High-performance copper-tin alloy ultrafine wire and preparation method thereof

By employing vacuum electromagnetic stirring melting, large deformation hot forging, and multi-stage drawing processes, combined with the addition of nickel and phosphorus, the problems of dendrite segregation and porosity defects in copper-tin alloy wires have been solved, enabling stable production and excellent performance of high-performance copper-tin alloy ultrafine wires, suitable for precision electronic devices and high-reliability cables.

CN123132701APending Publication Date: 2026-11-20SHENYANG INST OF ENG
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611408369.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing copper-tin alloy wires suffer from dendrite segregation, porosity defects, and high breakage rates during production, making it difficult to achieve stable production and high-performance applications.

Method used

The process employs vacuum electromagnetic stirring melting, multi-pass large deformation hot forging, gradient annealing, and multi-stage drawing combined with online dynamic annealing. By adding nickel and phosphorus elements, the as-cast microstructure and microstructure are optimized, defects are eliminated, and the ductility and stability of the material are improved.

Benefits of technology

It significantly reduces the wire breakage rate during the drawing process and obtains high-performance copper-tin alloy ultrafine wires with uniform structure, fine grains, and excellent performance. It has high strength, good ductility and conductivity, and is suitable for continuous production of precision electronic devices and high-reliability cables.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123132701A_ABST
    Figure CN123132701A_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of manufacturing ultra-fine copper-tin wire, and discloses a high-performance copper-tin alloy ultra-fine wire and a preparation method thereof. The high-performance copper-tin alloy ultra-fine wire is composed of the following components in percentage by mass: tin content of 0.1% to 0.6%, nickel content of 0.1% to 0.5%, phosphorus content of 0.01% to 0.1%, and the balance of copper and unavoidable impurities, with the total amount of impurities being ≤0.05%. The high-performance copper-tin alloy ultra-fine wire has a tensile strength of 1139 MPa, an elongation of 10%, and an electrical conductivity of 79% IACS when the final wire diameter is 0.03 mm. The preparation method significantly reduces the wire breakage rate during the drawing process, ensuring that the copper-tin alloy wire has excellent performance in the continuous production of precision electronic devices and high-reliability cables.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of manufacturing technology of ultra-fine copper-tin wire, and particularly relates to a high-performance copper-tin alloy ultra-fine wire and its preparation method. Background Technology

[0002] With the rapid development of the electronics industry, the demand for high-performance alloy materials is increasing daily. Copper-tin alloy wire has broad application prospects in integrated circuits, communication equipment, precision instruments, automotive electronics, and high-end electrical equipment. Especially in precision electronic devices and high-reliability cables, the excellent conductivity and durability of copper-tin alloy wire make it an ideal material to replace traditional copper wire. However, traditional copper-tin alloys face problems such as dendrite segregation, porosity defects, and a high breakage rate during processing, which seriously affect production efficiency and product performance. Therefore, developing copper-tin alloy wires with stable performance and lower processing difficulty has become an important research direction in the materials field to meet the ever-growing demand for high-performance alloy materials from the electronics industry.

[0003] In existing technologies, the preparation of copper-tin alloys mainly relies on hot forging and cold rotary forging processes to improve the as-cast microstructure, supplemented by annealing processes to regulate material properties. However, existing methods often depend on single-element (such as rare earth elements or trace additives) optimization in composition design, failing to fully synergistically regulate the alloy's fluidity, grain refinement, and work hardening behavior. This results in a high wire breakage rate during drawing, making it difficult to achieve stable production of long-length wires. Furthermore, existing processes have limited effectiveness in homogenizing the as-cast microstructure, failing to completely eliminate dendrite segregation and porosity defects, further limiting the overall performance and industrial application of copper-tin alloy wires.

[0004] The invention patent describes a method for preparing ultra-long copper-tin alloy micro-wires (publication number CN118558767A, publication date: 20240830). This method produces wires through casting, continuous casting, cold forging, and multi-pass drawing. However, this method cannot solve the problems of alloy segregation and homogenization during the manufacturing process.

[0005] The invention patent for an ultra-fine, ultra-long copper alloy wire and its production method (publication number CN107904434A, publication date 20200331) describes a method for preparing copper-tin alloy wire using directional solidification technology. However, this method, which involves directly drawing the continuously cast copper-tin alloy rod after annealing, does not completely eliminate defects in the as-cast structure, thus requiring further optimization and improvement of the strength and processing performance of the copper-tin alloy wire.

