A homogenization process for large forgings of gamma-prime precipitation strengthened nickel-based superalloys
By combining alternating cross-solution line thermal pulses and forced air cooling, the problem of uneven γ′ solid solution in the heat center of large γ′ precipitation-strengthened nickel-based superalloy forgings was solved during heat treatment, achieving uniformity in microstructure and properties and improving the quality of the forgings.
Patent Information
- Application Number
- CN202611635743.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-21
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies, when processing large forgings of γ′ precipitation-strengthened nickel-based superalloys, struggle to achieve the required γ′ solid solution level in the thermal center without extending the single-stage high-temperature holding time, while simultaneously avoiding excessive solid solution on the surface and grain coarsening.
By employing alternating cross-solution line thermal pulses, multiple small-amplitude high-temperature and low-temperature segments are alternately processed, combined with initial forced air cooling and residual heat recovery technology, to control the temperature difference between different layers of the forging, ensuring that the thermal center reaches a quantifiable γ′ solid solution degree, and limiting excessive solid solution on the surface layer.
Effective γ′ solid solution of the thermal center was achieved, while excessive growth of surface grains was suppressed, improving the microstructure uniformity and mechanical properties of the forging and reducing the tensile stress peak caused by rapid cooling.
Smart Images

Figure CN123132784A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of high-temperature alloy heat treatment technology, and in particular to a homogenization process for large nickel-based high-temperature alloy forgings with γ′ precipitation strengthening. Background Technology
[0002] Among γ′ precipitation-strengthened nickel-based superalloys, GH4700 belongs to the Ni-Cr-Co based γ′ precipitation-strengthened wrought superalloy. The nominal composition used in publicly available research is approximately 0.05% C, 25% Cr, 20% Co, 1.65% Nb, 1.47% Al, 1.69% Ti, with the balance being Ni. During solution treatment at 1000–1060℃, γ′ gradually dissolves into the matrix accompanied by significant grain growth. Further heating at 1090–1150℃ slows down the changes in microstructure and properties, indicating that its solution treatment window is sensitive to initial microstructure and batch variations.
[0003] The existing homogenization method for GH4700 ingots involves holding at 1130–1150℃ for an extended period, followed by another extended holding at 1180–1210℃, with the aim of eliminating as-cast Nb, Ti segregation, and the Laves phase. After forging, large forgings have already undergone the aforementioned smelting and billet-making process. The main challenge in their subsequent heat treatment becomes: the surface layer experiences rapid heat exchange from the furnace gas, exceeding the γ′ solidification line first and accumulating excessive grain boundary migration time, while the thermal center is limited by thermal conductivity and cannot achieve sufficient solidification for a long time; if the single high-temperature holding is extended to compensate for the core, the surface layer is prone to coarsening; if the holding time is shortened, coarse γ′ phases remain in the core. Summary of the Invention
[0004] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is: to achieve a quantifiable degree of γ′ solid solution in the thermal center of GH4700 large forgings without compensating for the thermal hysteresis of the core with long-term single-stage oversolution insulation, while limiting the oversolution exposure of the surface layer.
[0005] To achieve the above objectives, the present invention provides a homogenization process for large nickel-based superalloy forgings with γ′ precipitation strengthening, wherein the maximum effective thickness H of the forging is not less than 150 mm, comprising: S1, take samples from the same furnace to determine the total melting temperature Tγ of the γ′ phase and the initial melting temperature Tm, and set temperature measurement points near the surface and thermal center of the forging section; S2, heat the forging to 25-45℃ below Tγ and hold it until the temperature difference between the two measuring points is no greater than 15℃ and the heating rate of the hot center is no greater than 0.3℃ / min for 20 minutes. S3, alternately implement 2 to 5 cross-solution line thermal pulses, the furnace temperature of each high-temperature segment is 8 to 18°C above Tγ and at least 25°C below Tm, lasting for 10 to 36 minutes, the furnace temperature of each low-temperature segment is 5 to 20°C below Tγ and lasts until the temperature difference is no greater than 12°C; the last high-temperature segment continues for 15 to 35 minutes after the thermal center reaches 2°C above Tγ, and the cumulative time above Tγ near the surface does not exceed 120 minutes; S4. Forced air cooling is stopped when the near-surface temperature is 70-110°C below Tγ and the thermal center is 40-90°C above the near-surface temperature. The near-surface temperature is then warmed up by 5-20°C in the insulation cavity using the residual heat inside the forging, and the temperature difference is reduced to less than 15°C. Forced air cooling is then performed again to below 750°C.
[0006] In a preferred embodiment of the present invention, S1, the reference temperature Tγ for complete melting of the γ′ phase and the initial melting temperature Tm are measured by taking samples from the same furnace. A group of temperature measuring points near the surface and a group of temperature measuring points at the hot center are arranged on the forging, and the maximum measured temperature difference between the two groups of temperature measuring points is ΔT. S2, heat the forging to 25-45℃ below Tγ and hold it until ΔT is not greater than 15℃ and the heating rate of the lowest measured temperature of the hot center is not greater than 0.3℃ / min for 20 minutes. S3, alternately implement 2 to 5 cross-solution line thermal pulses, with the furnace temperature setpoint for each high-temperature segment being 8 to 18°C above Tγ, and both the setpoint and the highest measured temperature near the surface not exceeding Tm-25°C, lasting for 10 to 36 minutes; the furnace temperature setpoint for each low-temperature segment being 5 to 20°C below Tγ and lasting until ΔT is not greater than 12°C; the last high-temperature segment continues for 15 to 35 minutes after the lowest measured temperature at the thermal center reaches 2°C above Tγ, and the cumulative time for the highest measured temperature near the surface to be higher than Tγ does not exceed 120 minutes; S4, forced air cooling is stopped when the lowest measured temperature near the surface is 70 to 110°C below Tγ and the highest measured temperature at the thermal center is 40 to 90°C higher than the lowest measured temperature near the surface, and forced air cooling is stopped. The residual heat inside the forging is used in the insulation cavity to raise the lowest measured temperature near the surface by 5 to 20°C and reduce ΔT to below 15°C, and then cooled to below 750°C.
[0007] In another preferred embodiment of the present invention, the shortest distance from any point inside the forging to the outer surface that can directly exchange heat with the processing atmosphere is taken, and the maximum value of the shortest distance is dmax, and H is set to 2dmax; the mass of the forging is 500 to 3000 kg, H is 150 to 350 mm, and a process extension section that can be removed is retained at both ends of the forging axially before processing.
[0008] In another preferred embodiment of the present invention, at least three parallel samples are obtained from the near-surface layer, 1 / 4 effective thickness, and thermal center region of the extended process section, respectively; differential scanning calorimetry is initially performed at 5°C / min under argon protection, and then the parallel samples are isothermally heated for 30 min at 5°C intervals and water-quenched within 30 s after being removed from the furnace; the maximum value among the lowest processing temperatures where the residual γ′ phase area fraction of each region is less than 0.5% is determined as Tγ, and the minimum value among the extrapolated onset temperature of the first melting endothermic peak of the differential scanning calorimetry curve of each region and the metallographic initial melting temperature is determined as Tm; Tγ is 1060~1090°C, and Tm-Tγ is not less than 100°C.
