A copper target material and a method for manufacturing the same
By combining variable-speed centrifugal casting with alternating magnetic field and annealing, the problems of coarse grains and high oxygen content in copper targets were solved, and high-purity, high-density, fine and uniform copper targets were prepared, improving film quality and production efficiency.
Patent Information
- Application Number
- CN202611648062.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-23
- Publication Date
- 2026-11-20
AI Technical Summary
Existing copper sputtering processes suffer from problems such as coarse and uneven grains, excessive oxygen content, and low production efficiency, resulting in uneven film quality and poor stability of the sputtering process.
A variable-speed centrifugal casting method combined with an alternating magnetic field is adopted. Impurities are removed by vacuum melting, and the grains are refined by the synergistic effect of the alternating magnetic field and centrifugal force. After annealing, precision machining is performed to ensure that the grain size is stable within 30μm.
This method achieves high-purity, high-density, low-oxygen-content, and fine-grained, uniform copper target materials, improving the uniformity of thin films and the stability of the sputtering process, and increasing production efficiency.
Smart Images

Figure CN123132818A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of target preparation technology, and particularly relates to a copper target and its preparation method. Background Technology
[0002] High-purity copper sputtering targets are core raw materials for preparing key films such as interconnect wires, functional electrodes, and barrier layers in integrated circuits, display panels, and photovoltaic cells. Their performance directly determines the uniformity, conductivity, and adhesion of the deposited thin film, ultimately affecting the performance, yield, and reliability of the end devices. With the rapid development of high-tech industries such as semiconductors and display panels towards higher precision, higher integration, and lower power consumption, the performance requirements for copper sputtering targets are becoming increasingly stringent. Typically, these requirements include a copper sputtering target purity ≥99.99%, density ≥99.7%, oxygen content ≤5ppm, fine and uniform grain size, and excellent surface quality.
[0003] Currently, the industry mainly uses vacuum melting and casting and hot extrusion forming processes to prepare copper sputtering targets. Although this process can produce high-purity copper ingots through vacuum melting and casting, it has significant drawbacks: First, the process is lengthy, involving multiple steps such as melting, casting, hot extrusion, multiple heat treatments and machining, resulting in low production efficiency and high costs. Second, although hot extrusion can break up some of the as-cast structure, subsequent high-temperature treatment will cause grain recrystallization and abnormal growth, resulting in coarse copper target grains (usually 70~80μm). Furthermore, repeated heating and cooling exacerbate the unevenness of the structure, and may even cause deformation and microcracks. Such coarse and uneven grain structure and cracks will reduce the uniformity of sputtering film formation and induce arcing and microparticle contamination, thereby damaging the film quality and the stability of the sputtering process.
[0004] Therefore, there is an urgent need to develop a method for preparing high-purity, low-oxygen, and fine-grained copper target materials. Summary of the Invention
[0005] The purpose of this application is to provide a copper sputtering target and its preparation method, which aims to solve the problems of large and uneven grains, excessive oxygen content and low production efficiency of existing copper sputtering targets.
[0006] To achieve the above-mentioned objectives, the technical solution adopted in this application is as follows: In a first aspect, this application provides a method for preparing a copper target, comprising the following steps: The copper raw material is subjected to pretreatment and vacuum melting in sequence to obtain copper molten liquid; The molten copper is poured into a casting mold for variable speed centrifugal casting. An alternating magnetic field is applied during the variable speed centrifugal casting process to electromagnetically stir the liquid and semi-solid copper melt in the casting mold. After the casting is completed, the mixture is cooled and demolded to obtain a copper billet. The copper billet is annealed and precision machined in sequence to obtain a copper target material.
[0007] Secondly, this application provides a copper target material, which is prepared by the preparation method of the copper target material provided in this application.
[0008] Compared with the prior art, this application has the following beneficial effects: (1) First, the moisture, oil and oxide layer on the surface of the copper raw material are removed by pretreatment. Then, the hydrogen, oxygen and nitrogen gaseous impurities and harmful impurities such as lead, bismuth and antimony in the copper melt are removed by vacuum melting environment, so as to achieve deep purification of copper melt and help reduce the impurity content and internal defects of the billet.
