A method for preparing a high-toughness long-life wear-resistant steel rod with a nominal diameter of 30-50 mm

By integrating and innovating multiple processes and controlling the content of harmful elements, wear-resistant steel bars with high Rockwell hardness and excellent impact toughness are formed, solving the problem of insufficient hardness and toughness of existing wear-resistant steel bars and improving the wear resistance and service life of the product.

CN123132733APending Publication Date: 2026-11-20WUKUN STEEL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611243850.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-17
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

The existing wear-resistant steel bars have low and fluctuating hardness and insufficient impact toughness, which limits the product's service life and market competitiveness.

Method used

Through integrated innovation of multiple processes such as chemical composition design, converter smelting, deoxidation and alloying, LF furnace refining, VD furnace vacuum refining, continuous casting, billet cooling and temperature-controlled rolling, the content of harmful elements is controlled to be low, resulting in high Rockwell hardness and excellent impact toughness.

Benefits of technology

It significantly improves the wear resistance and service life of wear-resistant steel bars, broadens their application range, and enhances the product's market competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The application discloses a preparation method of a high-toughness super-life wear-resistant steel rod with a nominal diameter of 30-50 mm, and belongs to the technical field of steel metallurgy and black metal pressure processing. The steel rod product with low contents of harmful elements S and P, low levels of coarse inclusions, high surface Rockwell hardness and small fluctuation range, and excellent impact toughness is obtained through the integrated innovation of multiple processes such as chemical composition design, converter smelting, deoxidization alloying process, tapping slag washing, LF furnace refining, VD furnace vacuum refining, continuous casting, billet cooling, rolling heating system, temperature control rolling, and steel rod cooling, the wear resistance, safety and service life of the product are improved, the use range is widened, and the market competitiveness of the product is significantly improved. The yield strength of the wear-resistant steel rod can reach 810-850 ReL / MPa, the reduction of area is greater than or equal to 38.0, the coarse inclusions are not more than 2 levels, the surface Rockwell hardness reaches 65-67, and the impact toughness reaches 16-19 J / cm 2 .
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of iron and steel metallurgy and ferrous metal pressure processing technology, and relates to a method for preparing a high-toughness, long-life wear-resistant steel bar with a nominal diameter of 30-50mm. Background Technology

[0002] Wear-resistant steel bars are medium-to-high carbon alloy steel bars specifically designed for high-wear applications. They feature high hardness, high wear resistance, and good impact toughness, and are primarily used in various ball mills and rod mills to produce wear-resistant steel balls. These products are widely used in wear-resistant fields such as mining, cement, and building materials. After undergoing quenching and tempering heat treatment, wear-resistant steel bars are required to possess high hardness to effectively resist material cutting and wear; good surface quality, high cleanliness, and excellent impact toughness to ensure they are not easily broken or bent under significant impact and tumbling, guaranteeing safe equipment operation; and high wear resistance to significantly extend service life and reduce overall operating costs.

[0003] Currently, there are research reports on the production technology of B2 wear-resistant steel bars in China. The production process involves hot metal pretreatment → converter smelting → LF furnace refining → (vacuum refining) → large billet full-process protective casting → bar rolling. This process improves control measures and strengthens management throughout the entire steelmaking process, from raw materials and auxiliary materials to steelmaking and rolling equipment, process control technology, and production process management, ensuring that the round steel surface is free of quality defects such as cracks, folds, scabs, and burrs. However, the wear-resistant steel balls made from the currently produced wear-resistant steel bars mostly have a Rockwell hardness (HRC) of 52-61, which is relatively low and fluctuates greatly; the impact toughness is mostly between 11-13 J / cm. 2 The impact toughness is low. Because the high hardness and high toughness of the material cannot be combined with flexibility, it restricts the improvement of product service life and market competitiveness.

[0004] Therefore, it is necessary to provide a method for preparing high-toughness, long-life wear-resistant steel bars with a nominal diameter of 30-50mm, so as to further improve the hardness, impact toughness and service life of existing wear-resistant steel bars, broaden the application channels of the products, and enhance the market competitiveness of the products. Summary of the Invention

[0005] To overcome the problems in the background technology, this invention integrates and innovates multiple processes, including chemical composition design, converter smelting, deoxidation and alloying process, slag washing, LF furnace refining, VD furnace vacuum refining, continuous casting, billet cooling, rolling heating system, temperature-controlled rolling, and steel bar cooling. This results in the production of steel bars with low content of harmful elements S and P, low level of coarse inclusions, high surface Rockwell hardness with small fluctuation range, and excellent impact toughness. This improves the wear resistance, safety, and service life of the products, broadens their application range, and significantly enhances their market competitiveness.

[0006] To achieve the above objectives, the present invention is implemented through the following technical solution: This invention proposes a method for preparing a high-toughness, long-life wear-resistant steel bar with a nominal diameter of 30-50mm, which is achieved through the following steps: A. Hot metal pretreatment and desulfurization: Blast furnace hot metal is transported to the KR process hot metal pretreatment unit for desulfurization treatment. The hot metal temperature is ≥1380℃, the stirring head insertion depth is controlled at 1900mm, and the concentration is 10.0~12.0kg / t. 钢 Add the following mass ratio of conventional CaO and CaF2 desulfurizing agent for desulfurization treatment: CaO 81.5wt%, SiO2 2.5wt%, S 0.075wt%, CaF2 6.5wt%, with the remainder being unavoidable impurities. The stirring time is controlled at 4 minutes. After stirring, perform a slag removal operation to ensure that ≥4 / 5 of the molten iron surface in the ladle is exposed and remove the desulfurization slag.

[0007] B. Steelmaking: The molten iron obtained from pre-treatment and desulfurization and high-quality scrap steel are processed at 920 kg / t. 钢 138kg / t 钢 The slag is added to the LD converter in the specified proportions and subjected to conventional top and bottom combined blowing. The converter smelting adopts the double slag method. In the early stage of smelting, the first batch of slag is added at 12-14 kg / t. 钢 10-12 kg / t 钢 Lime and lightly calcined dolomite are added to form slag. After the first batch of slag is formed and the furnace is turned over, a second batch of slag is added at a rate of 10-12 kg / t. 钢 8kg / t 钢 Lime and lightly calcined dolomite are added to form slag again, controlling the final carbon content of the molten steel to be 0.20wt%~0.35wt%, and the tapping temperature to ≤1600℃. Before tapping, active lime is added to the bottom of the ladle for slag washing, with a lime addition rate of 1.0 kg / t. 钢 The steel tapping process adopts a bottom-blowing argon process throughout, with the argon flow rate controlled at 20~25 NL / min.

