Nickel-platinum alloy target material and method for producing the same
Ni₃Pt and NiPt alloy powders were prepared by vacuum atomization through the mixed melting of Ni and Pt metals, followed by hot pressing and sintering. This solved the problem that existing nickel-platinum alloy targets could not form an ordered phase structure with high Pt content, and enabled the preparation of nickel-platinum alloy targets with high magnetic permeability, meeting the needs of ultra-high density magnetic storage technology.
Patent Information
- Application Number
- CN202611413394.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-20
AI Technical Summary
Existing nickel-platinum alloy target preparation technology cannot form an ordered phase structure of Ni₃Pt(L1₂) + NiPt(L1₀) in a high Pt content system, which is difficult to meet the requirements of high magnetic permeability and cannot support the development of ultra-high density magnetic storage technology.
Ni₃Pt alloy powder and NiPt alloy powder were prepared by mixing and melting Ni metal and Pt metal and then vacuum atomizing. After being mixed in a preset ratio, they were hot-pressed and sintered to prepare nickel-platinum alloy targets.
The prepared nickel-platinum alloy target material has high purity, high density and high magnetic permeability, with a magnetic permeability close to 100%, which meets the requirements of ultra-high density magnetic storage technology.
Smart Images

Figure CN123132816A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of target manufacturing technology, and in particular to a nickel-platinum alloy target and its preparation method. Background Technology
[0002] Magnetic storage technology is the core foundation of modern information technology. With the increasing demands for storage capacity, read / write speed, and long-term data reliability in the era of big data, traditional iron-based and cobalt-based magnetic storage materials are gradually approaching their physical limits and are unable to support the evolution of future ultra-high-density magnetic storage technologies. Heat-assisted magnetic recording (HAMR) is the core technology of next-generation high-density hard disk storage. Its core medium is a FePt vertical magnetic anisotropy multilayer thin film with an L10 ordered phase. Ni-30at%Pt alloy can be used as a crystal growth template for FePt layers, precisely guiding the easy magnetization axis of FePt grains to grow perpendicular to the thin film plane. It is a key material that determines the crystal quality and magnetic properties of HAMR medium. The development of high-performance nickel-platinum alloy targets for magnetic storage applications has significant technological and industrial value.
[0003] Existing nickel-platinum alloy target fabrication technologies are primarily geared towards integrated circuits and discrete devices, generally only applicable to low-platinum alloy systems with Pt content of 5-15 at%. No dedicated fabrication scheme has yet been developed for high-Pt-content nickel-platinum targets in the magnetic storage field. The ideal crystal form for Ni-30 at% Pt alloy targets is composed of an ordered Ni3Pt(L12) + NiPt(L10) phase structure to meet the high permeability requirements. However, the traditional smelting-forging-rolling method for target fabrication mainly improves permeability by controlling coercivity and crystal orientation. This mechanism is not suitable for high-Pt-content systems, failing to form a sufficiently uniform and dispersed ordered Ni3Pt(L12) and NiPt(L10) phase structure, thus failing to meet the high permeability requirements and hindering the development of next-generation ultra-high-density magnetic storage technologies. Summary of the Invention
[0004] This application provides a nickel-platinum alloy target and its preparation method, aiming to prepare a nickel-platinum alloy target with high purity, high density, good uniformity and high magnetic permeability.
[0005] The method for preparing the nickel-platinum alloy target provided in this application includes the following steps:
[0006] S1, Ni metal and Pt metal are mixed and melted at atomic ratios of 3:1 and 1:1 respectively, and then vacuum atomized to obtain Ni3Pt alloy powder and NiPt alloy powder.
[0007] S2, mix the Ni3Pt alloy powder and NiPt alloy powder according to a preset ratio to obtain alloy mixed powder;
[0008] S3, the alloy mixed powder is loaded into a mold, and the alloy mixed powder is hot-pressed and sintered under a preset vacuum degree to obtain a nickel-platinum alloy billet;
[0009] S4, the nickel-platinum alloy billet is processed to a preset size to obtain the target nickel-platinum alloy target.