[0006] Furthermore, while the aforementioned methods can improve wire processing performance to some extent, there is still room for further optimization in controlling as-cast structural defects, homogenizing the microstructure during hot working, and continuously regulating work hardening during the ultra-fine drawing stage. In addition, existing research on Cu-Sn-Ni-P alloys has largely focused on plates, strips, foils, or general wires. For the synergistic relationship between composition and hot working, short-time annealing, and staged drawing under 0.03 mm ultra-fine wire conditions, as well as the comprehensive matching of high strength, high elongation, and high conductivity, more suitable technical solutions are still needed.

[0007] Therefore, there is an urgent need for a solution that optimizes both composition and process. By innovating alloy composition design and processing technology, the technical bottlenecks of copper-tin alloy wires in casting segregation, processing breakage, and performance consistency can be solved to meet the continuous production needs of high-reliability wires. Summary of the Invention

[0008] To overcome the problems existing in related technologies, this invention discloses a high-performance copper-tin alloy ultrafine wire and its preparation method. The purpose of this invention is to solve the problems of increased wire breakage risk, performance fluctuations, and difficulty in balancing strength, plasticity, and conductivity caused by as-cast segregation, porosity and inclusion defects, uneven microstructure, and continuous drawing work hardening in the preparation of copper-tin alloy ultrafine wires. This invention provides a preparation scheme that synergistically integrates composition design with vacuum electromagnetic stirring melting, large deformation hot forging, intermediate homogenization annealing, staged drawing, and online short-time high-frequency induction annealing.

[0009] The technical solution is as follows: a high-performance copper-tin alloy ultrafine wire, which is composed of the following components by mass percentage: tin content of 0.1% to 0.6%, nickel content of 0.1% to 0.5%, phosphorus content of 0.01% to 0.1%, and the balance being copper and unavoidable impurities, with the total amount of impurities ≤ 0.05%.

[0010] Another object of the present invention is to provide a method for preparing high-performance copper-tin alloy ultrafine wires, the method comprising: S1, weigh high-purity copper, nickel added in the form of copper-nickel master alloy and phosphorus added in the form of copper-phosphorus master alloy, place the raw materials in a vacuum induction furnace to melt and cast into ingots. S2. After preheating and holding the ingot at the temperature, a hydraulic press is used to perform multiple hot forgings to break up the large dendrites in the casting state, promote dynamic recrystallization, and form a uniform fine-grained copper-tin alloy rod blank. S3, after the hot-forged uniform fine-grained copper-tin alloy billet is annealed and held at a temperature under argon protection, it is then slowly cooled in a vacuum induction furnace; S4. The annealed uniform fine-grained copper-tin alloy billet is sequentially subjected to coarse drawing, medium drawing and fine drawing. After each drawing stage, online dynamic annealing is performed using high-frequency induction heating until the high-performance copper-tin alloy ultrafine wire of the target size is obtained.

[0011] Furthermore, in step S1, the raw material is placed in a vacuum induction furnace for melting, with a vacuum degree ≤1×10⁻⁶. - The melting temperature is 1200-1300℃, the melting time is 2-3 hours, and electromagnetic stirring at 10-20 Hz is applied during the melting process. After the melting is completed, an alloy ingot is cast using a steel mold preheated to 200-300℃. The ingot has a diameter of 20 mm and a length of 1.5 m.

[0012] In step S1, the purity of the high-purity copper is ≥99.4%; the nickel is added in the form of a copper-nickel master alloy, and the phosphorus is added in the form of a copper-phosphorus master alloy with a purity ≥99.95%.

[0013] Furthermore, in step S2, the ingot preheating and heat preservation includes: preheating to 850℃~950℃ and holding for 1h~2h.

[0014] In step S2, a hydraulic press is used for multi-pass hot forging, with each pass involving a deformation of 30% to 40%, a total deformation of ≥80%, and a temperature of ≥750℃ during the hot forging process.

[0015] Furthermore, in step S3, the annealing temperature is 550–650°C, and the holding time is 2–4 hours.

[0016] In step S3, the temperature is slowly cooled to below 200°C in a vacuum induction furnace.

[0017] Furthermore, in step S4, when the rough drawing diameter is ≥2mm, the deformation per pass in the rough drawing is 20% to 35%; when the intermediate drawing diameter is 0.5mm ≤ diameter <2mm, the deformation per pass in the intermediate drawing is 15% to 20%; when the finish drawing diameter is <0.5mm, the deformation per pass in the finish drawing is 5% to 15%.

[0018] In step S4, the online dynamic annealing is performed with an annealing temperature set to 300–450°C and an annealing time of 10–30 seconds.