[0009] (2) In the molding stage, variable speed centrifugal casting is combined with the application of an alternating magnetic field. In the early stage of casting, a lower speed is used to allow the copper melt to fill the cavity smoothly and completely, preventing the copper melt from splashing and entrapping due to high speed, and the "raining" phenomenon caused by low speed, thereby avoiding defects such as cracks, delamination and inclusions. At the same time, the Lorentz force is used to promote the uniformity of the temperature field and the dispersion of nucleation particles by applying an alternating magnetic field. After the filling is completed, the speed is steadily increased to a higher speed. The strong centrifugal force not only generates a violent shearing effect at the solid-liquid interface to break dendrites, increase nucleation cores and refine grains, but also continuously keeps the copper melt in the mold. By pressing the copper molten metal into the dendrite interstices, strong feeding is achieved, reducing shrinkage porosity and increasing density. At the same time, the alternating magnetic field induced electromagnetic stirring in the liquid and semi-solid melt, and the resulting Lorentz force further enhanced melt convection, broke up the dendrites at the solidification front, and further refined the grains. In the later stage of solidification, the alternating magnetic field was stopped, and strong centrifugal force was used to continuously press the copper molten metal into the dendrite interstices, achieving strong feeding, reducing shrinkage porosity and increasing density, and fully completing the separation of inclusions. Therefore, under the synergistic effect of the centrifugal force field and the electromagnetic field, the density, grain size and uniformity of the copper billet were significantly improved.
[0010] (3) Annealing eliminates residual casting stress, refines grains, and stabilizes the internal structure, ensuring that the grain size is stable within 30 μm. Finally, precision machining yields a copper target material with high purity, high density, low oxygen content, and fine and uniform grains. Attached Figure Description
[0011] To more clearly illustrate the technical solutions in the embodiments of this application, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0012] Figure 1 This is a process flow diagram of the method for preparing the copper target provided in the embodiments of this application; Figure 2This is a microstructure image of the copper target material prepared in Example 1 of this application; Figure 3 This is a microstructure image of the copper target material prepared in Example 2 of this application; Figure 4 This is a microstructure image of the copper target material prepared in Example 3 of this application; Figure 5 This is a microstructure image of the copper target material prepared in Example 4 of this application; Figure 6 This is a microstructure image of the copper target material prepared in Example 5 of this application; Figure 7 This is a microstructure image of the copper target material prepared in Example 6 of this application; Figure 8 This is a microstructure image of the copper target material prepared in Comparative Example 1 of this application; Figure 9 This is a microstructure image of the copper target material prepared in Comparative Example 2 of this application; Figure 10 This is a microstructure image of the copper target material prepared in Comparative Example 3 of this application. Detailed Implementation
[0013] To make the technical problems, technical solutions, and beneficial effects of this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.
[0014] The first aspect of this application provides a method for preparing a copper target, such as... Figure 1 As shown, it includes the following steps: The copper raw material is subjected to pretreatment and vacuum melting in sequence to obtain copper molten liquid; The molten copper is poured into a casting mold for variable speed centrifugal casting. An alternating magnetic field is applied during the variable speed centrifugal casting process to electromagnetically stir the liquid and semi-solid copper melt in the casting mold. After the casting is completed, the mixture is cooled and demolded to obtain a copper billet. The copper billet is annealed and precision machined in sequence to obtain a copper target material.