[0009] In another preferred embodiment of the present invention, the near-surface temperature measuring point group includes blind hole temperature measuring points set at at least 3 high heat exchange positions, with the bottom of the hole 8-15 mm away from the surface of the forging; the thermal center temperature measuring point group extends from the axial blind hole opened in the process extension section to a position no more than 0.05H away from the thermal center of the cross section; a 1 / 4 effective thickness temperature measuring point group is added between the near-surface temperature measuring point group and the thermal center temperature measuring point group; ΔT is calculated based on the highest near-surface temperature and the lowest thermal center temperature during heating, and ΔT is calculated based on the highest thermal center temperature and the lowest near-surface temperature during cooling, and all temperature measuring holes are located within the allowance removed by subsequent machining.
[0010] In another preferred embodiment of the present invention, step S2 is carried out in a vacuum or argon circulating furnace. The furnace is loaded at a furnace temperature not higher than 300°C, and the temperature is raised to 650°C at a rate of 40-80°C / h and held at ΔT not greater than 25°C. Then, the temperature is raised to 90-110°C below Tγ at a rate of 25-45°C / h, and then raised to 25-45°C below Tγ at a rate of 8-18°C / h.
[0011] In another preferred embodiment of the present invention, the furnace temperature setting values of the high temperature section and the low temperature section in step S3 are switched at a rate of 2 to 6 °C / min; the duration τH of each high temperature section is H×(0.07 to 0.10) min / mm in millimeters; the low temperature section is not subject to forced air cooling and lasts for no less than 8 min.
[0012] In another preferred embodiment of the present invention, the controller calculates the near-surface supersolid heat dose Ds=∫max(Ts-Tγ,0)dt and the effective solid solution heat dose Dc=∫max[Tc-(Tγ-3℃),0]dt with a sampling period of no more than 5s, where Ts is the highest temperature of the near-surface temperature measurement point group during heating, Tc is the lowest temperature of the temperature measurement point group at the thermal center, and t is in minutes; Ds is integrated for each high-temperature segment and Dc is integrated over the entire process of step S3, so that Ds for each high-temperature segment is 100~450℃·min, and the sum of Ds for all high-temperature segments is 450~1500℃·min, and the last high-temperature segment ends when Dc reaches 150~450℃·min.
[0013] In another preferred embodiment of the present invention, the initial forced air cooling in step S4 uses circulating argon gas with an absolute pressure of 0.2 to 0.6 MPa, which is alternately supplied along the axial and radial directions of the forging, with a switching cycle of 60 to 180 seconds. This cools the near-surface layer at an average rate of 6 to 15°C / min within the range of Tγ to 100°C below Tγ, and ensures that the temperature difference between each near-surface temperature measurement point is no greater than 15°C. When the lowest temperature of the near-surface layer is 80 to 100°C below Tγ and the highest temperature of the thermal center is 50 to 80°C higher than the lowest temperature of the near-surface layer, the air supply is stopped.
[0014] In another preferred embodiment of the present invention, after the air supply is stopped, the external gas exchange of the insulation cavity is sealed, and the cavity wall temperature is maintained at 0-15°C below the lowest near-surface temperature when the air supply is stopped. The speed of the circulating fan is kept below 10% of the rated speed. The lowest near-surface temperature is raised by 8-18°C and ΔT is reduced to below 12°C within H×(0.10-0.25) min / mm. Forced air cooling is restarted after the temperature of all 1 / 4 effective thickness temperature measurement points is between the highest temperature of the thermal center and the lowest near-surface temperature.
[0015] In another preferred embodiment of the present invention, after restarting the forced air cooling, the average cooling rate of the highest temperature of the thermal center from 120°C below Tγ to 820°C is 3-8°C / min, and the difference in the average cooling rate of the near-surface layer, 1 / 4 effective thickness and adjacent temperature measuring layers in the thermal center is not greater than 2.5°C / min; a stop-cooling trigger temperature within 790-810°C is selected, and forced air cooling is paused when any temperature measuring point cools to the stop-cooling trigger temperature. Timing is started after all temperature measuring points reach 800±10°C and ΔT is not greater than 8°C, and the temperature is maintained for 14-18 hours. Then, the temperature is cooled to 650°C at a rate of 20-40°C / h and then air-cooled to below 100°C.
[0016] Compared with the prior art, the present invention has the following beneficial effects: By using the Tγ / Tm calibration of the three layers in the same furnace, the phase boundary drift caused by composition and initial structure is explicitly introduced into the control, which reduces the core undersolution caused by low reference temperature and prevents the narrowing of the initial melting safety window caused by high reference temperature.
[0017] The small thermal pulse across the solid solution line follows the sequence of "short-term high temperature to obtain dissolution driving force - low temperature segment to limit the continuous migration of surface grain boundaries and wait for the redistribution of heat in the core - restart after ΔT reaches the target", so that the increase of thermal center dose and surface overheating time no longer need to increase synchronously; Ds / Dc further transforms this mechanism into a recordable and reproducible process quantity.
[0018] After the initial forced air cooling creates a temperature field with a high core and a low surface temperature, the temperature difference is not immediately amplified. Instead, cooling is stopped based on both the absolute surface temperature and the core-surface temperature difference. The surface is then warmed up using internal sensible heat within a low-heat-loss insulation cavity. This process reduces the time difference between different layers passing through the γ′ precipitation sensitive zone and lowers the peak tensile stress generated by rapid cooling. Attached Figure Description
[0019] Figure 1 This is a metallographic micrograph of the corrosion structure of the radial section of the near-surface region of the forging after homogenization treatment and aging, as shown in Embodiment 2 of the present invention.
[0020] Figure 2 The image shows the corrosion metallographic microstructure of a radial section of a quarter-thickness effective thickness region of a forging after homogenization treatment and aging, as described in Embodiment 2 of the present invention.
[0021] Figure 3 This is a metallographic micrograph of the corrosion metallographic structure of the radial section of the hot center region of the forging after homogenization treatment and aging in Embodiment 2 of the present invention.
[0022] Figure 4 This is the EBSD inverse pole figure orientation diagram of the near-surface region of the forging after homogenization treatment and aging in Embodiment 2 of the present invention.
[0023] Figure 5 This is the EBSD inverse pole figure orientation diagram of the hot center region of the forging after homogenization treatment and aging in Embodiment 2 of the present invention. Detailed Implementation
[0024] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that, unless otherwise specified, the following embodiments and features described therein can be combined with each other.
[0025] Some exemplary embodiments of the invention have been described for illustrative purposes. It should be understood that the invention may be implemented in other ways not specifically shown in the accompanying drawings.
[0026] refer to Figures 1-5 This invention provides a homogenization process for large nickel-based superalloy forgings with γ′ precipitation strengthening.
[0027] The following embodiments use a vacuum / argon heat treatment furnace with an adjustable-speed circulating fan and zoned flow control valves. Furnace temperatures refer to the set values of the thermocouples controlling the effective heating zone of the charge; forging temperatures refer to the measured values of the armored thermocouples embedded in the blind holes of the machining allowance. The effective heating zone of the heat treatment furnace was confirmed according to GB / T 9452—2023 before the test. All thermocouples were calibrated in the same batch before use, with a sampling period of 5 seconds. Temperature records, valve status, fan speed, and furnace pressure were recorded using the same clock.