[0019] Combining all the above technical solutions, the beneficial effects of this invention are as follows: This invention solves the technical problems of unstable production and low performance of existing copper-tin alloys due to dendrite segregation, porosity defects, and high breakage rates during continuous production. The preparation steps of high-performance copper-tin alloy ultrafine wire are as follows: First, impurities and porosity in the melt are eliminated through vacuum electromagnetic stirring melting; then, the as-cast dendrite structure is broken using a large deformation hot forging process to optimize the crystal structure of the ingot; next, intermediate gradient annealing is performed to refine the grains and improve the mechanical properties of the material; finally, multi-stage drawing combined with online dynamic annealing effectively eliminates work hardening and improves the ductility and stability of the material. By adding nickel and phosphorus, tin segregation can be synergistically suppressed, improving melt fluidity. Simultaneously, dynamic annealing controls the microstructure of the material, ultimately obtaining high-performance copper-tin alloy ultrafine wire with uniform microstructure, fine grains, and superior performance. The diameter of the alloy ultrafine wire is 0.03 mm, the room temperature tensile strength is not less than 1139–1145 MPa, the elongation after fracture is not less than 6–10%, and the conductivity is not less than 72–79% IACS. Preferably, when the final wire diameter is 0.03mm, the tensile strength reaches 1139MPa, the elongation is 10%, and the conductivity is 79% IACS.

[0020] This preparation method significantly reduces the breakage rate during the drawing process, ensuring that copper-tin alloy wires have excellent performance in the continuous production of precision electronic devices and high-reliability cables.

[0021] The preparation method provided by this invention improves the as-cast structure and reduces dendrite segregation and porosity defects by adding nickel and phosphorus elements to the copper-tin alloy. At the same time, it adopts processes such as vacuum stirring melting, downward continuous casting, large deformation hot forging, intermediate gradient annealing, and multi-stage drawing and online dynamic annealing to obtain ultrafine copper-tin alloy wires with fine grains, uniform composition and excellent ductility. Attached Figure Description

[0022] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this disclosure and, together with the description, serve to explain the principles of this disclosure; Figure 1 This is a flowchart of the preparation method of high-performance copper-tin alloy ultrafine wire provided in the embodiments of the present invention. Detailed Implementation

[0023] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. However, the present invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0024] Example 1: A high-performance copper-tin alloy ultrafine wire, composed of the following components by mass percentage: tin content of 0.1% to 0.6%, nickel content of 0.1% to 0.5%, phosphorus content of 0.01% to 0.1%, with the balance being copper and unavoidable impurities, the total amount of impurities being ≤0.05%.

[0025] Preferably, the mass percentage of Sn is 0.1% to 0.5%, the mass percentage of Ni is 0.2% to 0.5%, and the mass percentage of P is 0.05% to 0.10%.

[0026] Preferably, the room temperature tensile strength of the alloy ultrafine wire is not less than 1185-1193 MPa, the elongation after fracture is not less than 7-9%, and the conductivity is not less than 75-77% IACS.

[0027] like Figure 1 As shown, the method for preparing high-performance copper-tin alloy ultrafine wires provided in this embodiment of the invention includes the following steps: S1, weigh high-purity copper, nickel added in the form of copper-nickel master alloy and phosphorus added in the form of copper-phosphorus master alloy, place the raw materials in a vacuum induction furnace to melt and cast into ingots. S2. After preheating and holding the ingot at the temperature, a hydraulic press is used to perform multiple hot forgings to break up the large dendrites in the casting state, promote dynamic recrystallization, and form a uniform fine-grained copper-tin alloy rod blank. S3, after the hot-forged uniform fine-grained copper-tin alloy billet is annealed and held at a temperature under argon protection, it is then slowly cooled in a vacuum induction furnace; S4. The annealed uniform fine-grained copper-tin alloy billet is sequentially subjected to coarse drawing, medium drawing and fine drawing. After each drawing stage, online dynamic annealing is performed using high-frequency induction heating until the high-performance copper-tin alloy ultrafine wire of the target size is obtained.

[0028] In step S1, the raw material is placed in a vacuum induction furnace for melting, with a vacuum degree ≤1×10⁻⁶. - ²Pa, heating temperature of 1200–1300℃, melting time of 2–3 hours, with electromagnetic stirring at 10–20 Hz applied during the melting process. After smelting, alloy ingots are cast using steel molds preheated to 200–300 °C. The ingots are 20 mm in diameter and 1.5 m in length. The purity of the high-purity copper is ≥99.4%; The nickel is added in the form of a copper-nickel master alloy, and the phosphorus is added in the form of a copper-phosphorus master alloy, with a purity of ≥99.95%.