[0015] The method for preparing the copper target provided in this application first removes moisture, oil, and surface oxide layers from the copper raw material through pretreatment. Then, a vacuum melting environment is used to remove gaseous impurities such as hydrogen, oxygen, and nitrogen, as well as harmful impurities such as lead, bismuth, and antimony from the molten copper, achieving deep purification of the molten copper and helping to reduce the impurity content and internal defects of the cast billet. In the forming stage, variable-speed centrifugal casting is combined with the application of an alternating magnetic field. In the initial stage of casting, a lower rotation speed allows the molten copper to fill the cavity smoothly and completely, preventing splashing and air entrapment caused by high rotation speed, and the "raining" phenomenon caused by low rotation speed, thereby avoiding defects such as cracks, delamination, and inclusions. Simultaneously, the application of the alternating magnetic field utilizes Lorentz force to promote uniform temperature field and disperse nucleation particles. After filling is complete, the rotation speed is steadily increased to a higher speed. The strong centrifugal force not only generates intense shearing at the solid-liquid interface to break dendrites, increase nucleation sites, and refine grains, but also continuously pressurizes the molten copper into the mold. The interdendritic space provides strong feeding, reducing shrinkage porosity and increasing density. Simultaneously, the maintained alternating magnetic field induces electromagnetic stirring in the liquid and semi-solid melts. The resulting Lorentz force further enhances melt convection, breaks up dendrites at the solidification front, and further refines the grains. In the later stages of solidification, the alternating magnetic field is stopped, and strong centrifugal force continuously forces the molten copper into the interdendritic space, achieving strong feeding, reducing shrinkage porosity and increasing density, and fully separating inclusions. Therefore, under the synergistic effect of the centrifugal force and electromagnetic field, the density, grain size, and uniformity of the copper billet are significantly improved. Annealing then eliminates residual casting stress, refines the grains, and stabilizes the internal structure, ensuring the grain size remains stable within 30 μm. Finally, precision machining yields high-purity, high-density, low-oxygen-content copper targets with fine and uniform grains.
[0016] Step S1, in the embodiment, the purity of the copper raw material is ≥99.99%.
[0017] In this embodiment, the pretreatment step includes drying the copper raw material under a vacuum of ≤10 Pa and a temperature of 120~180℃ for 2~4 hours. These copper particle pretreatment conditions can remove moisture, oil, and oxide layers from the surface of the copper particles.
[0018] In this embodiment, the vacuum melting process includes: melting the pretreated copper raw material under a vacuum of ≤5 Pa and a temperature of 1100~1200℃ for 30~60 min; subsequently, introducing inert gas into the furnace at a flow rate of 0.5~1.5 L / min to raise the furnace pressure to atmospheric pressure, and then holding at that temperature for another 5~30 min. First, melting under a vacuum of less than 5 Pa for 30~60 min completely melts the copper particles, utilizing the vacuum environment to remove gaseous impurities such as hydrogen, oxygen, and nitrogen, as well as harmful impurities such as lead, bismuth, and antimony from the molten copper, achieving deep purification of the molten copper; in the later stage of melting, introducing inert gas (such as argon) into the vacuum sintering furnace to raise the furnace pressure to atmospheric pressure, forming a weakly inert protective atmosphere to prevent the molten copper from undergoing violent oxidation upon contact with air when it exits the furnace, thus ensuring a low oxygen content in the molten copper.
[0019] Step S2, in this embodiment, involves pouring molten copper into a casting mold for variable-speed centrifugal casting, and applying an alternating magnetic field during the variable-speed centrifugal casting process. This includes: within 30 seconds after the vacuum melting process, pouring the molten copper into a casting mold preheated to 200-300°C and rotating at 1000-2000 r / min, while simultaneously applying an alternating magnetic field; after pouring, starting at an acceleration of 200-300 r / min... 2 Increase the rotation speed of the casting mold and maintain the application of an alternating magnetic field during acceleration. When the rotation speed reaches 4000~5000 r / min, stop applying the alternating magnetic field and stop acceleration, and continue rotating at 4000~5000 r / min for 1~3 minutes. In this embodiment, within 30 seconds after the vacuum melting process, the molten copper is quickly poured into the casting mold through a diversion device, thereby minimizing the contact time between the molten copper and air and preventing oxidation. In the initial stage of casting, controlling the rotation speed at a low range and simultaneously applying an alternating magnetic field ensures that the molten copper fills the cavity smoothly and completely. This avoids splashing and air entrapment caused by excessive rotation speed, and also prevents "raining" caused by excessively low rotation speed, thus avoiding defects such as cracks, internal delamination, and inclusions in the copper ingot. At the same time, the application of the alternating magnetic field utilizes the Lorentz force to promote melt convection, uniform temperature field, and dispersed nucleation particles. After the molten copper has filled the mold, the rotation speed is increased to 200~300 r / min. 2The acceleration increases the rotational speed, and an alternating magnetic field is maintained during the acceleration process. This acceleration range can achieve a smooth transition and quickly establish the required centrifugal pressure field. At the same time, the Lorentz force generated by the magnetic field works synergistically with the centrifugal force to further break up the growing dendrites, increase the nucleation rate, and make the grains fine and uniform. When the rotational speed reaches 4000~5000 r / min, the alternating magnetic field is stopped to prevent the already separated inclusions from being stirred back into the melt. The high centrifugal force continuously presses the copper melt into the micro-shrinkage zone between the dendrites, achieving strong feeding, thereby further reducing defects such as shrinkage cavities and shrinkage porosity, and making the ingot structure highly dense.