[0010] Optionally, the preset ratio is: the ratio of Ni3Pt alloy powder to NiPt alloy powder is 2:1 in terms of the amount of substance.
[0011] Optionally, the oxygen content of the Ni3Pt alloy powder and NiPt alloy powder is ≤100ppm.
[0012] Optionally, the particle size of the Ni3Pt alloy powder and the NiPt alloy powder is -150 mesh.
[0013] Optionally, the preset vacuum level is <10 Pa.
[0014] Optionally, the hot pressing sintering includes the following steps:
[0015] S31, the alloy mixture powder is heated to 550~650°C at a first heating rate and held at that temperature for a first preset time; then the alloy mixture powder is heated to 1000~1050°C at a second heating rate and held at that temperature for a second preset time; the second heating rate is less than the first heating rate.
[0016] S32, the alloy mixture powder is heated to 1100~1200℃ at a third heating rate, held at the temperature for a third preset time, and then pressurized to a preset pressure. After that, it is held at the preset pressure and 1100~1200℃ for a fourth preset time to obtain a nickel-platinum alloy billet.
[0017] S33, the nickel-platinum alloy billet is depressurized and cooled in the furnace before being taken out.
[0018] Optionally, the first heating rate is 7~9℃ / min, the second heating rate is 4~6℃ / min, and the third heating rate is 4~6℃ / min.
[0019] Optionally, the first preset duration is 20-40 minutes, the second preset duration is 40-80 minutes, the third preset duration is 40-80 minutes, and the fourth preset duration is 90-120 minutes.
[0020] Optionally, the preset pressure is 35~40MPa.
[0021] This application has the following beneficial effects:
[0022] This application employs a process of mixing and melting Ni metal and Pt metal and then vacuum atomizing to synthesize Ni3Pt and NiPt phase alloy powders in advance. After mixing the Ni3Pt alloy powder and NiPt alloy powder in a preset ratio, they are hot-pressed and sintered. The resulting nickel-platinum alloy target not only meets the basic requirements of high purity, high uniformity and high density, but also has extremely high magnetic permeability, which is close to 100%. This meets the high magnetic permeability requirements of ultra-high density magnetic storage technology for nickel-platinum alloy targets. Attached Figure Description
[0023] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0024] Figure 1 The flowcharts are for some embodiments of the preparation method of the nickel-platinum alloy target material of this application.
[0025] Figure 2 This is a schematic diagram of the process flow for some embodiments of the preparation method of the nickel-platinum alloy target material of this application;
[0026] Figure 3 Metallographic micrograph of the nickel-platinum alloy target material prepared in Example 1 of this application;
[0027] Figure 4 This is a metallographic micrograph of the nickel-platinum alloy target material prepared in Example 2 of this application. Detailed Implementation
[0028] To make the inventive objectives, features, and advantages of this application more apparent and understandable, the technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the embodiments described below are only a part of the embodiments of this application, and not all of them. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0029] The terms “first,” “second,” “third,” “fourth,” etc. (if present) in the specification and drawings of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of this application described herein can be implemented, for example, in orders other than those illustrated or described herein. Furthermore, the terms “comprising” and “having,” and any variations thereof, are intended to cover non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.
[0030] Experimental methods not specified in the embodiments of this application are generally performed under conventional conditions and conditions in the manual, or under conditions recommended by the manufacturer; the general equipment, materials, reagents, etc. used are all commercially available unless otherwise specified.
[0031] See Figure 1 , 2 In the embodiments of this application, the preparation method of the nickel-platinum alloy target includes steps S1 to S4:
[0032] S1, Ni metal and Pt metal are mixed and melted at atomic ratios of 3:1 and 1:1 respectively, and then vacuum atomized to obtain Ni3Pt alloy powder and NiPt alloy powder.