[0029] For example, in step S2, the ingot preheating and heat preservation includes: preheating to 850℃~950℃ and heat preservation for 1h~2h; In multi-pass hot forging using a hydraulic press, after 4 to 5 passes, the deformation amount in each pass is 30% to 40%, and the total deformation amount is ≥80%. The temperature during hot forging is ≥750℃, and finally a copper-tin alloy rod blank, namely a copper-tin-nickel-phosphorus alloy rod blank, is obtained.

[0030] Preferably, rough drawing is performed when the wire diameter is not less than 2 mm, with a single-pass deformation of 20% to 35%; intermediate drawing is performed when the wire diameter is 0.5 to 2 mm, with a single-pass deformation of 10% to 20%; and fine drawing is performed when the wire diameter is less than 0.5 mm, with a single-pass deformation of 5% to 15%.

[0031] For example, in step S3, the annealing temperature is 550-650°C, the holding time is 2-4 hours, and the temperature is slowly cooled to below 200°C in a vacuum induction furnace to further eliminate internal stress and homogenize the microstructure. For example, in step S4, when the rough drawing diameter is ≥2mm, the deformation per pass in the rough drawing is 20% to 35%; when the intermediate drawing diameter is 0.5mm ≤ diameter <2mm, the deformation per pass in the intermediate drawing is 15% to 20%; when the finish drawing diameter is <0.5mm, the deformation per pass in the finish drawing is 5% to 15%.

[0032] Preferably, the deformation per pass of precision drawing is 5% to 8%.

[0033] In step S4, the online dynamic annealing is performed with an annealing temperature set to 300–450°C and an annealing time of 10–30 seconds.

[0034] Online short-time annealing is set at least between rough drawing and intermediate drawing, and between intermediate drawing and fine drawing.

[0035] As demonstrated by the above embodiments, this invention improves melt fluidity by adding Ni and P elements to the copper-tin alloy, effectively reducing dendrite segregation, porosity, and inclusion defects in the as-cast microstructure, thus purifying the alloy composition. The synergistic effect of large-deformation hot forging and intermediate gradient annealing significantly refines the grains, homogenizes the composition distribution, and improves the processing stability of the billet. Multi-stage drawing and online dynamic annealing processes ensure coordinated deformation of the microstructure during drawing, reduce the breakage rate, and achieve continuous and stable production of ultrafine wires.

[0036] The copper-tin alloy wire and its preparation method provided by this invention have simple production steps, produce alloy wires with excellent ductility, and have production stability that is significantly higher than similar existing technologies, making them valuable for large-scale industrial production.

[0037] The present invention combines induction melting with electromagnetic stirring, which is beneficial to promoting the uniform distribution of Sn, Ni and P in the melt and reducing the adverse effects of gas and inclusion defects on ultrafine drawing.

[0038] The combination of large deformation multi-pass hot forging and intermediate homogenization annealing can break up coarse as-cast structures, reduce the inhomogeneity of structure and composition, and improve the subsequent plastic processing capability of the billet.

[0039] By gradually reducing the deformation per pass according to the wire diameter and implementing online short-time high-frequency induction annealing between drawing stages, the accumulation of work hardening can be alleviated, and the risk of local damage and wire breakage during the ultra-fine drawing stage can be reduced.

[0040] Through synergistic control of composition and process, the resulting 0.03 mm ultrafine wire achieved a tensile strength of 1139–1208 MPa, an elongation after fracture of 6%–10%, and an electrical conductivity of 72%–79% IACS, thus achieving a comprehensive match of strength, plasticity, and electrical conductivity.

[0041] Example 2: A high-performance copper-tin alloy ultrafine wire, the composition and mass ratio of which are as follows: tin content is 0.1%, nickel content is 0.2%, phosphorus content is 0.05%, and the balance is copper and unavoidable impurities, with the total amount of impurities ≤0.05%.

[0042] The preparation of high-performance copper-tin alloy ultrafine wires includes the following steps: (1) Weigh the alloy raw material as described above, place it in a vacuum furnace, and evacuate it to 1×10⁻⁶. - Below 2Pa, heat to 1250℃, melt for 3 hours, apply 15Hz electromagnetic stirring during melting, and then pour into ingots after forming a uniform molten liquid.