[0008] C. Deoxidation and Alloying: After the smelting of the molten steel is completed, when the amount of molten steel in the ladle is greater than 1 / 4, deoxidize and alloy in the following order: low-aluminum silicon-calcium-barium → ferrosilicon → high-carbon ferromanganese → high-carbon ferrochromium. Add the following substances to the ladle in sequence at a rate of 1.2 kg / t. 钢 Add the following low-alumina silicon-calcium-barium alloy in the following mass ratio: Si 52.2wt%, Al 0.8wt%, Ca 8.7wt%, Ba 11.3wt%, P 0.025wt%, S 0.018wt%, with the remainder being Fe and unavoidable impurities; at a rate of 2.8~3.2 kg / t. 钢Add the following ferrosilicon in the specified mass ratio: Si 72.2wt%, Al 1.5wt%, P 0.025wt%, S 0.018wt%, with the remainder being Fe and unavoidable impurities; at a concentration of 9.9~10.2 kg / t. 钢 Add the following high-carbon ferromanganese in the specified mass ratio: Mn 76.5wt%, C 6.7wt%, P 0.024wt%, S 0.015wt%, with the remainder being Fe and unavoidable impurities; at a concentration of 10.2~10.6 kg / t. 钢 Add the following high-carbon ferrochrome in the specified mass ratio: Cr 54.5 wt%, C 7.4 wt%, P 0.045 wt%, S 0.018 wt%, with the remainder being Fe and unavoidable impurities; add the above alloy when the ladle reaches 4 / 5 of its capacity.

[0009] D. Steel refining in the LF furnace: After tapping, the molten steel is hoisted to the LF furnace refining station and connected to the argon gas line. Argon gas is then blown at a low rate of 20-25 NL / min for 3 minutes. Then, the lower electrode is used to slag at setting 7-9, and 0.3-0.5 kg / t of ferrosilicon powder is added. 钢 Adjust the slag; after energizing for 8 minutes, raise the electrodes to observe the slag formation inside the furnace, then measure the temperature and take samples; if the slag is too thin, add 4.0–5.0 kg / t of lime. 钢 Then add 0.7 kg / t of ferrosilicon powder. 钢 0.5 kg / t of calcium carbide 钢 For slag adjustment, add pre-melted refining slag to adjust the slag basicity to 4.0~5.0; based on the steel sample analysis results, add alloys to adjust the steel composition, ensuring that all chemical components are within the target range, and control the oxygen activity of the molten steel ≤15ppm; control the number of electrode passes during the refining process ≤3; then heat the molten steel to 1600~1615℃, and use a small argon flow rate of 20~25NL / min to perform soft blowing of argon into the molten steel for 5 minutes, after which add a steel covering agent at a controlled amount of 1.0 kg / t. 钢 Then the molten steel is hoisted to the vacuum refining station of the VD furnace.

[0010] E. Vacuum Refining of Molten Steel in VD Furnace: After hoisting the molten steel from step D to the VD vacuum refining furnace, connect the argon blowing pipe and start argon gas blowing at a small rate of 20-30 NL / min for 2 minutes. Then, determine the oxygen content of the molten steel and simultaneously measure the temperature and take samples. After sampling, move the vacuum tank cover to the working position, close the cover, and begin vacuuming. When the vacuum reaches 67 Pa, begin vacuum degassing treatment while simultaneously performing bottom argon blowing. Control the argon gas flow rate at 40-50 NL / min. The degassing treatment time is 20 minutes under a vacuum of 67 Pa. After vacuum degassing, close the main vacuum valve, raise the tank cover, and take samples of the molten steel for oxygen and hydrogen determination. Then, perform soft argon blowing on the molten steel at a small rate of 20-30 NL / min for 4 minutes. After soft argon blowing, add a covering agent to the molten steel at a rate of 1.0 kg / t. 钢 Then the molten steel is hoisted to the casting station.

[0011] F. Steel casting: Under the conditions of tundish temperature of 1480~1495℃, casting speed of 1.8~1.9m / min, secondary cooling water volume of 0.6~0.7L / kg, crystallizer electromagnetic stirring current intensity of 300A and operating frequency of 3Hz, the molten steel obtained in step E is continuously cast into steel billets with a cross section of 165mm×165mm using a 7-strand small square billet casting machine with R9m straight arc continuous straightening.

[0012] G. Steel billet cooling: The steel billets from step F are sent to a designated area and stacked tightly into a pile. The residual heat of the steel billets themselves is used to keep them warm and slowly cool them down to below room temperature (25°C).

[0013] H. Steel billet heating: The steel billet from step G is sent into a heating furnace with a soaking section temperature of 1070~1100℃. After heating for 70~90 minutes, the billet is tapped, descaled by high-pressure water, and pushed to a fully continuous 16-stand bar rolling mill for rolling. The heating furnace is controlled with a reducing atmosphere to reduce steel billet oxidation and surface decarburization.

[0014] I. Temperature-controlled rolling: The steel billet from step H is fed into a two-roll high-rigidity short-stress bar mill with diameters of Φ650mm×6+Φ450mm×6+Φ450mm×2 for rolling. Under rolling conditions of 0.6~1.6m / s, it is rough rolled for 6 passes on the roughing mill; then, under rolling conditions of 2.8~4.8m / s, it is rolled for 4 passes on the intermediate rolling mill; finally, under rolling conditions of 5.2~8.8m / s, it is finished rolled for 2~4 passes on the finishing mill. After that, the rolled piece is cut into fixed lengths, bundled, and stacked for cooling. Once cooled to room temperature, high-toughness, long-life wear-resistant steel bars with a nominal diameter of 30~50mm are obtained.

[0015] Preferably, in step A, the chemical composition of the blast furnace molten iron, by mass percentage, includes C: 4.2-4.5%, Si: 0.15-0.30%, Mn: 0.20-0.30%, P: 0.070-0.090%, S≤0.035%, with the balance being Fe and unavoidable impurities.

[0016] Preferably, in step A, the chemical composition of the blast furnace molten iron is: C 4.2-4.5wt%, Si 0.15-0.30wt%, Mn 0.20-0.30wt%, P 0.070-0.090wt%, S≤0.035wt%, with the remainder being Fe and unavoidable impurities.

[0017] Preferably, in step B, the chemical composition of the pretreated desulfurized molten iron is: C 4.2-4.5%, Si 0.15-0.30%, Mn 0.20-0.30%, P 0.070-0.090%, S≤0.007%, with the remainder being Fe and unavoidable impurities; the chemical composition of the high-quality scrap steel is: C 0.21-0.26wt%, Si 0.25-0.50wt%, Mn 1.15-1.45wt%, P 0.020-0.035wt%, S 0.015-0.028wt%, with the remainder being Fe and unavoidable impurities.

