to the comparative examples and commercial materials. The actual conductivity measured in Examples 1-6 ranged from 2.95 to 4.91 × 10⁻⁶. 7S / m. Using commercially available Ag / 10wt%CdO (4.51×10⁻⁶) 7 Based on (S / m), Example 1 (4.86 S / m) showed an increase in conductivity of approximately 7.8% [i.e., (4.86-4.51) / 4.51×100%]. Using commercial Ag / 10wt%SnO2 (4.65×10⁻⁶ S / m) as a baseline, the conductivity was improved by approximately 7.8% [i.e., (4.86-4.51) / 4.51×100%]. 7 Based on S / m), Example 3 (4.91×10 7 The conductivity (S / m) increased by approximately 5.6% [i.e., (4.91-4.65) / 4.65×100%]. Using commercial Ag / 10wt% ZnO (4.45×10⁻⁶ S / m), the conductivity was increased by approximately 5.6% [i.e., (4.91-4.65) / 4.65×100%]. 7 Based on S / m), Example 5 (4.82×10 7 The conductivity (S / m) increased by approximately 8.3% [i.e., (4.82-4.45) / 4.45×100%]. Comparative Example 1 (4.27×10⁻⁶) showed a decrease. 7 Based on S / m), Example 2 (4.79×10 7 The conductivity (S / m) increased by approximately 12.2% [i.e., (4.79-4.27) / 4.27×100%]. Comparative Example 5 (4.53×10... 7 Based on S / m), Example 2 (4.79×10 7 The conductivity (S / m) increased by approximately 5.7% [i.e., (4.79-4.53) / 4.53×100%]. Comparative Example 2 (4.09×10... 7 Based on S / m), Example 4 (4.63×10 7 The conductivity (S / m) increased by approximately 13.2% [i.e., (4.63-4.09) / 4.09×100%]. Comparative Example 6 (4.08×10⁻⁶) showed a similar increase. 7 Based on S / m), Example 4 (4.63×10 7 The conductivity (S / m) increased by approximately 13.4% [i.e., (4.63-4.08) / 4.08×100%]. Comparative Example 3 (2.38×10⁻⁶) showed a similar increase. 7 Based on S / m), Example 6 (2.95×10 7 The conductivity (S / m) increased by approximately 23.9% [i.e., (2.95-2.38) / 2.38×100%]. Comparative Example 4 (2.12×10⁻⁶) showed a similar increase. 7 Based on S / m), Example 6 (2.95×10 7 The conductivity (S / m) increased by approximately 39.2% [i.e. (2.95-2.12) / 2.12×100%].
[0064] The actual hardness range measured in Examples 1-6 was 98.1~149.5 HV. Based on commercial Ag / 10wt%CdO (80.2 HV), the hardness of Example 1 (129.6 HV) increased by approximately 61.6% [i.e., (129.6-80.2) / 80.2×100%]. Based on commercial Ag / 10wt%SnO2 (85.5 HV), the hardness of Example 3 (136.7 HV) increased by approximately 59.9% [i.e., (136.7-85.5) / 85.5×100%]; and based on commercial Ag / 10wt%ZnO (85.1 HV), the hardness of Example 5 (132.5 HV) increased by approximately 55.7% [i.e., (132.5-85.1) / 85.1×100%]. Compared to Comparative Example 1 (142.9 HV), the hardness of Example 2 (135.4 HV) decreased by approximately 5.2% [i.e., (142.9 - 135.4) / 142.9 × 100%]. Compared to Comparative Example 5 (107.8 HV), the hardness of Example 2 (135.4 HV) increased by approximately 25.6% [i.e., (135.4 - 107.8) / 107.8 × 100%];
[0065] Compared to Comparative Example 3 (109.4 HV), the hardness of Example 6 (98.1 HV) decreased by approximately 10.3% [i.e., (109.4 - 98.1) / 109.4 × 100%]. Compared to Comparative Example 4 (84.2 HV), the hardness of Example 6 (98.1 HV) increased by approximately 16.5% [i.e., (98.1 - 84.2) / 84.2 × 100%]. Compared to Comparative Example 2 (160.3 HV), the hardness of Example 4 (149.5 HV) decreased by approximately 6.7% [i.e., (149.5 - 160.3) / 160.3 × 100%]. Compared with Comparative Example 6 (118.4 HV), the hardness of Example 4 (149.5 HV) increased by approximately 26.3% [i.e. (149.5-118.4) / 118.4×100%].