[0043] (2) The ingot is preheated to 900°C and held for 2 hours. Then, it is hot forged in multiple passes using a hydraulic press. The deformation amount of each pass is 30%, and the total deformation amount reaches 90%. The final forging temperature during the forging process is not lower than 750°C, forming a uniform fine-grained copper-tin alloy rod blank. (3) The hot-forged uniform fine-grained copper-tin alloy rod blank is annealed under argon protection at a temperature of 550°C. After holding at the temperature for 2 hours, it is slowly cooled to below 200°C in the furnace.

[0044] (4) The annealed uniform fine-grained copper-tin alloy billet was subjected to rough drawing, intermediate drawing and fine drawing in sequence. Online annealing was set during the drawing process. The annealing temperature was 450℃ and the annealing time was 10s. Finally, a micro wire with a diameter of 0.03mm was obtained. That is, a high-performance copper-tin alloy ultrafine wire.

[0045] Test Example 2 shows that the prepared high-performance copper-tin alloy ultrafine wire has a tensile strength of 1139 MPa, an elongation of 10%, and a conductivity of 79% IACS.

[0046] Example 3: A high-performance copper-tin alloy ultrafine wire, the constituent elements and contents of which are as follows: tin content is 0.5%, nickel content is 0.5%, phosphorus content is 0.1%, and the balance is copper and unavoidable impurities, with the total impurities ≤0.05%.

[0047] The preparation of high-performance copper-tin alloy ultrafine wires includes the following steps: (1) Weigh the alloy raw material as described above, place it in a vacuum furnace, and evacuate it to 1×10⁻⁶. - Below 2 Pa, heat to 1250℃, melt for 3 hours, apply 20Hz electromagnetic stirring during melting, and then pour into ingots after forming a uniform molten liquid.

[0048] (2) The ingot is preheated to 950°C and held for 2 hours. Then, it is hot forged in multiple passes using a hydraulic press. The deformation amount of each pass is 35%, and the total deformation amount reaches 90%. The final forging temperature during the forging process is not lower than 750°C, forming a uniform fine-grained copper-tin alloy rod blank. (3) The hot-forged uniform fine-grained copper-tin alloy rod blank is annealed under argon protection at a temperature of 600°C. After holding at the temperature for 2 hours, it is slowly cooled to below 200°C in the furnace.

[0049] (4) The annealed uniform fine-grained copper-tin alloy billet was subjected to rough drawing, intermediate drawing and fine drawing in sequence. During the drawing process, online annealing was set, the annealing temperature was 400℃ and the annealing time was 15s. Finally, a micro wire with a diameter of 0.03mm was obtained; that is, a high-performance copper-tin alloy ultrafine wire.

[0050] The high-performance copper-tin alloy ultrafine wire prepared in Test Example 3 has a tensile strength of 1208 MPa, an elongation of 6%, and a conductivity of 72% IACS.

[0051] Example 4: A high-performance copper-tin alloy ultrafine wire, the constituent elements and contents of which are as follows: tin content is 0.5%, nickel content is 0.4%, phosphorus content is 0.05%, and the balance is copper and unavoidable impurities, with the total impurities ≤0.08%.

[0052] The preparation of high-performance copper-tin alloy ultrafine wires includes the following steps: (1) Weigh the alloy raw material as described above, place it in a vacuum furnace, and evacuate it to 1×10⁻⁶. - Below 2 Pa, heat to 1250℃, melt for 3 hours, apply 20Hz electromagnetic stirring during melting, and then pour into ingots after forming a uniform molten liquid.

[0053] (2) The ingot is preheated to 930°C and held for 2 hours. Then, it is hot forged in multiple passes using a hydraulic press. The deformation amount of each pass is 35%, and the total deformation amount reaches 90%. The final forging temperature during the forging process is not lower than 750°C, forming a uniform fine-grained copper-tin alloy rod blank. (3) The hot-forged copper-tin alloy rod blank with uniform fine grains is annealed under argon protection at a temperature of 650°C. After holding at the temperature for 2 hours, it is slowly cooled to below 200°C in the furnace.

[0054] (4) The annealed uniform fine-grained copper-tin alloy billet was subjected to rough drawing, intermediate drawing and fine drawing in sequence. During the drawing process, online annealing was set, the annealing temperature was 380℃ and the annealing time was 15s. Finally, a micro wire with a diameter of 0.03mm was obtained, namely a high-performance copper-tin alloy ultrafine wire.

[0055] The high-performance copper-tin alloy ultrafine wire prepared in Test Example 4 has a tensile strength of 1190 MPa, an elongation of 8%, and a conductivity of 76% IACS.