[0028] The high heat transfer locations near the surface are determined by empty furnace flow field testing and pre-loading temperature mapping, including at least the windward side, leeward side, and geometric corner / thin edge locations. The bottom of the temperature measuring hole is 8–15 mm from the final removed surface; the core blind hole is machined along the axis by an extended section, with the bottom of the hole no more than 0.05H from the geometric thermal center. Thermocouples are in metal contact with the bottom of the hole and electrically isolated by a high-purity alumina sleeve, and the orifice is sealed with a heat-resistant fiber plug.
[0029] In this embodiment, the "high-temperature segment duration" is timed from the start of the furnace temperature setpoint to the switch to the high-temperature target, and the "low-temperature segment duration" is timed from the start of the switch to the low-temperature target. Ds and Dc are calculated from adjacent sampling points using the trapezoidal integral method. If the dose is close to the upper limit but the core has not yet reached the endpoint, the controller does not increase the temperature, but ends the pulse, performs low-temperature homogenization, and then enters the next pulse; if the core endpoint is still not met by the fifth pulse, the component is judged as having a process abnormality and is not compensated by extending the surface overheating time.
[0030] The chemical compositions described below are by mass percentage. All embodiments used GH4700 forgings that underwent vacuum induction melting followed by vacuum arc remelting, ingot diffusion homogenization, and forging.
[0031] Example 1 The GH4700 disc forging from heat A was selected, with the following chemical composition: C 0.048%, Cr 24.82%, Co 19.75%, Nb 1.60%, Al 1.43%, Ti 1.66%, Si 0.08%, Mn 0.05%, Fe 0.55%, B 0.005%, Zr 0.028%, S 0.002%, P 0.004%, balance Ni. The forging contains two axially removable extension sections, with a processed weight of 500 kg and a maximum effective thickness H = 150 mm. Three parallel samples were obtained using the aforementioned method, yielding a temperature gradient (Tγ) of 1060℃ and a temperature gradient (Tm) of 1258℃.
[0032] Temperature measuring holes with a bottom distance of 8 mm from the surface are installed at three near-surface high heat exchange hotspots, and temperature measuring holes are installed at two points representing 1 / 4 of the effective thickness. Two core blind holes with a bottom distance of 0.05H from the thermal center of the cross-section are machined using an extended process section. The furnace is loaded at 250℃, heated to 650℃ at a rate of 40℃ / h and held until ΔT = 22℃. Then, it is heated to 950℃ (110℃ below Tγ) at a rate of 25℃ / h, and then to 1035℃ (25℃ below Tγ) at a rate of 8℃ / h. It is held at 1035℃ until ΔT = 13℃ and the core minimum temperature rise rate is 0.22℃ / min for 20 consecutive minutes.
[0033] Two thermal pulses were implemented. The first high-temperature phase switched at 2°C / min to 1068°C (8°C above Tγ), lasting 10 minutes; then switched to 1055°C (5°C below Tγ) without forced air cooling, lasting 22 minutes until ΔT=10°C. The second high-temperature phase remained at 1068°C. The core minimum temperature reached 1062°C 11 minutes after entering this phase, continuing for another 15 minutes, for a total duration of 26 minutes. The near-surface temperature was cumulatively above Tγ for 34 minutes, while both furnace temperature and the highest near-surface temperature were below Tm-25°C.
[0034] Immediately, argon gas was circulated for forced cooling at an absolute pressure of 0.2 MPa, switching between axial and radial cooling every 60 seconds. The average cooling rate of the near-surface layer from Tγ to 100°C below Tγ was 6.0°C / min, with a maximum temperature difference of 11°C between surface points. When the lowest near-surface temperature reached 980°C (80°C below Tγ) and the highest core temperature reached 1030°C (50°C above Tγ), the ventilation was stopped and external ventilation was sealed. The cavity wall temperature was maintained at 980°C, and the fan stopped. After 15 minutes, the lowest near-surface temperature rose by 8°C to 988°C, and the highest core temperature reached 999°C, with ΔT = 11°C, and the point at 1 / 4 thickness falling between the two.
[0035] The air cooling system was restarted, resulting in an average cooling rate of 3.0℃ / min for the core to drop from 940℃ to 820℃, with a maximum cooling rate difference of 1.4℃ / min between adjacent layers. 810℃ was selected as the trigger temperature for stopping cooling. Air cooling was paused when any surface point reached 810℃. After all measuring points reached 800±10℃ and ΔT=8℃, the system was held at 800℃ for 14 hours, then furnace-cooled at 20℃ / h to 650℃, and finally air-cooled to below 100℃. The extended section was removed, and samples were taken according to the testing plan.
[0036] Example 2 Solid disc forgings from heat B of GH4700 were selected. The chemical composition was: C 0.052%, Cr 25.05%, Co 20.10%, Nb 1.66%, Al 1.48%, Ti 1.70%, Si 0.07%, Mn 0.06%, Fe 0.48%, B 0.004%, Zr 0.025%, S 0.002%, P 0.004%, with the balance being Ni. The forging had a processed weight of 1500 kg, a maximum effective thickness H = 220 mm, and extended sections on both axial end faces. Three parallel samples from each of the three layers were used to obtain a temperature gradient (Tγ) of 1075℃ and a temperature gradient (Tm) of 1265℃.
[0037] Temperature measuring holes with a bottom distance of 12 mm from the surface are installed at four near-surface high heat exchange hotspots, and temperature measuring holes are installed at four points representing 1 / 4 of the effective thickness. Two core blind holes are machined with a bottom distance of 0.03H from the thermal center of the cross-section. The furnace is loaded at 200℃, heated to 650℃ at a rate of 60℃ / h and held until ΔT=18℃, then heated to 975℃ (100℃ below Tγ) at a rate of 35℃ / h, and then heated to 1040℃ (35℃ below Tγ) at a rate of 13℃ / h. The temperature is held until ΔT=10℃, and the core minimum temperature is continuously increased at a rate of 0.18℃ / min for 20 minutes.
[0038] Three thermal pulses were implemented. The high-temperature pulses were all set at 1088℃ (13℃ above Tγ), with a switching rate of 4℃ / min. The high-temperature pulses lasted for 18 min, 20 min, and 22 min, respectively. The two low-temperature pulses were set at 1063℃ (12℃ below Tγ), with no forced air cooling, lasting for 34 min and 37 min, respectively, with endpoint ΔT values of 11℃ and 9℃. The core minimum temperature reached 1077℃ 4 min after the start of the third high-temperature pulse, and continued for another 18 min. The Ds for the three high-temperature pulses were 180℃·min, 220℃·min, and 260℃·min, respectively, with a total Ds of 660℃·min. The total Dc for the entire S3 process was 300℃·min. The cumulative temperature above Tγ in the near-surface layer was 52 min.
[0039] Argon gas was circulated at an absolute pressure of 0.4 MPa for cooling, switching between axial and radial cooling every 120 seconds. The average cooling rate near the surface was 10.5 °C / min between Tγ and 100 °C below Tγ, with a maximum temperature difference of 9 °C between surface points. Airflow was stopped when the lowest near-surface temperature reached 985 °C (90 °C below Tγ) and the highest core temperature reached 1050 °C (65 °C above Tγ). The insulation chamber was sealed, with the chamber wall temperature at 978 °C (7 °C lower), and the fan speed at 5% of the rated value. After 37.4 min (H × 0.17 min / mm), the lowest surface temperature rose by 13 °C to 998 °C, and the highest core temperature reached 1007 °C, with ΔT = 9 °C. All points at 1 / 4 of the thickness were located between 998 and 1007 °C.