[0033] Specifically, this step uses electrolytic Ni metal blocks and Pt sheets with a purity of not less than 4N to prepare Ni3Pt (Pt atomic ratio 25%) alloy powder and NiPt alloy powder (Pt atomic ratio 50%) through vacuum melting and vacuum atomization, respectively. The melting equipment can be a vacuum induction melting furnace, a vacuum arc melting furnace, or an electron beam melting furnace, and the vacuum atomization unit can be integrated with the melting equipment. The prepared Ni3Pt alloy powder and NiPt alloy powder must meet the requirements of oxygen content ≤100ppm and particle size -150 mesh to ensure that the final target product has extremely low oxygen content and good density and uniformity of the target material. -150 mesh means the sieve aperture corresponding to a particle size of less than or equal to 150 mesh.
[0034] S2, mix Ni3Pt alloy powder and NiPt alloy powder according to the preset ratio to obtain alloy mixed powder.
[0035] Specifically, for Ni-30at%Pt alloy targets, the ratio of Ni3Pt alloy powder to NiPt alloy powder is 2:1 by molar amount.
[0036] In some embodiments, a dual-motion powder mixer is used to mix Ni3Pt alloy powder and NiPt alloy powder for 8-12 hours. The dual-motion powder mixer is a high-end powder mixing equipment with two independent drive motion systems. The first motion system makes the cylinder rotate as a whole, and the second motion system makes the internal spiral ribbon / blade group of the cylinder rotate independently. This can ensure that the mixing state of the entire batch of powder is highly consistent and can ensure the stability of the composition and particle size distribution of samples taken from different batches and different locations.
[0037] S3. The alloy mixed powder is loaded into a mold and sintered under a preset vacuum degree (<10Pa) by vacuum hot pressing (VHP) to obtain a nickel-platinum alloy billet.
[0038] In the hot pressing sintering process, alloy powder is first loaded into a high-temperature resistant mold, which is then placed in a vacuum or high-purity inert atmosphere. At a temperature below the melting point of the material, axial mechanical pressure and high temperature are applied simultaneously, causing the powder particles to gradually weld together through plastic deformation, rearrangement, atomic diffusion, and sintering neck growth, ultimately achieving a high-density near-net-shape blank. The mold is either a CC mold or a graphite mold, with CC molds being preferred. CC molds have advantages such as high temperature and high strength, excellent thermal shock and fatigue resistance, high dimensional accuracy, good near-net-shape forming effect, low contamination risk, and uniform pressure transmission. The hot pressing sintering of alloy mixed powders can be carried out using vacuum hot pressing sintering furnaces, spark plasma sintering furnaces, hot isostatic pressing equipment, etc.
[0039] Hot pressing sintering includes the following steps:
[0040] S31, the alloy mixture powder is heated to 550~650℃ at a first heating rate and held at that temperature for a first preset time; then the alloy mixture powder is heated to 1000~1050℃ at a second heating rate and held at that temperature for a second preset time.
[0041] The second heating rate is lower than the first heating rate to reduce the thermal gradient inside and outside the compact, avoid uneven heating and cooling that could cause thermal stress, which could lead to compact delamination and microcracks. The slow heating in the temperature range close to sintering also provides a uniform temperature basis for the formation of the sintering neck.
[0042] In some specific embodiments, the first heating rate is selected as 7~9℃ / min, the first preset duration is selected as 20~40min, the second heating rate is selected as 4~6℃ / min, and the second preset duration is selected as 40~80min.
[0043] S32, the alloy mixed powder is heated to 1100~1200℃ at the third heating rate, held at the temperature for the third preset time, and then pressurized to the preset pressure. After that, it is held at the preset pressure and 1100~1200℃ for the fourth preset time to obtain the nickel-platinum alloy billet.
[0044] This step is the final densification stage of the billet under high temperature and high pressure conditions. The high temperature of 1100~1200℃ fully activates grain boundary diffusion and bulk diffusion, and the high pressure thoroughly compacts the micro closed pores left by the previous process. Long-term heat and pressure are maintained to weld the pore boundaries through atomic diffusion, and finally a high-density billet is obtained.