[0018] Preferably, in step H, the tapping temperature is 960~990℃.

[0019] Preferably, in step I, the stack cooling temperature is ≤400℃.

[0020] In another aspect, this invention provides a high-toughness, long-life wear-resistant steel bar with a nominal diameter of 30-50 mm prepared by the above-mentioned preparation method. The wear-resistant steel bar has the following chemical composition by weight percentage: C 0.79-0.82 wt%, Si 0.22-0.28 wt%, Mn 0.82-0.88 wt%, Cr... The composition is as follows: 0.57-0.64 wt%, S≤0.007 wt%, P≤0.008 wt%, O≤0.0015 wt%, N≤0.0020 wt%, H≤0.0001 wt%, with the remainder being Fe and unavoidable impurities; the microstructure of the high-toughness, long-life wear-resistant steel bar is 86%~90% sorbite and 10~14% pearlite; the yield strength ReL of the wear-resistant steel bar is 810~850 MPa; the reduction of area Z≥38.0%; the surface hardness HRC of the wear-resistant steel balls produced from the wear-resistant steel bar is 65~67; and the impact toughness of the wear-resistant steel balls produced from the wear-resistant steel bar is 16~19 J / cm. 2 The coarse inclusions in the wear-resistant steel bar are grade A+B+C+D≤2.0.

[0021] The beneficial effects of this invention are: 1. This invention employs a top-and-bottom combined blowing argon blowing mode in converter smelting, controlling the final carbon content to 0.20wt%-0.35wt% for high-carbon tapping. The tapping process utilizes full-process slag washing, significantly reducing the total oxygen content of the molten steel and improving its cleanliness. A dual-slag dephosphorization method is used, achieving a dephosphorization rate >95%, significantly reducing the final phosphorus content and substantially decreasing the content of harmful elements in the molten steel. A certain amount of Cr is added to the steel to form alloy carbides, improving the hardenability and strengthening the steel matrix's strength and toughness. The LF furnace uses ferrosilicon powder for slag conditioning and deoxidation, avoiding the formation of brittle Al2O3 inclusions and improving the impact toughness and durability of the steel bars. Wear resistance; the molten steel undergoes vacuum refining in a VD furnace, significantly reducing the gas content and inclusions in the steel, thus improving the ductility, toughness, and wear resistance of the steel bars; the billet in the rolling process is heated at a lower temperature, reducing billet oxidation and surface decarburization, and controlling the initial rolling temperature promotes the refinement of austenite grains and accelerates the transformation rate of supercooled austenite during phase transformation, resulting in a fine sorbite + pearlite microstructure with excellent ductility and toughness; both the billet and steel bar are subjected to slow cooling, which rapidly promotes the release of thermal stress, eliminates the hydrogen embrittlement effect, avoids crack defects in the billet and steel bar, and improves the wear resistance and service life of the wear-resistant steel balls.

[0022] 2. The wear-resistant steel bars prepared by this invention have high steel cleanliness, low gas content and low content of harmful elements S and P, with P≤0.008wt%, S≤0.007wt%, O≤0.0015wt%, N≤0.0020wt%, H≤0.0001wt%, and coarse inclusions A+B+C+D≤2.0 grade; the wear-resistant steel balls produced from it have a Rockwell hardness HRC of 65-67, high hardness with small fluctuation, and an impact toughness of 16-19 J / cm. 2 Between these parameters, the impact toughness is excellent; this invention improves the product's wear resistance, safety, and service life, broadens its application range, and significantly enhances the product's market competitiveness.

[0023] 3. The process of this invention has strong applicability and controllability. The wear-resistant steel bars produced have high cleanliness, high toughness, and long service life. The wear-resistant steel balls produced by it have high hardness and small fluctuations, good quality uniformity, and excellent impact toughness, making them suitable for large-scale industrial application. Detailed Implementation

[0024] The present invention will be further described in detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited to the content described.

[0025] Example 1 This embodiment prepares wear-resistant steel bars using the following method: A. Hot Metal Pretreatment and Desulfurization: Blast furnace hot metal (chemical composition: C 4.2wt%, Si 0.15wt%, Mn 0.20wt%, P 0.070wt%, S 0.035wt%, balance Fe and unavoidable impurities) is transported to the KR process hot metal pretreatment unit for desulfurization treatment. The hot metal temperature is 1380℃, the stirring head insertion depth is controlled at 1900mm, and the treatment rate is 10.0kg / t. 钢 Add the following amounts of desulfurizing agent: CaO 81.5wt%, SiO2 2.5wt%, S 0.075wt%, CaF2 6.5wt%, with the remainder being unavoidable impurities. Control the stirring time to 4 minutes. After stirring, perform the slag removal operation to ensure that ≥4 / 5 of the molten iron surface in the ladle is exposed and remove the desulfurization slag.

[0026] The composition of the molten iron after pretreatment is controlled as follows: C 4.2wt%, Si 0.15wt%, Mn 0.20wt%, P 0.070wt%, S 0.007wt%, with the remainder being Fe and unavoidable impurities.

[0027] B. Steelmaking: The pretreated, deeply desulfurized molten iron from step A and high-quality scrap steel (chemical composition: C 0.21wt%, Si 0.25wt%, Mn 1.15wt%, P 0.020wt%, S 0.015wt%, the remainder being Fe and unavoidable impurities) are processed at 920 kg / t. 钢 138kg / t 钢 Molten iron and high-quality scrap steel are added to the LD converter in a specific ratio for conventional top and bottom combined blowing. The converter smelting adopts the double-slag method. In the early stage of smelting, the first batch of slag is prepared at 12 kg / t. 钢 10kg / t 钢 Lime and lightly calcined dolomite are added to form slag. After the first batch of slag is formed and the furnace is turned over, the second batch of slag is added at a rate of 10 kg / t. 钢 8kg / t 钢 Lime and lightly calcined dolomite are added to form slag again, controlling the final carbon content of the molten steel to 0.20 wt%, and the tapping temperature to 1600℃. Before tapping, active lime is added to the bottom of the ladle for slag washing, with a lime addition rate of 1.0 kg / t. 钢 The steel tapping process adopts a bottom-blowing argon process throughout, with the argon flow rate controlled at 20 NL / min.