[0020] In this embodiment, during the variable-speed centrifugal casting process, the temperature of the circulating cooling water is controlled at 20~30℃, and the flow rate is 1~2L / min. The cooling water temperature and flow rate range of this embodiment can rapidly reduce the temperature of the molten copper, causing it to solidify and effectively inhibiting grain growth.
[0021] In this embodiment, the intensity of the alternating magnetic field is 0.1~0.5T, the frequency is 10~30Hz, and the wall thickness of the copper billet is 50~80mm. Since copper is a highly conductive material, the skin depth of the alternating magnetic field in the copper melt is relatively shallow. This embodiment uses an alternating magnetic field of 10~30Hz, achieving a skin depth of 42~73mm, matching the skin depth to the copper billet wall thickness, satisfying a skin depth ≥ 0.8 times the copper billet wall thickness (50~80mm), thus ensuring that the magnetic field effectively penetrates to the core of the copper billet. Under the magnetic field parameters of this embodiment, the generated Lorentz force is sufficient to create strong electromagnetic stirring in the liquid and semi-solid melts, thereby enhancing melt convection, homogenizing the melt temperature field, breaking up dendrites at the solidification front, increasing the nucleation rate, promoting equiaxed crystal formation, and improving grain uniformity. Therefore, the synergistic effect of electromagnetic stirring and the high centrifugal force generated by variable-speed centrifugation jointly strengthens the melt feeding and mass transfer process, ultimately significantly improving the density and grain refinement of the copper billet.
[0022] Step S3: In this embodiment, the annealing temperature is 300~500℃, and the holding time is 2~4h. The annealing parameters in this embodiment can effectively eliminate casting residual stress, refine grains, and stabilize the internal structure, ensuring that the grain size is stable within 30μm.
[0023] In the embodiments, the copper target material has a purity of ≥99.99%, a grain size of ≤30μm, a density of ≥99.8%, and an oxygen content of ≤5ppm.
[0024] The second aspect of this application provides a copper target material, which is prepared by the copper target material preparation method provided in this application.
[0025] The copper target material provided in this application embodiment is prepared by the copper target material preparation method provided in this application embodiment, and therefore has excellent properties such as high purity, high density, fine and uniform grains, and low oxygen content.
[0026] The following description is based on specific embodiments.
[0027] Example 1 This embodiment provides a method for preparing a copper target, including the following steps: (1) Raw material pretreatment: Select cathode copper raw material with a purity of 99.99% and crush it into copper particles with a particle size of 5~10mm; place the copper particles in a vacuum drying oven and dry them for 3h under a vacuum of 10Pa and a temperature of 150℃.
[0028] (2) Vacuum melting treatment: The pretreated copper particles are sent into the graphite crucible of the vacuum induction melting furnace. After the vacuum is evacuated to below 5 Pa, the temperature is raised to 1150℃ and held for 45 min to completely melt the copper particles and obtain copper molten liquid. Then, high-purity argon gas is introduced into the furnace at a flow rate of 1.0 L / min until the gas pressure in the furnace rises to atmospheric pressure, and the temperature is held for another 15 min.