[0040] A second air cooling process was used to reduce the core temperature from 955℃ to 820℃ at an average rate of 5.5℃ / min, with a maximum temperature difference of 1.8℃ / min between adjacent layers. 800℃ was selected as the shutdown trigger temperature. Air cooling was stopped when any surface point reached 800℃. Once all measuring points reached 800±10℃ and ΔT=6℃, the temperature was held at 800℃ for 16 hours, followed by furnace cooling at 30℃ / h to 650℃. The furnace was then air-cooled to below 100℃. The extended process section was removed and samples were taken.
[0041] Example 3 Large disc forgings from heat C of GH4700 were selected. Their chemical composition was: C 0.055%, Cr 25.22%, Co 20.25%, Nb 1.71%, Al 1.53%, Ti 1.75%, Si 0.08%, Mn 0.05%, Fe 0.42%, B 0.005%, Zr 0.030%, S 0.002%, P 0.004%, with the balance being Ni. The forging had a processed weight of 3000 kg, a maximum effective thickness H = 350 mm, and extended sections retained at both axial ends. Four parallel samples from each of the three layers were used to obtain a temperature gradient (Tγ) of 1090℃ and a temperature gradient (Tm) of 1270℃.
[0042] Temperature measuring holes with a bottom distance of 15 mm from the surface are installed at six near-surface high heat exchange hotspots, and temperature measuring holes are installed at four points representing 1 / 4 of the effective thickness. Three core blind holes are machined with a bottom distance of no more than 0.01H from the thermal center of the cross-section. The furnace is loaded at 300℃, heated to 650℃ at a rate of 80℃ / h and held until ΔT = 25℃. The temperature is then increased to 1000℃ (90℃ below Tγ) at a rate of 45℃ / h, and further increased to 1045℃ (45℃ below Tγ) at a rate of 18℃ / h. Holding is continued until ΔT = 15℃ and the core minimum temperature rise rate is 0.30℃ / min for 20 consecutive minutes.
[0043] Five thermal pulses were applied at a rate of 6℃ / min. The high-temperature pulses were set sequentially to 1098℃, 1100℃, 1102℃, 1105℃, and 1108℃, which correspond to 8℃, 10℃, 12℃, 15℃, and 18℃ above Tγ, respectively, with each pulse lasting 35 minutes. The low-temperature pulses were all set to 1070℃, which is 20℃ below Tγ. These pulses were applied without forced air cooling and lasted for 74 minutes, 69 minutes, 63 minutes, and 58 minutes, respectively, ending with a ΔT of no more than 12℃. The temperature dips (Ds) for each high-temperature pulse were 100, 250, 300, 400, and 450℃·min, respectively, for a total Ds of 1500℃·min. The residual heat from the core during the first four pulses caused the core temperature to reach a minimum of 1092℃ at the start of the final high-temperature pulse. The final pulse lasted for 35 minutes, resulting in a total temperature dip (Dc) of 450℃·min for the entire S3 process. The cumulative temperature near the surface was 110 minutes above Tγ.
[0044] Forced cooling with circulating argon gas at an absolute pressure of 0.6 MPa was employed, switching between axial and radial flow paths every 180 seconds. The average cooling rate near the surface (Tγ to 100°C below Tγ) was 15.0°C / min, with a maximum temperature difference of 15°C between surface points. Airflow was stopped when the lowest near-surface temperature reached 990°C (100°C below Tγ) and the highest core temperature reached 1070°C (80°C above Tγ). The insulation cavity wall was maintained at 975°C (15°C below Tγ), with the fan operating at 10% of its rated speed. After 87.5 minutes (H×0.25 min / mm), the lowest near-surface temperature rose by 18°C to 1008°C, and the highest core temperature reached 1020°C, with a ΔT of 12°C. All points within the 1 / 4 thickness range fell within this range.
[0045] Re-air cooling was applied, reducing the core temperature from 970℃ to 820℃ at an average rate of 8.0℃ / min, with a maximum temperature difference of 2.5℃ / min between adjacent layers. 790℃ was selected as the trigger temperature for stopping cooling. Cooling was paused when any measuring point reached 790℃. After all measuring points reached 800±10℃ and ΔT=8℃, the temperature was held at 800℃ for 18 hours, then furnace cooled to 650℃ at a rate of 40℃ / h, and finally air-cooled to below 100℃. The extended section was then cut off and samples were taken.
[0046] Example 4 A GH4700 disc forging from heat D was selected. Its chemical composition was: C 0.049%, Cr 24.90%, Co 19.88%, Nb 1.62%, Al 1.45%, Ti 1.67%, Si 0.07%, Mn 0.05%, Fe 0.52%, B 0.004%, Zr 0.026%, S 0.002%, P 0.004%, with the balance being Ni. The processed mass was 800 kg, H = 180 mm, with an axially extended section. Three parallel samples were used, and the temperatures were measured to be Tγ = 1064℃ and Tm = 1260℃.
[0047] Three near-surface measuring points, two 1 / 4-thickness measuring points, and two core measuring points were arranged. The furnace was loaded at 220℃, and the temperature was increased to 650℃ at a rate of 50℃ / h and then uniformly heated. The temperature was then increased to 964℃ at a rate of 30℃ / h, and then increased to 1039℃ (25℃ below Tγ) at a rate of 10℃ / h. The temperature was held until ΔT=15℃, and the minimum core temperature was maintained for 20 minutes with a continuous heating rate of 0.25℃ / min.
[0048] Two high-temperature pulses were implemented, each set at 1072℃ (8℃ above Tγ). The first high-temperature pulse lasted 10 minutes. The low-temperature pulse was set at 1059℃ (5℃ below Tγ), maintained for 28 minutes without forced air cooling until ΔT = 12℃. In the second high-temperature pulse, the core reached 1066℃ after 5 minutes and continued for another 25 minutes, for a total duration of 30 minutes. The near-surface layer accumulated temperatures above Tγ for 42 minutes, with the highest temperature below Tm-25℃.
[0049] Forced gas cooling was initially performed using 0.25 MPa argon gas, switching between axial and radial cooling every 90 seconds, with an average cooling rate of 7.0 °C / min near the surface. Cooling was stopped when the lowest near-surface temperature reached 994 °C (70 °C below Tγ) and the highest core temperature reached 1034 °C (40 °C above Tγ). The cavity wall temperature was maintained at 994 °C, and the fan stopped. After 35 minutes, the lowest surface temperature rose by 5 °C to 999 °C, and the highest core temperature reached 1014 °C (ΔT = 15 °C). Gas cooling was then restarted, controlling the core temperature to drop from 944 °C to 820 °C at an average cooling rate of 4.0 °C / min. The temperature was homogenized around 800 °C to ΔT = 8 °C, held at 800 °C for 15 hours, cooled to 650 °C at a rate of 25 °C / h, and then air-cooled to below 100 °C. The extended section was then removed and samples were taken.
[0050] Example 5 The GH4700 disc forging from heat E was selected, with the following chemical composition: C 0.054%, Cr 25.18%, Co 20.20%, Nb 1.70%, Al 1.52%, Ti 1.74%, Si 0.08%, Mn 0.06%, Fe 0.45%, B 0.005%, Zr 0.029%, S 0.002%, P 0.004%, balance Ni; processed weight 2500 kg, H=320 mm, with axial extension section. The temperature (Tγ) and temperature (Tm) of the three parallel samples were measured to be 1087℃ and 1268℃, respectively.