[0045] In some specific embodiments, the third heating rate is selected as 4~6℃ / min, the third preset duration is selected as 40~80min, the fourth preset duration is selected as 90~120min, and the preset pressure is 35~40MPa.
[0046] S33, the nickel-platinum alloy billet is depressurized and cooled in the furnace before being taken out.
[0047] This step of slowly reducing pressure and slowly cooling in the furnace allows stress to be released gradually, avoiding cracking and warping of the billet caused by sudden pressure relief and rapid cooling, and ensuring the dimensional accuracy and structural integrity of the target billet.
[0048] S4. The nickel-platinum alloy billet is processed to the preset size to obtain the target nickel-platinum alloy target.
[0049] This step involves using a CNC lathe to precisely machine and trim the nickel-platinum alloy billet to the finished size. After cleaning, drying, and packaging, the finished nickel-platinum alloy target material can be obtained.
[0050] This application employs a process of mixing and melting Ni metal and Pt metal and then vacuum atomizing to synthesize Ni3Pt and NiPt phase alloy powders in advance. After mixing the Ni3Pt alloy powder and NiPt alloy powder in a preset ratio, they are hot-pressed and sintered. The resulting nickel-platinum alloy target not only meets the basic requirements of high purity, high uniformity and high density, but also has extremely high magnetic permeability, which is close to 100%. This meets the high magnetic permeability requirements of ultra-high density magnetic storage technology for nickel-platinum alloy targets.
[0051] Based on the above embodiments, in order to further illustrate the implementation of the technical solution of this application, the following specific embodiments are also proposed. It should be noted that the following specific embodiments are merely exemplary and are not intended to limit the scope of protection of this application in any way.
[0052] Example 1
[0053] This embodiment describes the preparation of a nickel-platinum alloy target.
[0054] Step 1: Prepare Ni3Pt (Pt atomic ratio 25%) and NiPt (Pt atomic ratio 50%) alloy powders using pure Ni blocks and pure Pt blocks with a purity of not less than 4N. Select integrated vacuum melting equipment and vacuum atomization unit. The oxygen content of Ni3Pt alloy powder and NiPt alloy powder is ≤100ppm, and the powder particle size is -150 mesh (not exceeding 100μm).
[0055] Step 2: Mix Ni3Pt alloy powder and NiPt alloy powder at a molar ratio of 2:1 and use a dual-motion powder mixer to mix the powders. After mixing, take samples from different locations to test the Ni and Pt content to ensure that the uniformity requirements are met.
[0056] Step 3: Load the alloy mixture powder into the CC mold, ensuring that the flatness of the mold is <1mm. Use graphite paper between the powder and the mold and spray boron nitride to separate them to prevent contamination.
[0057] Step 4: Place the mold containing the powder into a hot press furnace, evacuate to below 10 Pa, then power on and heat up to sinter in sections.
[0058] First, the alloy mixture powder is heated to 600℃ at a heating rate of 8℃ / min and held for 30min.
[0059] The alloy mixture powder was then heated from 600°C to 1000°C at a heating rate of 5°C / min and held at that temperature for 60 min.
[0060] The alloy powder mixture was then heated from 1000℃ to 1150℃ at a heating rate of 5℃ / min, held at that temperature for 60 min, and then pressurized to 40MPa within 60 min. The mixture was then held at 1150℃ and 40MPa for 120 min to obtain a nickel-platinum alloy billet. The nickel-platinum alloy billet was then depressurized and cooled in the furnace to below 200℃ before being removed.
[0061] Example 2
[0062] This embodiment describes the preparation of a nickel-platinum alloy target.
[0063] Step 1: Prepare Ni3Pt and NiPt alloy powders using pure Ni blocks and pure Pt blocks with a purity of not less than 4N. Select an integrated vacuum melting equipment and vacuum atomization unit. The oxygen content of Ni3Pt alloy powder and NiPt alloy powder is ≤100ppm and the powder particle size is -150 mesh.