[0056] The properties of the high-performance copper-tin alloy ultrafine wires prepared in Examples 2-4 are shown in Table 1. Table 1 As shown in Table 1, Example 2 maintains a tensile strength of 1139 MPa while exhibiting 10% elongation after fracture and 79% IACS conductivity; Example 3 achieves the highest tensile strength; and Example 4 demonstrates a good overall balance between tensile strength, elongation after fracture, and conductivity. These results indicate that 0.03 mm copper-tin-nickel-phosphorus alloy ultrafine wires possessing high strength, ductility, and conductivity can be prepared by combining Ni and P microalloying with vacuum electromagnetic stirring melting, large deformation hot forging, intermediate homogenization annealing, staged drawing, and online short-time annealing. Example 5: A high-performance copper-tin alloy ultrafine wire, composed of the following components by mass percentage: 0.1% tin, 0.1% nickel, 0.01% phosphorus, with the balance being copper and unavoidable impurities, the total amount of impurities being ≤0.05%.

[0057] The method for preparing high-performance copper-tin alloy ultrafine wires provided in this invention includes the following steps: (1) Weigh high-purity copper, nickel added in the form of copper-nickel master alloy and phosphorus added in the form of copper-phosphorus master alloy, place the raw materials in a vacuum induction furnace to melt and cast into ingots. (2) After preheating and holding the ingot, use a hydraulic press to perform multiple hot forgings to break up the large dendrites in the casting state, promote dynamic recrystallization, and form a uniform fine-grained copper-tin alloy rod billet. (3) After the hot-forged uniform fine-grained copper-tin alloy billet is annealed and held at a temperature under argon protection, it is slowly cooled in a vacuum induction furnace; (4) The uniform fine-grained copper-tin alloy rod blank after annealing is subjected to coarse drawing, medium drawing and fine drawing in sequence. After each drawing stage, high frequency induction heating is used for online dynamic annealing until the high-performance copper-tin alloy ultrafine wire of the target size is obtained.

[0058] In step (1), the raw materials are placed in a vacuum induction furnace for melting, with a vacuum degree ≤1×10 - ²Pa, heating temperature of 1200℃, melting time of 2h, electromagnetic stirring of 10Hz is applied during the melting process to form a uniform molten liquid, which is then poured into an ingot; The purity of the high-purity copper is ≥99.4%; The nickel is added in the form of a copper-nickel master alloy, and the phosphorus is added in the form of a copper-phosphorus master alloy, with a purity of ≥99.95%.

[0059] In step (2), the ingot preheating and heat preservation includes: preheating to 850°C and heat preservation for 1 hour; In multi-pass hot forging using a hydraulic press, the deformation amount in each pass is 30%, the total deformation amount is ≥80%, and the temperature during hot forging is ≥750℃.

[0060] In step (3), the annealing temperature is 550℃, and the holding time is 2h. The temperature is then slowly cooled to below 200℃ in a vacuum induction furnace to further eliminate internal stress and homogenize the microstructure. In step (4), when the rough drawing diameter is ≥2mm, the drawing deformation per pass in the rough drawing is 20%; when the intermediate drawing is 0.5mm, the drawing deformation per pass in the intermediate drawing is 15%; when the fine drawing diameter is <0.5mm, the drawing deformation per pass in the fine drawing is 10%.

[0061] In step (4), the online dynamic annealing is set to an annealing temperature of 300°C and an annealing time of 10 seconds.

[0062] Example 6: A high-performance copper-tin alloy ultrafine wire, composed of the following components by mass percentage: 0.6% tin, 0.5% nickel, 0.1% phosphorus, with the balance being copper and unavoidable impurities, the total amount of impurities being ≤0.05%.

[0063] A method for preparing high-performance copper-tin alloy ultrafine wires includes the following steps: (1) Weigh high-purity copper, nickel added in the form of copper-nickel master alloy and phosphorus added in the form of copper-phosphorus master alloy, place the raw materials in a vacuum induction furnace to melt and cast into ingots. (2) After preheating and holding the ingot, use a hydraulic press to perform multiple hot forgings to break up the large dendrites in the casting state, promote dynamic recrystallization, and form a uniform fine-grained copper-tin alloy rod billet. (3) After the hot-forged uniform fine-grained copper-tin alloy billet is annealed and held at a temperature under argon protection, it is slowly cooled in a vacuum induction furnace; (4) The uniform fine-grained copper-tin alloy rod blank after annealing is subjected to coarse drawing, medium drawing and fine drawing in sequence. After each drawing stage, high frequency induction heating is used for online dynamic annealing until the high-performance copper-tin alloy ultrafine wire of the target size is obtained.