[0051] Five near-surface measuring points, four quarter-thickness measuring points, and three core measuring points were arranged. The furnace was loaded at 280℃, heated to 650℃ at a rate of 75℃ / h and then homogenized, then heated to 997℃ at a rate of 42℃ / h, and then heated to 1042℃ (45℃ below Tγ) at a rate of 17℃ / h; the temperature was held to ΔT=14℃ with the core continuously heated at a rate of 0.28℃ / min for 20 minutes.
[0052] Five cross-line pulses were implemented. The high-temperature pulses were all set at 1105℃, which is 18℃ above Tγ. The first four pulses lasted for 34, 35, 35, and 35 minutes respectively, and the fifth pulse lasted for 36 minutes. The low-temperature pulses were set at 1067℃, which is 20℃ below Tγ. No forced air cooling was used, and the pulses were maintained until ΔT reached 12, 11, 10, and 9℃ respectively. At the beginning of the fifth pulse, the lowest core temperature remained at 1089℃ due to the thermal inertia of the previous low-temperature pulse, and the pulses continued for 35 minutes before ending. The cumulative temperature above Tγ in the near-surface layer was exactly 120 minutes, and all measured temperatures were below Tm-25℃.
[0053] Forced gas cooling with 0.55 MPa argon was used, switching between axial and radial cooling every 160 seconds, with an average cooling rate of 14℃ / min near the surface. Ventilation was stopped when the lowest near-surface temperature reached 977℃ (110℃ below Tγ) and the highest core temperature reached 1067℃ (90℃ above Tγ). The cavity wall was maintained at 970℃, and the fan operated at 6% of its rated speed. After 95 minutes, the lowest surface temperature rose by 20℃ to 997℃, and the highest core temperature reached 1012℃ (ΔT=15℃). Gas cooling was then initiated again, with the core cooling from 967℃ to 820℃ at an average rate of 7℃ / min. At 800±10℃ and ΔT=8℃, all points were held at 800℃ for 17 hours, then cooled at 38℃ / h to 650℃, followed by air cooling to below 100℃. The extended section was then removed and samples were taken.
[0054] Example 6 The GH4700 disc forging from heat F was selected, with the following chemical composition: C 0.051%, Cr 24.98%, Co 20.02%, Nb 1.64%, Al 1.46%, Ti 1.69%, Si 0.07%, Mn 0.05%, Fe 0.50%, B 0.004%, Zr 0.027%, S 0.002%, P 0.004%, balance Ni; processed weight 1100 kg, H=200 mm, with process extension section. The temperature Tγ of the three parallel samples was measured to be 1070℃ and Tm=1262℃.
[0055] Four near-surface measuring points, three 1 / 4-thickness measuring points, and two core measuring points were arranged. The furnace was loaded at 240℃, and the temperature was increased to 650℃ at a rate of 55℃ / h and then uniformly heated. The temperature was then increased to 970℃ at a rate of 32℃ / h, and then increased to 1035℃ (35℃ below Tγ) at a rate of 12℃ / h. The temperature was held until ΔT=11℃ and the minimum core temperature was maintained for 20 minutes at a continuous heating rate of 0.20℃ / min.
[0056] Three thermal pulses were implemented at a switching rate of 3℃ / min. The high-temperature settings were 1080℃, 1082℃, and 1084℃, lasting for 14 min, 17 min, and 20 min respectively, corresponding to τH coefficients of 0.07, 0.085, and 0.10 min / mm. The low-temperature setting was 1060℃, 10℃ below Tγ, without forced air cooling and continued until ΔT was no greater than 10℃. The Ds for the three high-temperature segments were 100, 150, and 200℃·min, respectively, with a total Ds of 450℃·min. In the final segment, the core reached 1072℃ after 5 min and continued for 15 min. The Dc for the entire S3 process was 150℃·min, and the cumulative temperature near the surface was higher than Tγ for 50 min.
[0057] Forced argon cooling at 0.3 MPa was used, switching between axial and radial cooling every 90 seconds, with an average cooling rate of 8°C / min near the surface. Cooling was stopped when the lowest near-surface temperature was 985°C (85°C below Tγ) and the highest core temperature was 1040°C (55°C above Tγ). The cavity wall was 4°C below the surface, and the fan operated at 3% of its rated speed. After 24 minutes (H×0.12 min / mm), the surface temperature rose by 9°C, ΔT=11°C, with all 1 / 4 thickness points located between the core and the surface. Cooling was then restarted, resulting in an average cooling rate of 4.5°C / min from 950°C to 820°C in the core, with a temperature difference of 1.6°C / min between adjacent layers. At 800±10°C and ΔT=7°C, the core was held at 800°C for 15 hours, then cooled to 650°C at 25°C / h, followed by air cooling to below 100°C. The extended section was then removed and samples were taken.
[0058] Unless otherwise stated, the following comparative examples are the same as those in Example 2.
[0059] Comparative Example 1 The difference is that only the three cross-line high-temperature sections and two low-temperature sections in Example 2 are changed to a single-section continuous heat preservation at 1088℃, and the process ends when the total Ds near the surface reaches 660℃·min; the initial air cooling, cooling stop and recovery, and aging are exactly the same.
[0060] Comparative Example 2 The difference is that the S1 to S3 and the initial argon parameters of Example 2 are fully retained, but when the surface reaches 985°C and the core is 65°C higher, the air is not stopped and forced air cooling continues until any measuring point reaches 790 to 810°C, and then the temperature is evenly aging according to Example 2.
[0061] Comparative Example 3 The difference is that the furnace temperature setting value of the three high-temperature sections in Example 2 is changed from Tγ+13℃ to Tγ+25℃, while the number of sections, duration, low-temperature section, air cooling, temperature recovery and aging remain unchanged.
[0062] Comparative Example 4 The difference is that the two low-temperature segments in Example 2 are both fixed at 8 minutes, and the waiting time for ΔT to be no greater than 12°C is no longer required; the high and low temperature settings, pulse duration, air cooling, temperature recovery and aging time remain unchanged.
[0063] Comparative Example 5 The difference is that the segmented heating path is the same as in Example 2, but when the near-surface layer reaches 1040°C, it immediately enters S3 without waiting for ΔT to be no greater than 15°C and the core heating rate to be no greater than 0.3°C / min; the rest of the pulse, air cooling, reheating and aging remain unchanged.
[0064] Comparative Example 6 The difference is that the forging from heat B is still used, but the measured Tγ=1075℃ of that heat is not used. Instead, a fixed nominal value of 1060℃ is used as the basis for all relative temperature and dosage calculations. All relative offsets, times, gas cooling triggers and aging rules are the same as in Example 2.
[0065] Test methods Furnace temperature and process temperature. The effective heating zone of the heat treatment furnace is confirmed according to GB / T 9452—2023. Data is collected synchronously at each measuring point with a 5-second cycle. ΔT is the difference between the measured values of the most unfavorable surface layer and the core at the corresponding stage; Ds and Dc are calculated using trapezoidal integrals. The "passage time difference" is calculated based on the moment when the temperature of each layer decreases through Tγ-175℃, and the difference between the latest and earliest times is taken.