[0066] The actual tensile strength measured in Examples 1-6 ranged from 195.2 to 316.4 MPa. Compared with commercial Ag / 10wt%CdO (250.8 MPa), the tensile strength of Example 1 (301.2 MPa) was increased by approximately 20.1% [i.e. (301.2-250.8) / 250.8×100%]. Based on commercial Ag / 10wt%SnO2 (230.1 MPa), the tensile strength of Example 3 (309.3 MPa) increased by approximately 34.4% [i.e. (309.3-230.1) / 230.1×100%]; based on commercial Ag / 10wt%ZnO (285.4 MPa), the tensile strength of Example 5 (303.1 MPa) increased by approximately 6.2% [i.e. (303.1-285.4) / 285.4×100%]; and based on Comparative Example 1 (215.2 MPa), the tensile strength of Example 2 (305.6 MPa) increased by approximately 42.0% [i.e. (305.6-215.2) / 215.2×100%]. Compared to Comparative Example 5 (288.2 MPa), the tensile strength of Example 2 (305.6 MPa) increased by approximately 6.0% [i.e., (305.6-288.2) / 288.2×100%]. Compared to Comparative Example 2 (257.1 MPa), the tensile strength of Example 4 (316.4 MPa) increased by approximately 23.1% [i.e., (316.4-257.1) / 257.1×100%]; compared to Comparative Example 6 (298.3 MPa), the tensile strength of Example 4 (316.4 MPa) increased by approximately 6.1% [i.e., (316.4-298.3) / 298.3×100%]. Compared to Comparative Example 3 (180.4 MPa), the tensile strength of Example 6 (195.2 MPa) increased by approximately 8.2% [i.e., (195.2-180.4) / 180.4×100%]. Compared to Comparative Example 4 (162.6 MPa), the tensile strength of Example 6 (195.2 MPa) increased by approximately 20.0% [i.e., (195.2-162.6) / 162.6×100%].
[0067] The actual elongation measured in Examples 1-6 ranged from 15.3 to 21.4 MPa. Based on commercial Ag / 10wt%CdO (25.5%), the elongation of Example 1 (19.7%) decreased by approximately 22.7% [i.e., (25.5-19.7) / 25.5×100%]. Based on commercial Ag / 10wt%SnO2 (24.6%), the elongation of Example 3 (21.4%) decreased by approximately 13.0% [i.e., (24.6-21.4) / 24.6×100%]; and based on commercial Ag / 10wt%ZnO (15.2%), the elongation of Example 5 (19.2%) increased by approximately 26.3% [i.e., (19.2-15.2) / 15.2×100%]. Compared to Comparative Example 1 (14.5%), the elongation of Example 2 (20.8%) was increased by approximately 43.4% [i.e., (20.8-14.5) / 14.5×100%]. Compared to Comparative Example 5 (16.1%), the elongation of Example 2 (20.8%) was increased by approximately 28.7% [i.e., (20.8-16.1) / 16.1×100%]. Compared to Comparative Example 2 (12.5%), the elongation of Example 4 (18.5%) was increased by approximately 48.0% [i.e., (18.5-12.5) / 12.5×100%]; compared to Comparative Example 6 (14.5%), the elongation of Example 4 (18.5%) was increased by approximately 27.6% [i.e., (18.5-14.5) / 14.5×100%]. Compared to Comparative Example 3 (10.8%), the elongation of Example 6 (15.3%) was increased by approximately 41.7% [i.e., (15.3-10.8) / 10.8×100%]. Compared to Comparative Example 4 (9.8%), the elongation of Example 6 (15.3%) was increased by approximately 56.1% [i.e., (15.3-9.8) / 9.8×100%].