[0028] C. Deoxidation and Alloying: After tapping the molten steel from step B, when the ladle contains more than 1 / 4 tonnes of molten steel, deoxidize and alloy it in the following order: low-aluminum silicon-calcium-barium → ferrosilicon → high-carbon ferromanganese → high-carbon ferrochromium. Add the following substances sequentially to the ladle at a rate of 1.2 kg / t. 钢The following amounts of low-alumina silicon-calcium-barium alloy were added (Si 52.2wt%, Al 0.8wt%, Ca 8.7wt%, Ba 11.3wt%, P 0.025wt%, S 0.018wt%, with the remainder being Fe and unavoidable impurities); at a rate of 2.8 kg / t. 钢 The amount of ferrosilicon added is 72.2 wt% Si, 1.5 wt% Al, 0.025 wt% P, 0.018 wt% S, with the remainder being Fe and unavoidable impurities; at 9.9 kg / t 钢 The following amount of high-carbon ferromanganese (Mn 76.5wt%, C 6.7wt%, P 0.024wt%, S 0.015wt%, the remainder being Fe and unavoidable impurities) was added at a rate of 10.2 kg / t. 钢 Add high-carbon ferrochrome (Cr 54.5wt%, C 7.4wt%, P 0.045wt%, S 0.018wt%, the remainder being Fe and unavoidable impurities) to the ladle when the molten steel reaches 4 / 5 of its capacity; after tapping, the molten steel is hoisted to the LF furnace for refining.

[0029] D. Steel refining in the LF furnace: After tapping the molten steel in step C, hoist it to the LF furnace refining station, connect the argon gas line, and start the argon gas supply at a low rate (20 NL / min) for 3 minutes. Then, lower the electrode and use setting 7-9 for slag formation, adding 0.3 kg / t of argon gas. 钢 Ferrosilicon powder is used to adjust the slag; after energizing for 8 minutes, the electrodes are raised to observe the slag formation inside the furnace, followed by temperature measurement and sampling; if the slag is too thin, 4.0 kg / t is added. 钢 Add lime, then add 0.7 kg / t 钢 Ferrosilicon powder, 0.5 kg / t 钢 Calcium carbide is used to adjust the slag, and conversely, pre-melted refining slag is added to adjust the slag, controlling the slag basicity to 4.0. Based on the steel sample analysis results, alloys are added to adjust the composition of the molten steel, ensuring that all chemical components are within the target range, and controlling the oxygen activity of the molten steel to 15 ppm. The number of electrode passes during the refining process is controlled to 3. Then, the molten steel temperature is heated to 1615℃, and soft blowing of argon gas is performed on the molten steel using a small flow rate of 20 NL / min for 5 minutes. After that, a steel covering agent is added, with the addition amount controlled at 1.0 kg / t. 钢 Then the molten steel is hoisted to the vacuum refining station of the VD furnace.

[0030] E. Vacuum Refining of Molten Steel in VD Furnace: After hoisting the molten steel from step D to the VD vacuum refining furnace, connect the argon blowing pipe and purge with a small argon flow rate (20 NL / min) for 2 minutes. Then, determine the oxygen content of the molten steel and simultaneously measure the temperature and take samples. After sampling, move the vacuum tank cover to the working position, close the cover, and begin vacuuming. When the vacuum reaches 67 Pa, begin vacuum degassing treatment while simultaneously performing bottom argon blowing. The argon flow rate is controlled at 40 NL / min, and the degassing time is 20 minutes under a vacuum of 67 Pa. After vacuum degassing, close the main vacuum valve, raise the tank cover, and take samples of the molten steel for oxygen and hydrogen determination. Then, perform soft argon blowing with a small argon flow rate of 20 NL / min for 4 minutes. After soft argon blowing, add a covering agent to the molten steel at a rate of 1.0 kg / t. 钢 Then the molten steel is hoisted to the casting station.

[0031] F. Steel casting: Under the conditions of tundish temperature of 1495℃, casting speed of 1.8m / min, secondary cooling water volume of 0.6L / kg, crystallizer electromagnetic stirring current intensity of 300A and operating frequency of 3Hz, the molten steel from step E is continuously cast into billets with a cross section of 165mm×165mm using a 7-strand small square billet casting machine with R9m straight arc continuous straightening.

[0032] G. Steel billet cooling: The steel billets from step F are sent to a designated area and stacked tightly into a pile. The residual heat of the steel billets themselves is used to keep them warm and cool them slowly, reducing the temperature of the steel billets to below 25°C.

[0033] H. Billet heating: The billet from step G is sent into a heating furnace with a soaking section temperature of 1100℃ and heated for 70 minutes. The furnace is controlled to maintain a reducing atmosphere to reduce billet oxidation and surface decarburization. The billet exits at a temperature of 990℃ and is then descaled by high-pressure water before being pushed to a fully continuous 16-stand bar mill for rolling.

[0034] I. Temperature-controlled rolling: The steel billet from step H is fed into a fully continuous 16-stand bar mill for rolling. It is roughed for 6 passes at a speed of 0.6 m / s on the roughing mill; then it is rolled for 4 passes at a speed of 2.8 m / s on the intermediate mill; finally, it is rolled for 4 passes at a speed of 5.2 m / s on the finishing mill. After that, the rolled piece is cut into fixed lengths, bundled and stacked for cooling at a temperature of 400℃. After cooling to room temperature, a high-toughness, long-life wear-resistant steel bar with a nominal diameter of 30 mm is obtained.

[0035] The chemical composition of the wear-resistant steel bar obtained in this embodiment is as follows: C 0.79wt%, Si 0.22wt%, Mn 0.82wt%, Cr 0.57wt%, S 0.007wt%, P 0.008wt%, O 0.0015wt%, N 0.0020wt%, H 0.0001wt%, with the remainder being Fe and unavoidable impurities.

[0036] The mechanical properties, microstructure, and inclusions of the wear-resistant steel bars prepared in this embodiment are shown in Tables 1 and 2.

[0037] Table 1 Table 2 Example 2 A. Hot Metal Pretreatment and Desulfurization: Blast furnace hot metal (chemical composition: C 4.3wt%, Si 0.24wt%, Mn 0.24wt%, P 0.080wt%, S 0.025wt%, the remainder being Fe and unavoidable impurities) is transported to the KR process hot metal pretreatment unit for desulfurization treatment. The hot metal temperature is 1400℃, the stirring head insertion depth is controlled at 1900mm, and the concentration is 11.0kg / t. 钢 Add the appropriate amount of CaO and CaF2 desulfurizing agent (CaO 81.5wt%, SiO2 2.5wt%, S 0.075wt%, CaF2 6.5wt%, the remainder being unavoidable impurities), and control the stirring time to 4 minutes; after stirring, perform the slag removal operation to ensure that the molten iron surface in the ladle is exposed by ≥4 / 5, and remove the desulfurization slag.