[0066] Surface cracks. Before removing the extended section, fluorescent penetrant testing was performed on the accessible outer surface of the forging according to GB / T 18851.1—2024, and the results were evaluated according to the observation conditions specified in GB / T 5097—2020. The number and location of relevant linear indicators with a length of not less than 1 mm were recorded; the same penetrant material, cleaning time, and development time were used for all groups.
[0067] Metallographic structure and grain size. Samples were taken from near the surface (10–15 mm from the treated surface), 1 / 4 of the effective thickness, and the thermal center. Sample preparation, polishing, and etching were performed according to GB / T 13298—2015. The average grain size was determined according to the cross-sectional method of GB / T 6394—2017. At least 15 fields of view were randomly selected for each layer, and the total number of cross-sectional grain boundary intersections was not less than 500. The average value and the minimum value of the three layers were reported, and the area fraction of abnormal coarse grains was statistically analyzed for regions where the area of the largest grain was greater than 4 times the area of the median grain in that layer.
[0068] Quantitative analysis of the γ′ phase. Evaluation samples after solution treatment were taken from the furnace witness block in the extended process section and immediately rapidly cooled with inert gas; samples in the final aged state were taken from three layers. Microstructure was analyzed according to GB / T 13298—2015, and area fraction statistics were performed according to GB / T 15749—2008. The same field emission scanning electron microscope, accelerating voltage, and threshold algorithm were used, with no fewer than 20 fields of view per layer. The area fraction of residual coarse γ′ particles with an equivalent diameter greater than 0.5 μm was statistically analyzed in the solution-treated state; the equivalent circular diameter of no fewer than 1000 γ′ particles was statistically analyzed in the aged state, and the span of the average diameter across the three layers was reported.
[0069] Vickers hardness. The HV10 test was conducted according to GB / T 4340.1—2024. Ten effective indentations were taken from the near-surface layer, one-quarter of the effective thickness, and the core. The center-to-center distance and distance from the boundary of the indentations met the standards. After removing the maximum and minimum values, the average of the eight points was taken. The maximum difference between the average values of the three layers was taken as the hardness span.
[0070] Residual stress. Near-surface residual stress in the original forging was determined using X-ray diffraction sin²ψ method according to GB / T 7704—2017 and Amendment No. 1. To avoid introducing additional stress through mechanical grinding, an oxide layer not exceeding 30 μm was uniformly removed by electrolysis. Using diffraction planes suitable for the γ-matrix and calibrated diffraction elastic constants, three points were measured in both the axial and radial directions, and the maximum tensile stress was reported. This method reflects near-surface stress and does not treat the core value after destructive cutting as the original core residual stress.
[0071] Tensile properties. Three proportional specimens were prepared along the main forging direction at the near-surface layer, 1 / 4 effective thickness, and hot spot. Room temperature tensile testing was performed according to GB / T 228.1—2021, and high-temperature tensile testing was performed at 700℃ according to GB / T 228.2—2015. Rp0.2, Rm, and A were determined, and the arithmetic mean of the three specimens is given in Table 4; individual values and standard deviations were also retained. The difference in cross-sectional properties was expressed as the maximum value minus the minimum value among the three layer averages, without mixing samples from different directions in the same statistic.
[0072] Table 1 Process Control Results Note: Values marked with "*" are re-evaluated based on the actual measured Tγ=1075℃ of furnace B; Although Comparative Example 6 was controlled at a fixed nominal Tγ=1060℃, the effective solution time and Dc were significantly insufficient when calculated based on the actual phase boundary.
[0073] Table 2. Grain and γ′ phase results Table 3 Hardness and Near-Surface Residual Stress Table 4 Tensile Properties In Examples 1-6, the maximum surface-core temperature difference during the high-temperature thermal pulse phase was controlled at 10-15 °C. After the initial forced air cooling and subsequent recovery from residual heat after cooling was stopped, the maximum surface-core temperature difference further converged to 9-15 °C, and the time difference between different layers passing through Tγ-175 °C was only 4-10 min. In Comparative Example 2, where the recovery from residual heat after cooling was stopped was eliminated, the maximum surface-core temperature difference reached 118 °C during the initial cooling process and remained at 70 °C after cooling was stopped. The time difference between different layers passing through the aforementioned temperature range was extended to 23 min. These results demonstrate that using surface temperature and surface-core temperature difference as dual trigger conditions to stop forced air cooling, and utilizing residual heat from the thermal center to implement self-warming of the near-surface layer, can suppress excessively rapid cooling of the surface layer of large forgings, allowing different layers to pass through the sensitive temperature range for γ′ phase precipitation more synchronously.
[0074] Example 2 and Comparative Example 1 used the same heat batch, forging size, cumulative near-surface solution heat dose Ds, and subsequent cooling and aging regimes. The only difference was that Comparative Example 1 replaced the three thermal pulses spanning the γ′ phase complete solution reference temperature with a single continuous high-temperature treatment. In Example 2, the effective solution heat dose Dc at the thermal center increased from 210 ℃·min in Comparative Example 1 to 300 ℃·min, while the grain size span decreased from 31 μm to 3 μm, the area fraction of abnormal coarse grains decreased from 6.5% to 0.2%, and the maximum area fraction of residual coarse γ′ phase after solution treatment decreased from 1.8% to 0.3%. This indicates that distributing the high-temperature heat into multiple small-amplitude, cross-line thermal pulses can utilize the low-temperature homogenization phase between adjacent high-temperature sections to promote the continued transfer of heat to the thermal center, improving the effective solution degree at the thermal center without increasing the total near-surface heat load, and avoiding excessive grain growth on the surface caused by a single continuous solution treatment.
[0075] The residual heat recovery after cooling significantly improved the uniformity of the γ′ phase and its mechanical properties after aging. In Example 2, the average diameter of the γ′ phase after aging varied from 74 nm near the surface and 77 nm at 1 / 4 thickness to 80 nm at the thermal center, with an interlayer span of only 6 nm. In Comparative Example 2, where residual heat recovery was not performed, the average diameters were 55 nm, 82 nm, and 112 nm, respectively, with the span increasing to 57 nm. Correspondingly, Example 2 had an HV10 hardness span of 6 and a maximum residual tensile stress near the surface of 68 MPa, while Comparative Example 2 had a hardness span and a maximum residual tensile stress near the surface that increased to 45 and 238 MPa, respectively.
[0076] In Example 2, the difference between the core and surface yield strength at room temperature was 10 MPa, and the difference between the core and surface yield strength at 700 °C was 12 MPa; in Comparative Example 2, the differences were 170 MPa and 190 MPa, respectively. This comparison demonstrates that the residual heat recovery after cooling redistributes the internal heat of the forging, making the nucleation, growth, and subsequent aging response of the γ′ phase on the core and surface more consistent, thereby simultaneously reducing the hardness gradient, strength gradient, and near-surface residual tensile stress.