[0068] The contact resistance measured in Examples 1-6 ranged from 34.42 to 74.62 μΩ. Compared to commercial Ag / 10wt% CdO (35.58 μΩ), the contact resistance of Example 1 (35.14 μΩ) decreased by approximately 1.2% [i.e., (35.58 - 35.14) / 35.58 × 100%]; compared to commercial Ag / 10wt% SnO2 (48.32 μΩ), the contact resistance of Example 3 (34.42 μΩ) decreased by approximately 28.8% [i.e., (48.32 - 34.42) / 48.32 × 100%]; compared to commercial Ag / 10wt% ZnO (45.14 μΩ), the contact resistance of Example 5 (36.26 μΩ) decreased by approximately 19.7% [i.e., (45.14 - 36.26) / 45.14 × 100%]; and compared to Comparative Example 1 (46.52 μΩ), the contact resistance of Example 2 (37.65 ....2% [i.e., (35.58 - 35.14) / 35.14 × 100%] [i.e., (35.58 - 35.14) / 35.14 × 100%] [i.e., (35.58 - 35.14) / 35.14 × 100%] [i.e., (35.58 - 35.14) / 35.14 × 100%] [i.e., (35.58 - The contact resistance of Example 2 (37.65 μΩ) decreased by approximately 19.1% [i.e., (46.52-37.65) / 46.52×100%]. Compared to Comparative Example 5 (49.72 μΩ), the contact resistance of Example 2 (37.65 μΩ) decreased by approximately 24.3% [i.e., (49.72-37.65) / 49.72×100%]. Compared to Comparative Example 2 (51.22 μΩ), the contact resistance of Example 4 (42.13 μΩ) decreased by approximately 17.7% [i.e., (51.22-42.13) / 51.22×100%]; compared to Comparative Example 6 (56.46 μΩ), the contact resistance of Example 4 (42.13 μΩ) decreased by approximately 25.4% [i.e., (56.46-42.13) / 56.46×100%]. Compared to Comparative Example 3 (82.56 μΩ), the contact resistance of Example 6 (74.62 μΩ) was reduced by approximately 9.6% [i.e., (82.56 - 74.62) / 82.56 × 100%]. Compared to Comparative Example 4 (88.68 μΩ), the contact resistance of Example 6 (74.62 μΩ) was reduced by approximately 15.9% [i.e., (88.68 - 74.62) / 88.68 × 100%].
[0069] The mass loss measured in Examples 1-6 ranged from 3.8% to 8.3%. Based on commercial Ag / 10wt% CdO (mass loss 5.2%), the mass loss in Example 1 (mass loss 4.2%) was reduced by approximately 19.2% [i.e., (5.2-4.2) / 5.2×100%]; based on commercial Ag / 10wt% SnO2 (mass loss 5.5%), the mass loss in Example 3 (mass loss 3.8%) was reduced by approximately 30.9% [i.e., (5.5-3.8) / 5.5×100%]. [00%]; Based on commercial Ag / 10wt%ZnO (mass loss 6.4%), the mass loss of Example 5 (mass loss 4.1%) was reduced by approximately 35.9% [i.e. (6.4-4.1) / 6.4×100%]; Based on Comparative Example 1 (mass loss 5.8%), the mass loss of Example 2 (mass loss 4.5%) was reduced by approximately 22.4% [i.e. (5.8-4.5) / 5.8×100%]. Based on Comparative Example 5 (mass loss 6.3%), the mass loss of Example 2 (mass loss 4.5%) was reduced by approximately 28.6% [i.e. (6.3-4.5) / 6.3×100%]. Compared to Comparative Example 2 (mass loss of 6.1%), the mass loss of Example 4 (mass loss of 3.9%) was reduced by approximately 36.1% [i.e., (6.1-3.9) / 6.1×100%]; compared to Comparative Example 6 (mass loss of 7.1%), the mass loss of Example 4 (mass loss of 3.9%) was reduced by approximately 45.1% [i.e., (7.1-3.9) / 7.1×100%]. Compared to Comparative Example 3 (mass loss of 9.2%), the mass loss of Example 6 (mass loss of 8.3%) was reduced by approximately 9.8% [i.e., (9.2-8.3) / 9.2×100%]. Compared to Comparative Example 4 (mass loss of 8.9%), the mass loss of Example 6 (mass loss of 8.3%) was reduced by approximately 6.7% [i.e., (8.9-8.3) / 8.9×100%]. The overall performance was significantly improved, demonstrating significant application value in the field of electrical contact composite materials.