[0038] The composition of the molten iron after pretreatment is controlled as follows: C 4.3wt%, Si 0.24wt%, Mn 0.25wt%, P 0.080wt%, S 0.005wt%, with the remainder being Fe and unavoidable impurities.

[0039] B. Steelmaking: The pretreated, deeply desulfurized molten iron from step A and high-quality scrap steel (chemical composition: C 0.24wt%, Si 0.35wt%, Mn 1.33wt%, P 0.028wt%, S 0.021wt%, the remainder being Fe and unavoidable impurities) are processed at 920 kg / t. 钢 138kg / t 钢 Molten iron and high-quality scrap steel are added to the LD converter in a specific ratio for conventional top and bottom combined blowing. The converter smelting adopts the double-slag method. In the early stage of smelting, the first batch of slag is prepared at 13 kg / t. 钢 11kg / t 钢Lime and lightly calcined dolomite are added to form slag. After the first batch of slag is formed and the furnace is turned over, the second batch of slag is added at a rate of 11 kg / t. 钢 8kg / t 钢 Lime and lightly calcined dolomite are added to form slag again, controlling the final carbon content of the molten steel to 0.28 wt% and the tapping temperature to 1595℃. Before tapping, active lime is added to the bottom of the ladle for slag washing, with a lime addition rate of 1.0 kg / t. 钢 The steel tapping process adopts a bottom-blowing argon process throughout, with the argon flow rate controlled at 23 NL / min.

[0040] C. Deoxidation and Alloying: After tapping the molten steel from step B, when the ladle contains more than 1 / 4 tonnes of molten steel, deoxidize and alloy it in the following order: low-aluminum silicon-calcium-barium → ferrosilicon → high-carbon ferromanganese → high-carbon ferrochromium. Add the following substances sequentially to the ladle at a rate of 1.2 kg / t. 钢 The following amounts of low-alumina silicon-calcium-barium alloy were added (Si 52.2wt%, Al 0.8wt%, Ca 8.7wt%, Ba 11.3wt%, P 0.025wt%, S 0.018wt%, with the remainder being Fe and unavoidable impurities); at a rate of 3.0 kg / t. 钢 The amount of ferrosilicon added is 72.2 wt% Si, 1.5 wt% Al, 0.025 wt% P, 0.018 wt% S, with the remainder being Fe and unavoidable impurities; at a rate of 10.0 kg / t. 钢 The following amount of high-carbon ferromanganese (Mn 76.5wt%, C 6.7wt%, P 0.024wt%, S 0.015wt%, the remainder being Fe and unavoidable impurities) was added at a rate of 10.4 kg / t. 钢 The following amounts of high-carbon ferrochrome (Cr 54.5wt%, C 7.4wt%, P 0.045wt%, S 0.018wt%, with the remainder being Fe and unavoidable impurities) are added; the above alloys are added when the ladle reaches 4 / 5 of its capacity; after tapping, the molten steel is hoisted to the LF furnace for refining.

[0041] D. Steel refining in the LF furnace: After tapping the molten steel in step C, hoist the molten steel to the LF furnace refining station, connect the argon gas line, turn on the argon gas and purge with a small argon flow rate (23 NL / min) for 3 minutes. Then, lower the electrode and use setting 7-9 for slag formation, adding 0.4 kg / t of slag. 钢 Ferrosilicon powder is used to adjust the slag; after energizing for 8 minutes, the electrodes are raised to observe the slag formation inside the furnace, followed by temperature measurement and sampling; if the slag is too thin, 4.6 kg / t is added. 钢 Add lime, then add 0.7 kg / t 钢 Ferrosilicon powder, 0.5 kg / t 钢Calcium carbide is used to adjust the slag, and conversely, pre-melted refining slag is added to adjust the slag, controlling the slag basicity to 4.7. Based on the steel sample analysis results, alloys are added to adjust the steel composition, ensuring all chemical components are within the target range, and the oxygen activity of the molten steel is controlled at 13 ppm. The number of electrode passes during the refining process is controlled to be 2. Then, the molten steel is heated to 1608℃, and soft blowing of argon gas is performed at a flow rate of 23 NL / min for 5 minutes. Afterwards, a steel covering agent is added at a rate of 1.0 kg / t. 钢 Then the molten steel is hoisted to the vacuum refining station of the VD furnace.

[0042] E. Vacuum Refining of Molten Steel in VD Furnace: After hoisting the molten steel from step D to the VD vacuum refining furnace, connect the argon blowing pipe and purge with a small argon flow rate (25 NL / min) for 2 minutes. Then, determine the oxygen content of the molten steel and simultaneously measure the temperature and take samples. After sampling, move the vacuum tank cover to the working position, close the cover, and begin vacuuming. When the vacuum reaches 67 Pa, begin vacuum degassing treatment while simultaneously performing bottom argon blowing. The argon flow rate is controlled at 45 NL / min, and the degassing time is 20 minutes under a vacuum of 67 Pa. After vacuum degassing, close the main vacuum valve, raise the tank cover, and take samples of the molten steel for oxygen and hydrogen determination. Then, perform soft argon blowing with a small argon flow rate of 25 NL / min for 4 minutes. After soft argon blowing, add a covering agent to the molten steel at a rate of 1.0 kg / t. 钢 Then the molten steel is hoisted to the casting station.

[0043] F. Steel casting: Under the conditions of tundish temperature of 1490℃, casting speed of 1.9m / min, secondary cooling water volume of 0.65L / kg, crystallizer electromagnetic stirring current intensity of 300A and operating frequency of 3Hz, the molten steel from step E is continuously cast into billets with a cross section of 165mm×165mm using a 7-strand small square billet casting machine with R9m straight arc continuous straightening.

[0044] G. Steel billet cooling: The steel billets from step F are sent to a designated area and stacked tightly into a pile. The residual heat of the steel billets themselves is used to keep them warm and slowly cool them down to below room temperature (25°C).

[0045] H. Steel billet heating: The steel billet from step G is sent into a heating furnace with a soaking section temperature of 1090℃ and heated for 80 minutes. The furnace is controlled to maintain a reducing atmosphere to reduce steel billet oxidation and surface decarburization. The steel billet exits at a temperature of 980℃ and is then descaled by high-pressure water and pushed to a fully continuous 16-stand bar mill for rolling.