[0077] The upper limit of the high-temperature thermal pulse and the control of the thermal dose play an important role in preventing near-surface overheating. Example 3, located in the upper region of the high-temperature parameters of this invention, has average grain sizes of 58 μm, 54 μm, and 51 μm at the surface, 1 / 4 thickness, and thermal center, respectively, with a grain span of 7 μm, an abnormal coarse grain area fraction of 0.5%, and no linear defects detected. Comparative Example 3, by simply increasing the high-temperature bias to Tγ+25 ℃, saw its near-surface average grain size increase to 94 μm, grain span expand to 44 μm, abnormal coarse grain area fraction increase to 9.2%, and one linear indication detected. These results demonstrate that limiting the upper limit of the thermal pulse to within Tγ+18 ℃, while simultaneously ensuring that the furnace temperature setpoint and the highest measured near-surface temperature do not exceed Tm-25 ℃, can achieve effective solid solution of the γ′ phase while reducing the risk of abnormal coarsening, grain boundary weakening, and localized initial melting in the near-surface.
[0078] The core-surface temperature difference as the termination criterion in the low-temperature homogenization phase has an independent function. In Comparative Example 4, simply changing the low-temperature phase to a fixed 8-minute holding time, the maximum core-surface temperature difference at the start of the next high-temperature phase increased from 10 °C in Example 2 to 28 °C, with the grain size span and γ′ phase diameter span increasing to 30 μm and 34 nm, respectively. In Comparative Example 5, after removing the dual entry criteria of core-surface temperature difference and thermal center heating rate in the subsolution homogenization phase, the maximum core-surface temperature difference at the start of the first high-temperature phase reached 46 °C, the maximum area fraction of the residual coarse γ′ phase after solution treatment increased to 3.0%, and the grain size span increased to 35 μm. A fixed holding time is difficult to adapt to large forgings with different masses, thicknesses, and furnace loading conditions. The core-surface temperature difference criterion is used to ensure uniformity of the spatial temperature field, while the thermal center heating rate criterion is used to confirm that the thermal center is close to thermal equilibrium; the two cannot be simply substituted for each other.
[0079] Calibrating Tγ and Tm within the same heat batch can avoid control benchmark deviations caused by material batch fluctuations. Comparative Example 6 uses a fixed nominal temperature 15 °C lower than the measured Tγ of Heat B for control. Although the control system judged the forging to have undergone solution treatment based on the nominal temperature, after recalculation according to the actual Tγ of this heat batch, the effective solution heat dose Dc at the hot center was only 35 °C·min. The maximum area fraction of the residual coarse γ′ phase after solution treatment reached 4.8%, and the diameter span of the γ′ phase after aging was 25 nm, with a hardness span of 23. Its room temperature yield strength was only 760 MPa for the surface layer and 700 MPa for the hot center, lower than 850 MPa and 840 MPa in Example 2. These results demonstrate that calibrating Tγ and Tm within the same heat batch is the process basis for ensuring the accuracy of thermal pulse temperature, effective solution heat dose, and initial melt safety margin.
[0080] As can be seen from Examples 1-6, the grain size range of the obtained forgings is controlled between 3 and 10 μm, the area fraction of abnormal coarse grains is 0.2% to 0.8%, the maximum area fraction of residual coarse γ′ phase after solution treatment is 0.3% to 0.5%, the diameter range of γ′ phase after aging is 5 to 12 nm, the HV10 hardness range is 6 to 10, and the maximum residual tensile stress near the surface is 62 to 88 MPa, with no linear defects detected. While maintaining high strength at room temperature and 700 °C, the strength difference between the surface layer and the thermal center in each example is small, indicating that the present invention achieves synergistic homogenization of microstructure, precipitation strengthening state, residual stress, and load-bearing capacity.
[0081] Depend on Figure 1 As can be seen, the near-surface region is mainly composed of nearly equiaxed grains with relatively uniform size. The grain boundaries are continuous and have clear outlines. Annealing twins are visible inside some grains, and no abnormal coarse grain bands are formed that are continuously distributed along the surface of the forging. The near-surface region of large forgings heats up rapidly and usually withstands high instantaneous temperatures and cumulative high-temperature heat, making it the most susceptible location for grain boundary migration and abnormal grain growth. Figure 1 The near-surface layer still maintains a uniform grain structure, proving that the present invention avoids significant coarsening of the near-surface layer due to prolonged overheating by limiting the surface heat dose and controlling the thermal pulse termination across the γ′ solid solution temperature.
[0082] Depend on Figure 2 As can be seen, the grains in this region are also predominantly of near-equiaxed morphology, with continuous grain boundary distribution. No obvious alternating zones of coarse and fine grains or local mixed-grain structures are observed between different fields of view. The quarter-thickness region is located between the surface fast-response zone and the thermal center hysteresis zone, reflecting whether a significant microstructure transition gradient is formed during the heat transfer process into the forging.
[0083] Depend on Figure 3 It is evident that the grain boundaries in the hot center region are fully exposed, and the grains are mainly in a near-equiaxed morphology, with no large-area residual elongated deformed grains, continuous mixed grain regions, or abnormally large grain aggregation areas observed. The hot center is the region with the most sluggish temperature response during the heating process and the slowest cooling process for large forgings, and it is also the location where insufficient heat penetration and incomplete microstructure transformation are most likely to occur during conventional homogenization treatment. Figure 3 The thermal center tissue shown is close to the near-surface tissue, proving that the present invention utilizes the control of the thermal dose in the core and the self-reheating process after the heating is stopped to enable the thermal center to obtain a sufficient but not excessive effective high temperature effect.
[0084] Depend on Figure 4As can be seen, different orientations and colors are dispersed within the scanning area, without forming a large area of single color bands that span the field of view; the color within a single grain is generally uniform, and non-Σ3 high-angle grain boundaries form a continuous network, with locally visible Σ3 annealed twin bands defined by paired white boundaries. These results demonstrate that no obvious single strong preferred orientation is formed in the near-surface region, nor are there any orientation clusters composed of a few abnormally large grains with the same orientation.
[0085] Depend on Figure 5 It is evident that the thermal center region is also composed of nearly equiaxed, oriented, and dispersed grains, with different colored grains interspersed and no continuous oriented bands of the same color appearing; non-Σ3 high-angle grain boundaries are continuously distributed, and a small number of Σ3 annealed twins are distributed in narrow strips. This indicates that the thermal center did not develop an abnormal growth structure where a few oriented grains preferentially engulf surrounding grains due to prolonged high-temperature retention.
[0086] This invention sequentially couples together simultaneous furnace temperature calibration, subsolution dual-criteria temperature equalization, cross-γ′ solution line thermal dose pulses, dual-trigger shutdown and residual heat recovery, and layered rate-limited cooling and aging. Near-surface oversolution thermal dose Ds is used to suppress surface overheating and abnormal grain growth, while the effective solution thermal dose Dc at the hot center ensures sufficient solution at the hot center. Shutdown and residual heat recovery further reduce the time difference between different layers passing through the γ′ precipitation sensitive temperature zone. Each step controls the sources of inhomogeneity in the heating, solution, and cooling stages, and forms a synergistic effect in the continuous thermal history, thereby improving the microstructure consistency, performance stability, and heat treatment pass rate of GH4700 large forgings along the effective thickness direction.
[0087] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Anyone skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention are also considered valid.