[0064] In step (1), the raw materials are placed in a vacuum induction furnace for melting, with a vacuum degree ≤1×10 - ²Pa, heating temperature of 1300℃, melting time of 3h, electromagnetic stirring of 20Hz is applied during the melting process to form a uniform molten liquid, which is then poured into an ingot; The purity of the high-purity copper is ≥99.4%; The nickel is added in the form of a copper-nickel master alloy, and the phosphorus is added in the form of a copper-phosphorus master alloy, with a purity of ≥99.95%.

[0065] In step (2), the ingot preheating and heat preservation include: preheating to 950°C and heat preservation for 2 hours; In multi-pass hot forging using a hydraulic press, the deformation amount in each pass is 40%, the total deformation amount is ≥80%, and the temperature during hot forging is ≥750℃.

[0066] In step (3), the annealing temperature is 650℃, and the holding time is 4h. The temperature is then slowly cooled to below 200℃ in a vacuum induction furnace to further eliminate internal stress and homogenize the microstructure. In step (4), when the rough drawing diameter is ≥2mm, the drawing deformation per pass in the rough drawing is 35%; when the intermediate drawing is 1.95mm, the drawing deformation per pass in the intermediate drawing is 20%; when the fine drawing diameter is <0.5mm, the drawing deformation per pass in the fine drawing is 15%.

[0067] In step (4), the online dynamic annealing is performed with an annealing temperature of 450°C and an annealing time of 30 seconds.

[0068] Example 7: A high-performance copper-tin alloy ultrafine wire, composed of the following components by mass percentage: tin content of 0.35%, nickel content of 0.3%, phosphorus content of 0.055%, with the balance being copper and unavoidable impurities, the total amount of impurities being ≤0.05%.

[0069] A method for preparing high-performance copper-tin alloy ultrafine wires includes the following steps: (1) Weigh high-purity copper, nickel added in the form of copper-nickel master alloy and phosphorus added in the form of copper-phosphorus master alloy, place the raw materials in a vacuum induction furnace to melt and cast into ingots. (2) After preheating and holding the ingot, use a hydraulic press to perform multiple hot forgings to break up the large dendrites in the casting state, promote dynamic recrystallization, and form a uniform fine-grained copper-tin alloy rod billet. (3) After the hot-forged uniform fine-grained copper-tin alloy billet is annealed and held at a temperature under argon protection, it is slowly cooled in a vacuum induction furnace; (4) The uniform fine-grained copper-tin alloy rod blank after annealing is subjected to coarse drawing, medium drawing and fine drawing in sequence. After each drawing stage, high frequency induction heating is used for online dynamic annealing until the high-performance copper-tin alloy ultrafine wire of the target size is obtained.

[0070] In step (1), the raw materials are placed in a vacuum induction furnace for melting, with a vacuum degree ≤1×10 - ²Pa, heating temperature of 1250℃, melting time of 2.5h, electromagnetic stirring of 15Hz is applied during the melting process to form a uniform molten liquid, which is then poured into an ingot; The purity of the high-purity copper is ≥99.4%; The nickel is added in the form of a copper-nickel master alloy, and the phosphorus is added in the form of a copper-phosphorus master alloy, with a purity of ≥99.95%.

[0071] In step (2), the ingot preheating and heat preservation include: preheating to 900℃ and heat preservation for 1.5h; In multi-pass hot forging using a hydraulic press, the deformation amount in each pass is 35%, the total deformation amount is ≥80%, and the temperature during hot forging is ≥750℃.

[0072] In step (3), the annealing temperature is 600℃, and the holding time is 3h. The temperature is then slowly cooled to below 200℃ in a vacuum induction furnace to further eliminate internal stress and homogenize the microstructure. In step (4), when the rough drawing diameter is ≥2mm, the drawing deformation per pass in the rough drawing is 28.5%; when the intermediate drawing is 1.25mm, the drawing deformation per pass in the intermediate drawing is 17.5%; when the fine drawing diameter is <0.5mm, the drawing deformation per pass in the fine drawing is 12.5%.

[0073] In step (4), the online dynamic annealing is performed with an annealing temperature of 375°C and an annealing time of 20 seconds.