[0029] (3) Magnetic field-assisted variable speed centrifugal casting: Within 30 seconds after vacuum melting, molten copper is poured into a casting mold that has been preheated to 250°C and is rotating at 1500 r / min through a guide device. At the same time, the circulating cooling water system of the variable speed centrifugal casting machine is turned on, and the temperature of the circulating cooling water is controlled at 25°C and the flow rate is 1.5 L / min. During casting, an alternating magnetic field is applied through an alternating magnetic field generator located on the outer periphery of the casting mold to electromagnetically stir the liquid and semi-solid copper melt. After pouring, the mixture is stirred at an acceleration of 250 r / min. 2 The rotational speed of the casting mold was increased, and an alternating magnetic field was maintained during the acceleration process. When the speed reached 4500 r / min, the alternating magnetic field and acceleration were stopped, and the mold continued to rotate at 4500 r / min for 2 minutes to allow the molten copper to completely solidify. After molding was completed, the variable-speed centrifugal casting machine and circulating cooling water were stopped sequentially, and the mold was demolded after cooling to room temperature in the furnace, resulting in a copper billet with a wall thickness of 65 mm. The intensity of the alternating magnetic field was 0.3 T, and the frequency was 20 Hz.
[0030] (4) Post-processing: The copper billet is sent into an annealing furnace and heated to 450°C under an argon protective atmosphere. It is held for 3 hours to eliminate internal stress. The annealed copper billet is then precision turned and precision bored to produce copper target material that meets the specified dimensions.
[0031] Example 2 This embodiment provides a method for preparing a copper target, which differs from Embodiment 1 in that: Step (3) Magnetic field-assisted variable speed centrifugal casting: Within 30 seconds after vacuum melting, the molten copper is poured into a casting mold that has been preheated to 250°C and is rotating at 1000 r / min through a flow guide device. At the same time, the circulating cooling water system of the variable speed centrifugal casting machine is turned on, and the temperature of the circulating cooling water is controlled at 25°C and the flow rate is 1.5 L / min. During the casting process, an alternating magnetic field is applied through an alternating magnetic field generator located on the outer periphery of the casting mold to electromagnetically stir the liquid and semi-solid copper melt. After the pouring is completed, the flow rate is increased to 200 r / min. 2 The rotational speed of the casting mold was increased, and an alternating magnetic field was maintained during the acceleration process. When the speed reached 4000 r / min, the alternating magnetic field and acceleration were stopped, and the mold continued to rotate at 4000 r / min for 2 minutes to allow the molten copper to completely solidify. After molding was completed, the variable-speed centrifugal casting machine and circulating cooling water were stopped sequentially, and the mold was demolded after cooling to room temperature in the furnace, resulting in a copper billet with a wall thickness of 80 mm. The intensity of the alternating magnetic field was 0.3 T, and the frequency was 10 Hz.
[0032] Example 3 This embodiment provides a method for preparing a copper target, which differs from Embodiment 1 in that: Step (3) Magnetic field-assisted variable speed centrifugal casting: Within 30 seconds after vacuum melting, the molten copper is poured into a casting mold that has been preheated to 250°C and is rotating at 2000 r / min through a flow guide device. At the same time, the circulating cooling water system of the variable speed centrifugal casting machine is turned on, and the temperature of the circulating cooling water is controlled at 25°C and the flow rate is 1.5 L / min. During the casting process, an alternating magnetic field is applied through an alternating magnetic field generator located on the outer periphery of the casting mold to electromagnetically stir the liquid and semi-solid copper melt. After the pouring is completed, the flow rate is increased to 300 r / min. 2 Increase the rotation speed of the casting mold and maintain the application of an alternating magnetic field during the acceleration process; when the rotation speed reaches 5000 r / min, stop applying the alternating magnetic field and stop the acceleration, and rotate at 5000 r / min for 2 minutes to allow the copper molten metal to completely solidify, i.e., after the molding is completed, stop the variable speed centrifugal casting machine and the circulating cooling water in sequence, and demold after cooling to room temperature in the furnace to obtain a copper billet with a wall thickness of 50 mm; wherein, the strength of the alternating magnetic field is 0.3T and the frequency is 30Hz.