Claims
1. A homogenization process for large nickel-based superalloy forgings with γ′ precipitation strengthening, wherein the maximum effective thickness H of the forging is not less than 150 mm, characterized in that... include: S1, take samples from the same furnace to determine the reference temperature Tγ for complete melting of the γ′ phase and the initial melting temperature Tm. Arrange temperature measurement points near the surface and temperature measurement points at the hot center on the forging, and take the maximum measured temperature difference between the two groups of temperature measurement points as ΔT. S2, heat the forging to 25-45℃ below Tγ and hold it until ΔT is not greater than 15℃ and the heating rate of the lowest measured temperature of the hot center is not greater than 0.3℃ / min for 20 minutes. S3, alternately implement 2 to 5 cross-solution line thermal pulses, with the furnace temperature setpoint for each high-temperature segment being 8 to 18°C above Tγ, and both the setpoint and the highest measured temperature near the surface not exceeding Tm-25°C, lasting for 10 to 36 minutes; the furnace temperature setpoint for each low-temperature segment being 5 to 20°C below Tγ and lasting until ΔT is not greater than 12°C; the last high-temperature segment continues for 15 to 35 minutes after the lowest measured temperature at the thermal center reaches 2°C above Tγ, and the cumulative time for the highest measured temperature near the surface to be higher than Tγ does not exceed 120 minutes; S4, forced air cooling is stopped when the lowest measured temperature near the surface is 70 to 110°C below Tγ and the highest measured temperature at the thermal center is 40 to 90°C higher than the lowest measured temperature near the surface, and forced air cooling is stopped. The residual heat inside the forging is used in the insulation cavity to raise the lowest measured temperature near the surface by 5 to 20°C and reduce ΔT to below 15°C, and then cooled to below 750°C.
2. The homogenization treatment process for γ′ precipitation-strengthened nickel-based superalloy large forgings according to claim 1, characterized in that, For any point inside the forging, take the shortest distance to the outer surface that can directly exchange heat with the processing atmosphere, and take the maximum value of the shortest distance as dmax, and let H=2dmax; the mass of the forging is 500-3000kg, H is 150-350mm, and before processing, retain a process extension section that can be removed at both ends of the forging in the axial direction.
3. The homogenization treatment process for γ′ precipitation-strengthened nickel-based superalloy large forgings according to claim 2, characterized in that, At least three parallel samples were obtained from the near-surface layer, 1 / 4 effective thickness, and thermal center region of the extended process section, respectively. Differential scanning calorimetry (DSC) was initially performed at 5 °C / min under argon protection. The parallel samples were then isothermated for 30 min at 5 °C intervals and water-quenched within 30 s after being removed from the furnace. The maximum value among the lowest treatment temperatures where the residual γ′ phase area fraction in each region was less than 0.5% was determined as Tγ. The minimum value among the extrapolated onset temperature of the first melting endothermic peak and the initial melting temperature of the differential scanning calorimetry curve in each region was determined as Tm. Tγ was 1060–1090 °C, and Tm-Tγ was not less than 100 °C.
4. The homogenization treatment process for γ′ precipitation-strengthened nickel-based superalloy large forgings according to claim 2, characterized in that, The near-surface temperature measuring point group includes blind hole temperature measuring points set at at least 3 high heat exchange positions, with the bottom of the hole 8-15 mm away from the surface of the forging; the thermal center temperature measuring point group extends from the axial blind hole opened in the process extension section to a position no more than 0.05H away from the thermal center of the cross section; a 1 / 4 effective thickness temperature measuring point group is added between the near-surface temperature measuring point group and the thermal center temperature measuring point group; ΔT is calculated based on the highest near-surface temperature and the lowest thermal center temperature during heating, and ΔT is calculated based on the highest thermal center temperature and the lowest near-surface temperature during cooling, and all temperature measuring holes are located within the allowance removed during subsequent machining.
5. The homogenization treatment process for γ′ precipitation-strengthened nickel-based superalloy large forgings according to claim 1, characterized in that, Step S2 is carried out in a vacuum or argon circulating furnace. The furnace is loaded at a temperature not higher than 300°C, and the temperature is raised to 650°C at a rate of 40-80°C / h and held until ΔT is not greater than 25°C. Then, the temperature is raised to 90-110°C below Tγ at a rate of 25-45°C / h, and then raised to 25-45°C below Tγ at a rate of 8-18°C / h.
6. The homogenization treatment process for γ′ precipitation-strengthened nickel-based superalloy large forgings according to claim 2, characterized in that, In step S3, the furnace temperature settings for the high-temperature section and the low-temperature section are switched at a rate of 2 to 6 °C / min; the duration τH of each high-temperature section is H×(0.07 to 0.10) min / mm in millimeters; the low-temperature section does not implement forced air cooling and lasts for no less than 8 minutes.
7. The homogenization treatment process for γ′ precipitation-strengthened nickel-based superalloy large forgings according to claim 6, characterized in that, The controller calculates the near-surface supersolid heat dose Ds=∫max(Ts-Tγ,0)dt and the effective solid solution heat dose Dc=∫max[Tc-(Tγ-3℃),0]dt with a sampling period of no more than 5s, where Ts is the highest temperature of the near-surface temperature measurement point group during heating, Tc is the lowest temperature of the temperature measurement point group at the thermal center, and t is in min. Ds is integrated for each high-temperature segment and Dc is integrated over the entire process of step S3, so that Ds for each high-temperature segment is 100~450℃·min, and the sum of Ds for all high-temperature segments is 450~1500℃·min. The last high-temperature segment ends when Dc reaches 150~450℃·min.
8. The homogenization treatment process for γ′ precipitation-strengthened nickel-based superalloy large forgings according to claim 4, characterized in that, The initial forced air cooling in step S4 uses circulating argon gas with an absolute pressure of 0.2–0.6 MPa, which is alternately supplied along the axial and radial directions of the forging, with a switching cycle of 60–180 s. This cools the near-surface layer at an average rate of 6–15 °C / min within the range of Tγ to 100 °C below Tγ, and ensures that the temperature difference between each near-surface temperature measurement point is no greater than 15 °C. When the lowest near-surface temperature is 80–100 °C below Tγ and the highest temperature of the thermal center is 50–80 °C higher than the lowest near-surface temperature, the air supply is stopped.
9. The homogenization treatment process for γ′ precipitation-strengthened nickel-based superalloy large forgings according to claim 8, characterized in that, After stopping the air supply, the external gas exchange of the sealed insulation cavity is closed, and the cavity wall temperature is maintained at 0-15°C below the lowest near-surface temperature when the air supply stops. The speed of the circulating fan is kept below 10% of the rated speed. Within H×(0.10-0.25) min / mm, the lowest near-surface temperature is raised by 8-18°C and ΔT is reduced to within 12°C. Forced air cooling is restarted after the temperature of all 1 / 4 effective thickness temperature measurement points is between the highest temperature of the thermal center and the lowest near-surface temperature.
10. The homogenization treatment process for γ′ precipitation-strengthened nickel-based superalloy large forgings according to claim 9, characterized in that, After restarting the forced air cooling, the average cooling rate of the highest temperature in the thermal center from 120°C below Tγ to 820°C is 3-8°C / min, and the difference in the average cooling rate between the near-surface layer, 1 / 4 of the effective thickness, and adjacent temperature measuring layers in the thermal center is no greater than 2.5°C / min. Select a stop-cooling trigger temperature within the range of 790-810°C. When any temperature measuring point cools to the stop-cooling trigger temperature, the forced air cooling is paused. After all temperature measuring points reach 800±10°C and ΔT is no greater than 8°C, the timing is started. The temperature is maintained for 14-18 hours, and then cooled to 650°C at a rate of 20-40°C / h, followed by air cooling to below 100°C.