[0064] Step 2: Mix Ni3Pt alloy powder and NiPt alloy powder at a molar ratio of 2:1 and use a dual-motion powder mixer to mix the powders. After mixing, take samples from different locations to test the Ni and Pt content to ensure that the uniformity requirements are met.
[0065] Step 3: Load the alloy mixture powder into the CC mold, ensuring that the flatness of the mold is <1mm. Use graphite paper between the powder and the mold and spray boron nitride to separate them to prevent contamination.
[0066] Step 4: Place the mold containing the powder into a hot press furnace, evacuate to below 10 Pa, then power on and heat up to sinter in sections.
[0067] First, the alloy mixture powder is heated to 600℃ at a heating rate of 8℃ / min and held for 30min.
[0068] The alloy mixture powder was then heated from 600°C to 1000°C at a heating rate of 5°C / min and held at that temperature for 60 min.
[0069] The alloy powder mixture was then heated from 1000℃ to 1200℃ at a heating rate of 5℃ / min, held at that temperature for 60 min, and then pressurized to 35MPa within 60 min. It was then held at 1200℃ and 35MPa for 90 min to obtain a nickel-platinum alloy billet. The nickel-platinum alloy billet was depressurized and cooled in the furnace to below 200℃ before being removed.
[0070] Comparative Example 1
[0071] A nickel-platinum alloy target was prepared in this comparative example.
[0072] Step 1: Mix pure Ni metal powder (purity not less than 4N) and pure Pt metal powder (purity not less than 4N) in a ratio of 7:3 and use a dual-motion powder mixer to mix the powders. After mixing, take samples from different locations to test the Ni and Pt content to ensure that the uniformity requirements are met.
[0073] Step 2: Load the alloy mixture powder into the CC mold, ensuring that the flatness of the mold is <1mm. Use graphite paper between the powder and the mold and spray boron nitride to separate them to prevent contamination.
[0074] Step 3: Place the mold containing the powder into a hot press furnace, evacuate to below 10 Pa, then power on and heat up to sinter in sections.
[0075] First, the alloy mixture powder is heated to 600℃ at a heating rate of 8℃ / min and held for 30min.
[0076] The alloy mixture powder was then heated from 600°C to 1000°C at a heating rate of 5°C / min and held at that temperature for 60 min.
[0077] The alloy powder mixture was then heated from 1000℃ to 1150℃ at a heating rate of 5℃ / min, held at that temperature for 60 min, and then pressurized to 40MPa within 60 min. The mixture was then held at 1150℃ and 40MPa for 120 min to obtain a nickel-platinum alloy billet. The nickel-platinum alloy billet was then depressurized and cooled in the furnace to below 200℃ before being removed.
[0078] Comparative Example 2
[0079] A nickel-platinum alloy target was prepared in this comparative example.
[0080] Step 1: Prepare Ni-30at%Pt alloy powder (Pt atomic content 30%) using pure Ni blocks with a purity of not less than 4N and pure Pt blocks. The oxygen content of the Ni-30at%Pt alloy powder is ≤100ppm and the powder particle size is -150 mesh.
[0081] Step 2: Load Ni-30at%Pt alloy powder into a CC mold, ensuring the mold flatness is <1mm. Use graphite paper between the powder and the mold and spray boron nitride to separate them to prevent contamination.
[0082] Step 3: Place the mold containing the powder into a hot press furnace, evacuate to below 10 Pa, then power on and heat up to sinter in sections.
[0083] First, the alloy mixture powder is heated to 600℃ at a heating rate of 8℃ / min and held for 30min.
[0084] The alloy mixture powder was then heated from 600°C to 1000°C at a heating rate of 5°C / min and held at that temperature for 60 min.
[0085] The alloy powder mixture was then heated from 1000℃ to 1150℃ at a heating rate of 5℃ / min, held at that temperature for 60 min, and then pressurized to 40MPa within 60 min. The mixture was then held at 1150℃ and 40MPa for 120 min to obtain a nickel-platinum alloy billet. The nickel-platinum alloy billet was then depressurized and cooled in the furnace to below 200℃ before being removed.