[0033] Example 4 This embodiment provides a method for preparing a copper target, which differs from Embodiment 1 in that: In step (2), after the copper molten liquid is obtained, high-purity argon gas is not introduced into the furnace; that is, after the copper particles are completely melted to obtain copper molten liquid, the vacuum pump is turned off, the vacuuming is stopped, and the air inlet valve is opened to allow the outside air to slowly enter the furnace until the gas pressure in the furnace rises to atmospheric pressure.
[0034] Example 5 This embodiment provides a method for preparing a copper target, which differs from Embodiment 1 in that: In step (3), "120s" is used instead of "30s," meaning that the molten copper is poured into the furnace 120 seconds after the vacuum melting process ends.
[0035] Example 6 This comparative example provides a method for preparing a copper target, which differs from Example 1 in that: In step (3), the strength of the alternating magnetic field is 0.3T and the frequency is 50Hz.
[0036] Comparative Example 1 This comparative example provides a method for preparing a copper target, which differs from Example 1 in that: In step (3), "centrifugal casting" is used instead of "magnetic field-assisted variable speed centrifugal casting", that is, the centrifugal speed is kept constant throughout the process and no alternating magnetic field is applied, as follows: Within 30 seconds after vacuum melting, the molten copper is poured into a casting mold that has been preheated to 250°C and is rotating at 3000 r / min through a flow guide device. At the same time, the circulating cooling water system of the centrifugal casting machine is turned on, and the cooling water temperature is controlled at 25°C and the flow rate is 1.5 L / min. After pouring, the rotation speed and circulating cooling water are kept constant, and the machine continues to rotate for 14 minutes to allow the molten copper to solidify completely. After molding, the centrifugal casting machine and circulating cooling water are stopped in sequence, and the casting is demolded after cooling to room temperature in the furnace to obtain a copper billet with a wall thickness of 65 mm.
[0037] Comparative Example 2 This comparative example provides a method for preparing a copper target, which differs from Example 1 in that: In step (3), "magnetic field-assisted centrifugal casting" is used instead of "magnetic field-assisted variable speed centrifugal casting", that is, the centrifugal speed is kept constant throughout the process, as follows: Within 30 seconds of vacuum melting, molten copper is poured into a preheated casting mold (250°C, rotating at 1500 rpm) using a guide device. Simultaneously, the centrifugal casting machine's circulating cooling water system is activated, maintaining a temperature of 25°C and a flow rate of 1.5 L / min. During pouring, an alternating magnetic field is applied via a generator located around the mold's periphery. After pouring, the alternating magnetic field, rotation speed, and circulating cooling water are maintained constant, and the mold continues to rotate for 14 minutes to allow complete solidification. After molding, the centrifugal casting machine and circulating cooling water are stopped sequentially. The mold is then demolded after cooling to room temperature, yielding a 65 mm thick copper billet. The alternating magnetic field strength is 0.3 T, and the frequency is 20 Hz.
[0038] Comparative Example 3 This comparative example provides a method for preparing a copper target, which differs from Example 1 in that: In step (3), "variable speed centrifugal casting" is used instead of "magnetic field-assisted variable speed centrifugal casting", that is, no alternating magnetic field is applied during the entire molding process, as follows: Within 30 seconds after vacuum melting, molten copper is poured into a preheated casting mold at 250°C and rotating at 1500 r / min using a guide device. Simultaneously, the circulating cooling water system of the variable speed centrifugal casting machine is activated, controlling the circulating cooling water temperature at 25°C and the flow rate at 1.5 L / min. After pouring, the machine is accelerated at 250 r / min. 2 Increase the rotation speed of the casting mold; when the speed reaches 4500 r / min, stop accelerating and continue rotating at 4500 r / min for 2 minutes to allow the copper molten metal to completely solidify. After the molding is completed, stop the variable speed centrifugal casting machine and the circulating cooling water in sequence. After cooling to room temperature with the furnace, demold to obtain a copper billet with a wall thickness of 65 mm.