[0070] The above description is merely a preferred embodiment of the present invention and is illustrative rather than restrictive. Those skilled in the art will understand that many changes, modifications, and even equivalents can be made within the spirit and scope defined by the claims of the present invention, all of which will fall within the protection scope of the present invention.
Claims
1. A multidimensional gradient structure conductive reinforced phase material, characterized in that, The material is Ti3ZnC2 / Ti3C2T. x @Zn y O z It has a three-dimensional / two-dimensional / zero-dimensional gradient structure, with the innermost layer being a three-dimensional Ti3ZnC2 structure and the outermost layer being an in-situ constructed two-dimensional layered structure Ti3C2T. x Both have in-situ loaded zero-dimensional nanoparticle structures of Zn on their surfaces. y O z Where y is 0.8~1.2, z is 0.8~1.3, and y / z is 0.6~1.5, Zn y O z The particle size of the nanoparticles is 20~50 nm.
2. The method for preparing the multidimensional gradient structure conductive enhancement phase material as described in claim 1, characterized in that... The specific steps include the following: S1: The precursor Ti3AlC2 is subjected to mechanical-plasma synergistic activation treatment to introduce Al vacancy defects on its surface, thereby obtaining defective Ti3AlC2 powder. S2: After mixing the powder obtained above with the pore-forming agent, a columnar sample is formed by cold isostatic pressing using a molybdenum wire as the current collector and used as a porous electrode sample. S3: The above porous electrode sample, together with the counter electrode and the reference electrode, was placed in molten salt to carry out an electrochemical molten salt replacement reaction. After the reaction was completed, post-processing was performed to obtain the three-dimensional structure Ti3ZnC2. S4: The powder obtained above is ultrasonically dispersed in a buffer solution containing hydroxycarboxylic acid, and then subjected to photochemical etching and oxidation treatment, washing, and vacuum drying to obtain the final product.
3. The method for preparing the multidimensional gradient structure conductive reinforced phase material as described in claim 2, characterized in that, Step S1 includes the following steps and parameters: First, Ti3AlC2 powder and anhydrous ethanol are mixed in a mortar and pestle mill at a mass ratio of 1:(0.5~1) at a speed of 30~80 rpm for a total mixing time of 0.5~2.5 h. Then, the mixture is vacuum dried and sieved to obtain pretreated powder with a particle size of 2~50 μm. Next, the pretreated powder is placed in an RF plasma chamber... Processing under a mixed atmosphere, With a content of 5 vol.%~15 vol.%, a chamber pressure of 30~50 Pa, a radio frequency power of 50~150 W, and a processing time of 30~60 min, defect-type Ti3AlC2 powder with Al vacancies on the surface is obtained.