[0086] Comparative Example 3
[0087] A nickel-platinum alloy target was prepared in this comparative example. The preparation steps were the same as in Example 1, except that the sintering step was different.
[0088] First, the alloy mixture powder is heated to 600℃ at a heating rate of 8℃ / min and held for 30min.
[0089] The alloy mixture powder was then heated from 600°C to 1000°C at a heating rate of 5°C / min and held at that temperature for 60 min.
[0090] The alloy powder mixture was then heated from 1000℃ to 1300℃ at a heating rate of 5℃ / min, held at that temperature for 60 min, and then pressurized to 40MPa within 60 min. It was then held at 1300℃ and 40MPa for 120 min to obtain a nickel-platinum alloy billet. The nickel-platinum alloy billet was depressurized and cooled in the furnace to below 200℃ before being removed.
[0091] Comparative Example 4
[0092] A nickel-platinum alloy target was prepared in this comparative example. The preparation steps were the same as in Example 1, except that the sintering step was different.
[0093] First, the alloy mixture powder is heated to 600℃ at a heating rate of 8℃ / min and held for 30min.
[0094] The alloy powder mixture was then heated from 600°C to 1000°C at a heating rate of 5°C / min, held at that temperature for 60 min, and then pressurized to 40 MPa within 60 min. It was then held at 1000°C and 40 MPa for 120 min to obtain a nickel-platinum alloy billet. The nickel-platinum alloy billet was depressurized and cooled in the furnace to below 200°C before being removed.
[0095] Table 1 Statistical Table of Target Material Sample Quality
[0096]
[0097] The purity, density, grain size (average size), and permeability (PTF) of the target samples prepared in Examples 1, 2 and Comparative Examples 1-4 were characterized, and their microstructure uniformity was statistically analyzed. The results are shown in Table 1.
[0098] The metallographic structures of the target samples prepared in Examples 1 and 2 are as follows: Figure 3 , 4 As shown, the grain structure of the target material samples is relatively fine and uniform; the magnetic permeability test results show that the target material samples prepared in Examples 1 and 2 have a magnetic permeability of nearly 100%.
[0099] Comparative Example 1 uses pure Ni metal powder and pure Pt metal powder to mix and sinter. The resulting Ni-30at%Pt alloy target has a low magnetic permeability. This is because the Ni and Pt atoms in the pure Ni powder and pure Pt powder are enriched in their respective original powder particles, and cannot form stable Ni3Pt (L12) and NiPt (L10) ordered phase structures. Even in regions where the composition matches the corresponding phase structure, the long-range ordering of the disordered solid solution requires overcoming a higher energy barrier. As a result, the ordered phase has a low proportion, poor degree of order, and scattered distribution, leading to low magnetic permeability of the target.
[0100] Comparative Example 2 uses pure Ni and pure Pt to directly prepare Ni-30at%Pt alloy powder with the required atomic ratio. The Ni-30at%Pt alloy powder is then hot-pressed and sintered to obtain Ni-30at%Pt alloy target material. However, the target material prepared by this technical route also has low permeability. This is because to decompose the Ni3Pt (L12) and NiPt (L10) ordered phase structures from the disordered solid solution of Ni-30at%Pt of a single composition, a solid phase transition process involving composition amplitude modulation / nucleation growth and long-range atomic rearrangement is required. Atoms must achieve composition redistribution through diffusion so that the local area reaches the stoichiometry of the two ordered phases respectively, and at the same time complete the lattice ordering transformation. However, the atomic diffusion rate under solid-state sintering is much lower than that under liquid state, and the formation of ordered phase is difficult to proceed fully, resulting in low permeability of the target material structure.