[0039] Relevant performance test analysis: 1. The average grain size and maximum grain size of the copper targets prepared in Examples 1-6 and Comparative Examples 1-3 were measured using a metallographic microscope. The test results are as follows: Figures 2-10 As shown.
[0040] 2. After encapsulating the copper targets prepared in Examples 1-6 and Comparative Examples 1-3 respectively, the actual density of each copper target was tested using the Archimedes density test method. The relative density was calculated as follows: relative density = actual density / theoretical density × 100%; 3. The oxygen content of the copper targets prepared in Examples 1-6 and Comparative Examples 1-3 was tested using an oxygen-nitrogen analyzer. The test results are shown in Table 1 below: Table 1 From Table 1 and Figures 2-10 It can be seen that the copper targets prepared in Examples 1-3 have high density, low oxygen content, fine and uniform grains with a maximum grain size of less than 30 μm. This is mainly due to the fact that in Example 1, after vacuum melting, inert gas protection was introduced, and variable speed centrifugal casting was performed 30 seconds after melting, while an alternating magnetic field was applied. Vacuum melting and inert gas protection deeply purified the copper solution and prevented the copper melt from oxidizing. In the early stage of casting, low-speed rotation and the application of an alternating magnetic field achieved stable filling, uniform temperature field, and dispersed nucleation particles. During the acceleration period, strong centrifugal force and Lorentz force worked together to break dendrites, increase the nucleation rate, refine the grains, and continuously press the copper melt into the dendrite gaps to achieve strong feeding, reduce shrinkage porosity and increase density. In the later stage of solidification, the alternating electric field was stopped to prevent the separated inclusions from being stirred back into the melt. High centrifugal force achieved strong feeding, further reducing defects such as shrinkage porosity and making the ingot structure highly dense.
[0041] The density, oxygen content, average grain size, and maximum grain size of the copper target material prepared in Example 4 were significantly worse than those in Example 1. The main reason is that in Example 4, inert gas was not introduced into the furnace for protection in the later stage of smelting. Instead, air was introduced to restore atmospheric pressure, which caused the copper molten metal to oxidize when it came into contact with air before being poured out of the furnace. This increased the oxygen content, which in turn formed oxide inclusions and hindered grain refinement, thus affecting the decrease in density.
[0042] The density, oxygen content, average grain size, and maximum grain size of the copper target material prepared in Example 5 were slightly worse than those in Example 1. The main reason is that in Example 5, casting was carried out 120 seconds after the smelting was completed, which prolonged the contact time between the copper melt and the air, causing the melt to absorb air and oxidize, thus increasing the oxygen content and affecting the density and grain uniformity of the copper billet.
[0043] The density, oxygen content, average grain size, and maximum grain size of the copper target material prepared in Example 6 were significantly worse than those in Example 1. The main reason is that Example 6 used a 50Hz high-frequency alternating magnetic field. Since copper is an ultra-high conductivity material, the skin depth of the high-frequency alternating magnetic field is shallow and does not meet the requirement of ≥0.8 times the wall thickness of the cast billet. As a result, the alternating magnetic field cannot effectively penetrate to the core of the copper cast billet, resulting in a lack of electromagnetic stirring effect in the core. This reduces the overall grain refinement effect and also affects the density and oxygen content of the copper cast billet.
[0044] The density, oxygen content, average grain size, and maximum grain size of the copper target material prepared in Comparative Example 1 were significantly worse than those in Example 1. The main reason is that Comparative Example 1 used a constant rotation speed and did not apply an alternating magnetic field during the forming process. It lacked the forced convection of the melt and the dendrite breaking effect of electromagnetic stirring. It also lacked the strong centrifugal force generated by variable speed centrifugation to strongly compensate for shrinkage and refine the grains. At the same time, the melt convection and degassing effect was weak. As a result, the grains were coarse and uneven, with many shrinkage cavities, low density, and high oxygen content.