4. The method for preparing the multidimensional gradient structure conductive reinforced phase material according to claim 2, characterized in that, Step S2 includes the following steps and parameters: the pore-forming agent is one or more of NaCl, LiCl, and KCl, and the mass ratio of defective Ti3AlC2 powder to the pore-forming agent is (8~9): (1~2); the cold isostatic pressing pressure is 50~100 MPa, the holding time is 3~7 min, and the porosity of the porous electrode is 30%~40%.
5. The method for preparing the multidimensional gradient structure conductive reinforced phase material according to claim 2, characterized in that, The counter electrode mentioned in step S3 is a high-purity zinc rod with a surface covered with a molybdenum mesh with a pore size of 0.2 mm. The reference electrode is a high-temperature resistant Ag / AgCl reference electrode for molten salt. The molten salt is a ternary molten salt of LiCl-KCl-NaCl with a mass ratio of LiCl:NaCl:KCl=(40~45):(8~10):(50~55).
6. The method for preparing the multidimensional gradient structure conductive reinforced phase material according to claim 2, characterized in that, The electrochemical molten salt displacement reaction described in step S3 includes the following steps and parameters: It is carried out in a vertical high-temperature molten salt reactor. First, the bottom ends of the three electrodes from step S3 are placed 3-6 cm above the molten salt surface. Then, under Ar atmosphere protection, the temperature is increased to 350-400℃ at a rate of 3-6℃ / min and held for 30-60 min to melt the molten salt. Next, the three electrodes are placed 1.5-2.5 cm below the molten salt surface, ensuring that the bottom of the electrodes is >1 cm from the bottom of the crucible. The temperature is further increased to 400-450℃ at a rate of 2-5℃ / min, using pulse potential control. The high potential is +0.7-+0.9 V, the low potential is +0.1-+0.2 V, the pulse period is 10-20 s, and the total reaction time is 4-8 h.
7. The method for preparing the multidimensional gradient structure conductive reinforced phase material according to claim 2, characterized in that, The post-processing described in step S3 includes: first, dissolving the cooled reaction product in deionized water at 80-100℃ to remove the molten salt, then removing the supernatant after standing, repeating this operation 4-6 times; then centrifuging and washing at 6000-10000 rpm for 3-10 min, repeating this operation 3-5 times until the conductivity of the supernatant is <38 μS / cm; finally, performing vacuum freeze-drying on the product for 6-10 h at a cold trap temperature of -50℃ and a vacuum degree <10 Pa to obtain the three-dimensional structure Ti3ZnC2.
8. The method for preparing the multidimensional gradient structure conductive reinforced phase material according to claim 2, characterized in that, The hydroxycarboxylic acid mentioned in step S4 is selected from one or more of citric acid, gluconic acid, tartaric acid or malic acid, and its content is 0.5~2wt.%; the buffer solution also contains the corresponding hydroxycarboxylic acid salt, the molar ratio of acid to salt is (1:0.3)~(1:1), and the pH value of the system is controlled at 4.5~5.
5.
9. The method for preparing the multidimensional gradient structure conductive reinforced phase material according to claim 2, characterized in that, The specific process of ultrasonic dispersion in step S4 is as follows: the three-dimensional structure Ti3ZnC2 obtained in step S3 is added to a buffer solution with a mass concentration of 15~25 mg / mL, and ultrasonically dispersed for 10~20 min at a power of 145~245 W and a frequency of 40 kHz to obtain a uniform suspension.
10. The method for preparing the multidimensional gradient structure conductive reinforced phase material according to claim 2, characterized in that, The photochemical etching oxidation treatment in step S4 includes the following steps and parameters: a uniform suspension containing Ti3ZnC2 is reacted in an ice bath under the protection of an O2 / Ar mixed gas, wherein the O2 volume fraction is 0.5%~5%, the ultraviolet light wavelength is 365 nm, the irradiance is 50~150 mW / cm², and the reaction time is 2.5~3.5 h, finally obtaining a three-dimensional / two-dimensional / zero-dimensional gradient structure Ti3ZnC2 / Ti3C2T x @Zn y O z Reinforcing phase materials.