[0046] I. Temperature-controlled rolling: The steel billet from step H is fed into a fully continuous 16-stand bar mill for rolling. It is roughed for 6 passes at a speed of 1.6 m / s on the roughing mill; then it is rolled for 4 passes at a speed of 4.8 m / s on the intermediate mill; and finally it is rolled for 3 passes at a speed of 8.8 m / s on the finishing mill. After that, the rolled piece is cut into fixed lengths, bundled and stacked for cooling at a temperature of 380℃. After cooling to room temperature, a high-toughness, long-life wear-resistant steel bar with a nominal diameter of 40 mm is obtained.

[0047] The chemical composition of the wear-resistant steel bar obtained in this embodiment is as follows: C 0.81wt%, Si 0.25wt%, Mn 0.86wt%, Cr 0.61wt%, S 0.005wt%, P 0.007wt%, O 0.0012wt%, N 0.0017wt%, H 0.00007wt%, with the remainder being Fe and unavoidable impurities.

[0048] The mechanical properties, microstructure, and inclusions of the wear-resistant steel bars prepared in this embodiment are shown in Tables 3 and 4.

[0049] Table 3 Table 4 Example 3 A. Hot Metal Pretreatment and Desulfurization: Blast furnace hot metal (chemical composition: C 4.5wt%, Si 0.30wt%, Mn 0.30wt%, P 0.090wt%, S 0.020wt%, the remainder being Fe and unavoidable impurities) is transported to the KR process hot metal pretreatment unit for desulfurization treatment. The hot metal temperature is 1410℃, the stirring head insertion depth is controlled at 1900mm, and the treatment rate is 12.0kg / t. 钢 Add the appropriate amount of CaO and CaF2 desulfurizing agent (CaO 81.5wt%, SiO2 2.5wt%, S 0.075wt%, CaF2 6.5wt%, the remainder being unavoidable impurities), and control the stirring time to 4 minutes; after stirring, perform the slag removal operation to ensure that the molten iron surface in the ladle is exposed by ≥4 / 5, and remove the desulfurization slag.

[0050] The composition of the molten iron after pretreatment is controlled as follows: C 4.5wt%, Si 0.30wt%, Mn 0.30wt%, S 0.090wt%, and the remainder is Fe and unavoidable impurities.

[0051] B. Steelmaking: The pretreated, deeply desulfurized molten iron from step A and high-quality scrap steel (chemical composition: C 0.26wt%, Si 0.50wt%, Mn 1.45wt%, P 0.035wt%, S 0.028wt%, the remainder being Fe and unavoidable impurities) are processed at 920 kg / t. 钢 138kg / t 钢 Molten iron and high-quality scrap steel are added to the LD converter in a specific ratio for conventional top and bottom combined blowing. The converter smelting employs a double-slag method. In the initial stage of smelting, lime and lightly calcined dolomite are added to the first batch of slag at 14 kg / t steel and 12 kg / t steel respectively to form slag. After the first batch of slag is formed and the furnace is turned over, the second batch of slag is added, at 12 kg / t steel. 钢 8kg / t 钢 Lime and lightly calcined dolomite are added to form slag again, controlling the final carbon content of the molten steel to 0.35 wt%, and the tapping temperature to 1585℃. Before tapping, active lime is added to the bottom of the ladle for slag washing, with a lime addition rate of 1.0 kg / t. 钢 The steel tapping process adopts a bottom-blowing argon process throughout, with the argon flow rate controlled at 25 NL / min.

[0052] C. Deoxidation and Alloying: After tapping the molten steel from step B, when the ladle contains more than 1 / 4 tonnes of molten steel, deoxidize and alloy it in the following order: low-aluminum silicon-calcium-barium → ferrosilicon → high-carbon ferromanganese → high-carbon ferrochromium. Add the following substances sequentially to the ladle at a rate of 1.2 kg / t. 钢 The following amounts of low-alumina silicon-calcium-barium alloy were added (Si 52.2wt%, Al 0.8wt%, Ca 8.7wt%, Ba 11.3wt%, P 0.025wt%, S 0.018wt%, with the remainder being Fe and unavoidable impurities); at a rate of 3.2 kg / t. 钢 The amount of ferrosilicon added (Si 72.2wt%, Al 1.5wt%, P 0.025wt%, S 0.018wt%, the remainder being Fe and unavoidable impurities) was 10.2 kg / t. 钢 Add high-carbon ferromanganese (Mn 76.5wt%, C 6.7wt%, P 0.024wt%, S 0.015wt%, the remainder being Fe and unavoidable impurities) in the specified amount; add high-carbon ferrochrome (Cr 54.5wt%, C 7.4wt%, P 0.045wt%, S 0.018wt%, the remainder being Fe and unavoidable impurities) in the amount required for 10.6kg / t of steel; the above alloys are added when the ladle is 4 / 5 full; after tapping, the molten steel is hoisted to the LF furnace for refining.

[0053] D. Steel refining in the LF furnace: After tapping the steel in step C, hoist the molten steel to the LF furnace refining station, connect the argon gas line, and start the argon gas supply at a low rate (25 NL / min) for 3 minutes. Then, lower the electrode and use setting 7-9 for slag formation, adding 0.5 kg / t of slag. 钢 Ferrosilicon powder is used to adjust the slag; after energizing for 8 minutes, the electrodes are raised to observe the slag formation inside the furnace, followed by temperature measurement and sampling; if the slag is too thin, 5.0 kg / t is added. 钢 Add lime, then add 0.7 kg / t 钢 Ferrosilicon powder, 0.5 kg / t 钢 Calcium carbide is used to adjust the slag, and conversely, pre-melted refining slag is added to adjust the slag, controlling the slag basicity to 5.0. Based on the steel sample analysis results, alloys are added to adjust the composition of the molten steel, ensuring that all chemical components are within the target range, and controlling the oxygen activity of the molten steel to 10 ppm. The number of electrode passes during the refining process is controlled to be 2. Then, the molten steel temperature is heated to 1600℃, and soft blowing of argon gas is performed on the molten steel using a small flow rate of 25 NL / min for 5 minutes. After that, a steel covering agent is added, with the addition amount controlled at 1.0 kg / t. 钢 Then the molten steel is hoisted to the vacuum refining station of the VD furnace.

[0054] E. Vacuum Refining of Molten Steel in VD Furnace: After hoisting the molten steel from step D to the VD vacuum refining furnace, connect the argon blowing pipe and purge with a small argon flow rate (30 NL / min) for 2 minutes. Then, determine the oxygen content of the molten steel and simultaneously measure the temperature and take samples. After sampling, move the vacuum tank cover to the working position, close the cover, and begin vacuuming. When the vacuum reaches 67 Pa, begin vacuum degassing treatment while simultaneously performing bottom argon blowing. The argon flow rate is controlled at 50 NL / min, and the degassing time is 20 minutes under a vacuum of 67 Pa. After vacuum degassing, close the main vacuum valve, raise the tank cover, and take samples of the molten steel for oxygen and hydrogen determination. Then, perform soft argon blowing with a small argon flow rate of 30 NL / min for 4 minutes. After soft argon blowing, add a covering agent to the molten steel at a rate of 1.0 kg / t. 钢 Then the molten steel is hoisted to the casting station.