[0045] The density, oxygen content, average grain size, and maximum grain size of the copper target material prepared in Comparative Example 2 were significantly worse than those in Example 1. The main reason is that Comparative Example 2 maintained a constant rotation speed throughout the molding process and failed to gradually increase the rotation speed during the solidification period to break up the growing dendrites, increase the nucleation rate, and refine the grains. It also failed to establish a strong centrifugal force in the later stage of solidification to continuously press the copper melt into the micro-shrinkage zone between the dendrites, resulting in insufficient strong feeding and the inability to provide sufficient shear force to break the dendrites in conjunction with electromagnetic stirring, resulting in coarse grains, which also affected the density and oxygen content.
[0046] The density, oxygen content, average grain size and maximum grain size of the copper target material prepared in Comparative Example 3 were significantly worse than those in Example 1. The main reason is that no alternating magnetic field was applied during the molding process of Comparative Example 3, and the electromagnetic stirring driven by Lorentz force was missing. This could not promote the uniformity of the temperature field and break up the dendrites at the solidification front in advance, resulting in a decrease in nucleation rate, coarser grains, and a weakening of melt convection and degassing effect, as well as an increase in oxygen content and a decrease in density.
[0047] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A method for preparing a copper target, characterized in that, Includes the following steps: The copper raw material is subjected to pretreatment and vacuum melting in sequence to obtain copper molten liquid; The molten copper is poured into a casting mold for variable speed centrifugal casting. An alternating magnetic field is applied during the variable speed centrifugal casting process to electromagnetically stir the liquid and semi-solid copper melt in the casting mold. After the casting is completed, the mixture is cooled and demolded to obtain a copper billet. The copper billet is annealed and precision machined in sequence to obtain a copper target material.
2. The preparation method according to claim 1, characterized in that, The steps of pouring the molten copper into a casting mold for variable-speed centrifugal casting, and applying an alternating magnetic field during the variable-speed centrifugal casting process include: Within 30 seconds after the vacuum melting process is completed, the molten copper is poured into a casting mold that has been preheated to 200~300℃ and is rotating at a speed of 1000~2000r / min, while an alternating magnetic field is applied. After pouring is complete, begin accelerating at 200~300 r / min. 2 Increase the rotational speed of the casting mold and maintain the applied alternating magnetic field during the acceleration process; When the rotational speed reaches 4000~5000 r / min, stop applying the alternating magnetic field and stop accelerating, and continue rotating at 4000~5000 r / min for 1~3 minutes.
3. The preparation method according to claim 2, characterized in that, During the variable speed centrifugal casting process, the temperature of the circulating cooling water is controlled at 20~30℃ and the flow rate is 1~2L / min.
4. The preparation method according to claim 1, characterized in that, The alternating magnetic field has an intensity of 0.1~0.5T and a frequency of 10~30Hz; And / or, the wall thickness of the copper casting is 50~80mm.
5. The preparation method according to claim 1, characterized in that, The pretreatment step includes drying the copper raw material under vacuum of ≤10Pa and temperature of 120~180℃ for 2~4 hours.
6. The preparation method according to claim 1, characterized in that, The vacuum melting process includes: melting the pretreated copper raw material under vacuum conditions ≤5Pa and temperature conditions of 1100~1200℃ for 30~60min; then, introducing inert gas into the furnace at a flow rate of 0.5~1.5L / min to raise the furnace pressure to atmospheric pressure, and then continuing to hold the temperature for 5~30min.
7. The preparation method according to claim 1, characterized in that, The annealing temperature is 300~500℃, and the holding time is 2~4h.
8. The preparation method according to claim 1, characterized in that, The purity of the copper raw material is ≥99.99%.
9. The preparation method according to claim 1, characterized in that, The copper target material has a purity of ≥99.99%, a grain size of ≤30μm, a density of ≥99.8%, and an oxygen content of ≤5ppm.
10. A copper target material, characterized in that, The copper target is prepared by the method for preparing the copper target according to any one of claims 1 to 9.