[0101] Comparative Example 3 uses a higher sintering temperature (1300℃), and the grain size of the target microstructure reaches as high as 85μm. This is because at the excessively high sintering temperature, the activation energy of grain boundary diffusion and volume diffusion of Ni and Pt atoms is fully overcome, the supply of atoms for grain boundary migration is sufficient, the grain growth rate is fast, resulting in grain coarsening. The excessively coarse grain structure will also lead to a decrease in the magnetic permeability of the target. Comparative Example 4 uses a lower sintering temperature (1000℃), and the density of the target is lower. This is because the sintering temperature is too low, which suppresses the volume diffusion of atoms. The limited grain boundary diffusion makes it difficult to achieve sufficient growth of the sintering neck and closure of pores, and the material migration rate is insufficient to support the densification requirements.
[0102] In this embodiment, Ni3Pt ordered phase alloy powder and NiPt ordered phase alloy powder are pre-synthesized separately and mixed in a certain proportion. The powder particles already have a complete ordered crystal structure and a precise stoichiometric ratio. The sintering process only requires short-range diffusion at the particle interface to achieve metallurgical bonding, without the need for large-scale component redistribution and solid-state phase transformation. Therefore, it can completely preserve the uniform ordered two-phase structure with few lattice defects and low magnetic domain migration resistance. Finally, while ensuring the high purity and high density of the target material, it achieves microstructure homogenization and extremely high magnetic permeability.
[0103] The above-described embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of this application.
Claims
1. A method for preparing a nickel-platinum alloy target, characterized in that, Including the following steps: S1, Ni metal and Pt metal are mixed and melted at atomic ratios of 3:1 and 1:1 respectively, and then vacuum atomized to obtain Ni3Pt alloy powder and NiPt alloy powder. S2, mix the Ni3Pt alloy powder and NiPt alloy powder according to a preset ratio to obtain alloy mixed powder; S3, the alloy mixed powder is loaded into a mold, and the alloy mixed powder is hot-pressed and sintered under a preset vacuum degree to obtain a nickel-platinum alloy billet; S4, the nickel-platinum alloy billet is processed to a preset size to obtain the target nickel-platinum alloy target.
2. The method for preparing the nickel-platinum alloy target according to claim 1, characterized in that, The preset ratio is: by mass, the ratio of Ni3Pt alloy powder to NiPt alloy powder is 2:
1.
3. The method for preparing the nickel-platinum alloy target according to claim 1, characterized in that, The oxygen content of the Ni3Pt alloy powder and NiPt alloy powder is ≤100ppm.
4. The method for preparing the nickel-platinum alloy target according to claim 1, characterized in that, The particle size of the Ni3Pt alloy powder and the NiPt alloy powder is -150 mesh.
5. The method for preparing the nickel-platinum alloy target according to claim 1, characterized in that, The preset vacuum level is <10 Pa.
6. The method for preparing the nickel-platinum alloy target according to claim 1, characterized in that, The hot pressing sintering includes the following steps: S31, the alloy mixture powder is heated to 550~650°C at a first heating rate and held at that temperature for a first preset time; then the alloy mixture powder is heated to 1000~1050°C at a second heating rate and held at that temperature for a second preset time; the second heating rate is less than the first heating rate. S32, the alloy mixture powder is heated to 1100~1200℃ at a third heating rate, held at the temperature for a third preset time, and then pressurized to a preset pressure. After that, it is held at the preset pressure and 1100~1200℃ for a fourth preset time to obtain a nickel-platinum alloy billet. S33, the nickel-platinum alloy billet is depressurized and cooled in the furnace before being taken out.
7. The method for preparing the nickel-platinum alloy target according to claim 6, characterized in that, The first heating rate is 7~9℃ / min, the second heating rate is 4~6℃ / min, and the third heating rate is 4~6℃ / min.
8. The method for preparing the nickel-platinum alloy target according to claim 6, characterized in that, The first preset duration is 20-40 minutes, the second preset duration is 40-80 minutes, the third preset duration is 40-80 minutes, and the fourth preset duration is 90-120 minutes.
9. The method for preparing the nickel-platinum alloy target according to claim 6, characterized in that, The preset pressure is 35~40MPa.
10. A nickel-platinum alloy target material, characterized in that, It is prepared by the method for preparing nickel-platinum alloy target material according to any one of claims 1-9.