[0055] F. Steel casting: Under the conditions of tundish temperature of 1480℃, casting speed of 1.9m / min, secondary cooling water volume of 0.7L / kg, crystallizer electromagnetic stirring current intensity of 300A, and operating frequency of 3Hz, the molten steel from step E is continuously cast into billets with a cross section of 165mm×165mm using a 7-strand small square billet casting machine with R9m straight arc continuous straightening.

[0056] G. Steel billet cooling: The steel billets from step F are sent to a designated area and stacked tightly into a pile. The residual heat of the steel billets themselves is used to keep them warm and slowly cool them down to below room temperature (25°C).

[0057] H. Steel billet heating: The steel billet from step G is sent into a heating furnace with a soaking section temperature of 1070℃ and heated for 90 minutes. The furnace is controlled to maintain a reducing atmosphere to reduce steel billet oxidation and surface decarburization. The steel billet exits at a temperature of 960℃ and is then descaled by high-pressure water and pushed to a fully continuous 16-stand bar mill for rolling.

[0058] I. Temperature-controlled rolling: The steel billet from step H is fed into a fully continuous 16-stand bar mill for rolling. It is roughed for 6 passes at a speed of 1.0 m / s on the roughing mill; then it is rolled for 4 passes at a speed of 4.0 m / s on the intermediate mill; finally, it is finished for 2 passes at a speed of 7.2 m / s on the finishing mill. After that, the rolled piece is cut into fixed lengths, bundled and stacked for cooling at a temperature of 360°C. After cooling to room temperature, a high-toughness, long-life wear-resistant steel bar with a nominal diameter of 50 mm is obtained.

[0059] The wear-resistant steel bar obtained in this embodiment has the following chemical composition: C 0.82wt%, Si 0.28wt%, Mn 0.88wt%, Cr 0.64wt%, S 0.005wt%, P 0.004wt%, O 0.0010wt%, N 0.0014wt%, H 0.00005wt%, with the remainder being Fe and unavoidable impurities.

[0060] The mechanical properties, microstructure, and inclusions of the wear-resistant steel bars prepared in this embodiment are shown in Tables 5 and 6. Table 5 Table 6 In summary, this invention integrates and innovates multiple processes, including chemical composition design, converter smelting, deoxidation and alloying, slag washing, LF furnace refining, VD furnace vacuum refining, continuous casting, billet cooling, rolling heating system, temperature-controlled rolling, and steel bar cooling, to produce steel bars with low content of harmful elements S and P, low level of coarse inclusions, high surface Rockwell hardness with small fluctuation range, and excellent impact toughness. The process mechanical properties, microstructure, and inclusions of the high-toughness, ultra-long-life wear-resistant steel bars with a nominal diameter of 30-50mm prepared by this invention are shown in Tables 7 and 8.

[0061] Table 7 Table 8 Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made to it in form and detail without departing from the scope defined by the claims of the present invention.