[0074] Experiments have shown that the high-performance copper-tin alloy ultrafine wires obtained in Examples 5-6 have similar tensile strength, elongation, and conductivity to the high-performance copper-tin alloy ultrafine wires obtained in Examples 2-4. This demonstrates that the preparation method significantly reduces the breakage rate during the drawing process, ensuring that copper-tin alloy wires exhibit excellent performance in the continuous production of precision electronic devices and high-reliability cables.

[0075] In the above embodiments, the descriptions of each embodiment have different focuses. For parts that are not described in detail or recorded in a certain embodiment, please refer to the relevant descriptions of other embodiments.

[0076] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by those skilled in the art within the scope of the technology disclosed in the present invention and within the spirit and principles of the present invention should be covered within the scope of protection of the present invention.

Claims

1. A high-performance copper-tin alloy ultrafine wire, characterized in that, This high-performance copper-tin alloy ultrafine wire is composed of the following components by mass percentage: tin content of 0.1% to 0.6%, nickel content of 0.1% to 0.5%, phosphorus content of 0.01% to 0.1%, with the balance being copper and unavoidable impurities, and the total amount of impurities ≤ 0.05%.

2. A method for preparing high-performance copper-tin alloy ultrafine wire, characterized in that, The method for preparing the high-performance copper-tin alloy ultrafine wire according to claim 1 includes: S1, weigh high-purity copper, nickel added in the form of copper-nickel master alloy and phosphorus added in the form of copper-phosphorus master alloy, place the raw materials in a vacuum induction furnace to melt and cast into ingots. S2. After preheating and holding the ingot at the temperature, a hydraulic press is used to perform multiple hot forgings to break up the large dendrites in the casting state, promote dynamic recrystallization, and form a uniform fine-grained copper-tin alloy rod blank. S3, after the hot-forged uniform fine-grained copper-tin alloy billet is annealed and held at a temperature under argon protection, it is then slowly cooled in a vacuum induction furnace; S4. The annealed uniform fine-grained copper-tin alloy billet is sequentially subjected to coarse drawing, medium drawing and fine drawing. After each drawing stage, online dynamic annealing is performed using high-frequency induction heating until the high-performance copper-tin alloy ultrafine wire of the target size is obtained.

3. The method for preparing high-performance copper-tin alloy ultrafine wire according to claim 2, characterized in that, In step S1, the raw material is placed in a vacuum induction furnace for melting, with a vacuum degree ≤1×10⁻⁶. - The melting temperature is 1200-1300℃, the melting time is 2-3 hours, and electromagnetic stirring at 10-20 Hz is applied during the melting process. After the melting is completed, an alloy ingot is cast using a steel mold preheated to 200-300℃.

4. The method for preparing high-performance copper-tin alloy ultrafine wire according to claim 2, characterized in that, In step S1, the purity of the high-purity copper is ≥99.4%; the nickel is added in the form of a copper-nickel master alloy, and the phosphorus is added in the form of a copper-phosphorus master alloy with a purity ≥99.95%.

5. The method for preparing high-performance copper-tin alloy ultrafine wire according to claim 2, characterized in that, In step S2, the ingot preheating and heat preservation include: preheating to 850℃~950℃ and holding for 1h~2h.

6. The method for preparing high-performance copper-tin alloy ultrafine wire according to claim 2, characterized in that, In step S2, a hydraulic press is used for multi-pass hot forging, with each pass involving a deformation of 30% to 40%, a total deformation of ≥80%, and a temperature of ≥750℃ during the hot forging process.

7. The method for preparing high-performance copper-tin alloy ultrafine wire according to claim 2, characterized in that, In step S3, the annealing temperature is 550–650°C, and the holding time is 2–4 hours.

8. The method for preparing high-performance copper-tin alloy ultrafine wire according to claim 2, characterized in that, In step S3, the temperature is slowly cooled to below 200°C in a vacuum induction furnace.

9. The method for preparing high-performance copper-tin alloy ultrafine wire according to claim 2, characterized in that, In step S4, when the rough drawing diameter is ≥2mm, the deformation per pass in the rough drawing is 20% to 35%; when the intermediate drawing diameter is 0.5mm ≤ diameter <2mm, the deformation per pass in the intermediate drawing is 15% to 20%; when the finish drawing diameter is <0.5mm, the deformation per pass in the finish drawing is 5% to 15%.

10. The method for preparing high-performance copper-tin alloy ultrafine wire according to claim 2, characterized in that, In step S4, the online dynamic annealing is performed with an annealing temperature set to 300–450°C and an annealing time of 10–30 seconds.

Citation Information

Patent Citations

  • Ultrafine and ultra-long copper alloy wire and production method thereof

    CN107904434A