Claims

1. A method for preparing a high-toughness, long-life wear-resistant steel bar with a nominal diameter of 30-50 mm, characterized in that, Follow these steps to achieve the following: A. Hot metal pretreatment and desulfurization: Blast furnace hot metal is transported to the KR process hot metal pretreatment unit for desulfurization treatment. The hot metal temperature is ≥1380℃, the stirring head insertion depth is controlled at 1900mm, and the concentration is 10.0~12.0kg / t. 钢 Add the following mass ratio of conventional CaO and CaF2 desulfurizing agent for desulfurization treatment: CaO 81.5wt%, SiO2 2.5wt%, S 0.075wt%, CaF2 6.5wt%, with the remainder being unavoidable impurities. The stirring time is controlled at 4 minutes. After stirring, perform a slag removal operation to ensure that ≥4 / 5 of the molten iron surface in the ladle is exposed and remove the desulfurization slag. B. Steelmaking: The molten iron obtained from pre-treatment and desulfurization and high-quality scrap steel are processed at 920 kg / t. 钢 138kg / t 钢 The slag is added to the LD converter in the specified proportions and subjected to conventional top and bottom combined blowing. The converter smelting adopts the double slag method. In the early stage of smelting, the first batch of slag is added at 12-14 kg / t. 钢 10-12 kg / t 钢 Lime and lightly calcined dolomite are added to form slag. After the first batch of slag is formed and the furnace is turned over, a second batch of slag is added at a rate of 10-12 kg / t. 钢 8kg / t 钢 Lime and lightly calcined dolomite are added to form slag again, controlling the final carbon content of the molten steel to be 0.20wt%~0.35wt%, and the tapping temperature to ≤1600℃. Before tapping, active lime is added to the bottom of the ladle for slag washing, with a lime addition rate of 1.0 kg / t. 钢 The steel tapping process adopts a bottom-blowing argon process throughout, with the argon flow rate controlled at 20~25 NL / min; C. Deoxidation and Alloying: After the smelting of the molten steel is completed, when the amount of molten steel in the ladle is greater than 1 / 4, deoxidize and alloy in the following order: low-aluminum silicon-calcium-barium → ferrosilicon → high-carbon ferromanganese → high-carbon ferrochromium. Add the following substances to the ladle in sequence at a rate of 1.2 kg / t. 钢 Add the following low-alumina silicon-calcium-barium alloy in the following mass ratio: Si 52.2wt%, Al 0.8wt%, Ca 8.7wt%, Ba 11.3wt%, P 0.025wt%, S 0.018wt%, with the remainder being Fe and unavoidable impurities; at a rate of 2.8~3.2 kg / t. 钢 Add the following ferrosilicon in the specified mass ratio: Si 72.2wt%, Al 1.5wt%, P 0.025wt%, S 0.018wt%, with the remainder being Fe and unavoidable impurities; at a concentration of 9.9~10.2 kg / t. 钢 Add the following high-carbon ferromanganese in the specified mass ratio: Mn 76.5wt%, C 6.7wt%, P 0.024wt%, S 0.015wt%, with the remainder being Fe and unavoidable impurities; at a concentration of 10.2~10.6 kg / t. 钢 Add the following high-carbon ferrochrome in the following mass ratio: Cr 54.5wt%, C 7.4wt%, P 0.045wt%, S 0.018wt%, with the remainder being Fe and unavoidable impurities; add the above alloy when the ladle reaches 4 / 5 of its capacity. D. Steel refining in the LF furnace: After tapping, the molten steel is hoisted to the LF furnace refining station and connected to the argon gas line. Argon gas is then blown at a low rate of 20-25 NL / min for 3 minutes. Then, the lower electrode is used to slag at setting 7-9, and 0.3-0.5 kg / t of ferrosilicon powder is added. 钢 Adjust the slag; after energizing for 8 minutes, raise the electrodes to observe the slag formation inside the furnace, then measure the temperature and take samples; if the slag is too thin, add 4.0–5.0 kg / t of lime. 钢 Then add 0.7 kg / t of ferrosilicon powder. 钢 0.5 kg / t of calcium carbide 钢 For slag adjustment, add pre-melted refining slag to adjust the slag basicity to 4.0~5.0; based on the steel sample analysis results, add alloys to adjust the steel composition, ensuring that all chemical components are within the target range, and control the oxygen activity of the molten steel ≤15ppm; control the number of electrode passes during the refining process ≤3; then heat the molten steel to 1600~1615℃, and use a small argon flow rate of 20~25NL / min to perform soft blowing of argon into the molten steel for 5 minutes, after which add a steel covering agent at a controlled amount of 1.0 kg / t. 钢 The molten steel is then hoisted to the vacuum refining station of the VD furnace; E. Vacuum Refining of Molten Steel in VD Furnace: After hoisting the molten steel from step D into the VD vacuum refining furnace, connect the argon blowing pipe and start argon gas blowing at a small rate of 20-30 NL / min for 2 minutes. Then, determine the oxygen content of the molten steel and simultaneously measure the temperature and take samples. After sampling, move the vacuum tank cover to the working position, close the cover, and begin vacuuming. When the vacuum reaches 67 Pa, begin vacuum degassing treatment while simultaneously performing bottom argon blowing. Control the argon gas flow rate at 40-50 NL / min. The degassing treatment time is 20 minutes under a vacuum of 67 Pa. After vacuum degassing, close the main vacuum valve, raise the tank cover, and take samples of the molten steel for oxygen and hydrogen determination. Then, perform soft argon blowing on the molten steel at a small rate of 20-30 NL / min for 4 minutes. After soft argon blowing, add a covering agent to the molten steel at a rate of 1.0 kg / t. 钢 Then the molten steel is hoisted to the casting station; F. Steel casting: Under the conditions of tundish temperature of 1480~1495℃, casting speed of 1.8~1.9m / min, secondary cooling water volume of 0.6~0.7L / kg, crystallizer electromagnetic stirring current intensity of 300A and operating frequency of 3Hz, the molten steel obtained in step E is continuously cast into steel billets with a cross section of 165mm×165mm using a 7-strand small square billet casting machine with R9m straight arc continuous straightening. G. Steel billet cooling: The steel billets from step F are sent to a designated site and stacked tightly into a stack. The residual heat of the steel billets themselves is used to keep them warm and slowly cool them down to below room temperature (25°C). H. Steel billet heating: The steel billet from step G is sent into a heating furnace with a soaking section temperature of 1070~1100℃. After heating for 70~90 minutes, the billet is tapped, descaled by high-pressure water, and pushed to a fully continuous 16-stand bar rolling mill for rolling. The heating furnace is controlled with a reducing atmosphere to reduce steel billet oxidation and surface decarburization. I. Temperature-controlled rolling: The steel billet from step H is fed into a two-roll high-rigidity short-stress bar mill with diameters of Φ650mm×6+Φ450mm×6+Φ450mm×2 for rolling. Under rolling conditions of 0.6~1.6m / s, it is rough rolled for 6 passes on the roughing mill; then, under rolling conditions of 2.8~4.8m / s, it is rolled for 4 passes on the intermediate rolling mill; finally, under rolling conditions of 5.2~8.8m / s, it is finished rolled for 2~4 passes on the finishing mill. After that, the rolled piece is cut into fixed lengths, bundled, and stacked for cooling. Once cooled to room temperature, high-toughness, long-life wear-resistant steel bars with a nominal diameter of 30~50mm are obtained.

2. The method for preparing a high-toughness, long-life wear-resistant steel bar with a nominal diameter of 30-50 mm according to claim 1, characterized in that, In step A, the chemical composition of the blast furnace molten iron is: C 4.2-4.5wt%, Si 0.15-0.30wt%, Mn 0.20-0.30wt%, P 0.070-0.090wt%, S≤0.035wt%, with the remainder being Fe and unavoidable impurities.

3. The method for preparing a high-toughness, long-life wear-resistant steel bar with a nominal diameter of 30-50 mm according to claim 1, characterized in that, In step B, the chemical composition of the pretreated desulfurized molten iron is: C 4.2-4.5%, Si 0.15-0.30%, Mn 0.20-0.30%, P 0.070-0.090%, S≤0.007%, with the remainder being Fe and unavoidable impurities; the chemical composition of the high-quality scrap steel is: C 0.21-0.26wt%, Si 0.25-0.50wt%, Mn 1.15-1.45wt%, P 0.020-0.035wt%, S 0.015-0.028wt%, with the remainder being Fe and unavoidable impurities.

4. The method for preparing a high-toughness, long-life wear-resistant steel bar with a nominal diameter of 30-50mm according to claim 1, characterized in that, In step H, the tapping temperature is 960~990℃.

5. The method for preparing a high-toughness, long-life wear-resistant steel bar with a nominal diameter of 30-50 mm according to claim 1, characterized in that, In step I, the stack cooling temperature is ≤400℃.

6. The high-toughness, long-life wear-resistant steel bar with a nominal diameter of 30-50 mm obtained by the preparation method according to any one of claims 1-5, characterized in that, The wear-resistant steel rod has the following chemical composition by weight percentage: C 0.79-0.82wt%, Si 0.22-0.28wt%, Mn 0.82-0.88wt%, Cr 0.57-0.64wt%, S≤0.007wt%, P≤0.008wt%, O≤0.0015wt%, N≤0.0020wt%, H≤0.0001wt%, with the remainder being Fe and unavoidable impurities. The microstructure of the high-toughness, long-life wear-resistant steel rod is 86%-90% sorbite and 10-14% pearlite. The yield strength ReL of the wear-resistant steel rod is 810-850MPa, the reduction of area Z≥38.0%, the surface hardness HRC of the wear-resistant steel balls produced from the wear-resistant steel rod is 65-67, and the impact toughness of the wear-resistant steel balls produced from the wear-resistant steel rod is 16-19 J / cm². 2 The coarse inclusions in the wear-resistant steel bar are grade A+B+C+D≤2.0.