Amorphous al2o3 / si compound layered composite coating and preparation and application thereof
By preparing an amorphous Al₂O₃/Si compound layered composite coating on a metal substrate, the chemical inertness of silicon-based materials is used to form a physical barrier, which solves the problems of structural stability and hydrogen barrier performance of existing coatings under high-temperature lithium salt corrosion environment, and achieves a synergistic improvement in the coating's corrosion resistance and hydrogen barrier performance.
Patent Information
- Application Number
- CN202611270450.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-20
AI Technical Summary
Existing hydrogen-barrier/deuterium/tritium coatings exhibit poor structural stability in high-temperature, highly corrosive environments, failing to effectively resist the erosion of active lithium salts, leading to changes in coating structure and a decline in hydrogen-barrier performance.
An amorphous Al₂O₃/Si compound layered composite coating is adopted, including an amorphous Al₂O₃ intermediate layer and an amorphous Si compound surface layer. By preparing an amorphous Al₂O₃ intermediate layer on the surface of a metal substrate and forming an amorphous Si compound surface layer thereon, the chemical inertness of silicon-based materials is used to form a dense physical barrier, blocking the penetration path of corrosive media.
It significantly improves the coating's corrosion resistance and hydrogen barrier properties, maintains structural stability, prevents active lithium erosion and coating peeling, and ensures long-term service reliability in extreme environments.
Smart Images

Figure CN123132822A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of nuclear energy and hydrogen energy surface engineering technology, and in particular to an amorphous Al2O3 / Si compound layered composite coating and its preparation and application. Background Technology
[0002] With the profound transformation of the global energy structure, hydrogen energy development and controlled nuclear fusion energy utilization have become important solutions for humanity to address the energy crisis and achieve sustainable development. In nuclear fusion reactors (such as ITER or CFETR), fission reactors, and various advanced power systems, structural materials must operate for extended periods in extreme multi-field coupling environments characterized by ultra-high temperatures, strong radiation, and high chemical reactivity. Particularly in the tritium breeding blanket of fusion reactors, the solid tritium breeder Li4SiO4 releases highly chemically reactive lithium (Li) during high-temperature operation, posing a severe corrosion challenge to the structural materials. Furthermore, in hydrogen energy storage and transportation, spacecraft thermal control components, and semiconductor manufacturing processes, material surfaces also face the common challenge of high-temperature atmosphere corrosion and synergistic damage from complex chemical media.
[0003] To effectively suppress the penetration and diffusion of hydrogen and its isotopes (deuterium and tritium) within materials, the industry commonly employs a method of preparing hydrogen / deuterium / tritium barrier coatings on the substrate surface. High-performance hydrogen / deuterium / tritium barrier coatings can provide extremely high hydrogen isotope penetration reduction factors (PRF) in their initial state, serving as a core barrier to ensure the safe operation of the system. However, experimental studies and service monitoring have revealed that the structural stability of existing hydrogen / deuterium / tritium barrier coatings faces significant challenges when exposed to high-temperature, highly corrosive media (especially active lithium salts). For example, in the tritium breeder blanket of a fusion reactor, the compatibility of the solid tritium breeder with the structural materials is a key factor determining the service life of the structural materials. Research indicates that the active Li released by the tritium breeder... + In high-temperature environments, it can chemically react with the coating, causing changes in the coating structure. Currently, most existing surface treatment processes focus on improving hydrogen barrier efficiency in the initial state, while seriously neglecting long-term service reliability in complex chemical corrosion environments.
[0004] Developing a corrosion-resistant surface treatment process that can maintain high hydrogen barrier performance, effectively resist the penetration of strong chemical media, and maintain structural integrity in extreme environments has become a key challenge in ensuring the safe operation of major energy equipment. Therefore, it is essential to develop composite coatings that combine corrosion resistance with hydrogen / deuterium / tritium barrier properties. Summary of the Invention
[0005] In view of this, this application provides an amorphous Al2O3 / Si compound layered composite coating and its preparation and application, in order to solve the problem of how to improve the hydrogen / deuterium / tritium barrier and corrosion resistance of metal coatings.
[0006] To achieve the above technical objectives, this application adopts the following technical solution: In a first aspect, this application provides an amorphous Al2O3 / Si compound layered composite coating, comprising an amorphous Al2O3 intermediate layer and an amorphous Si compound surface layer sequentially stacked on a metal substrate.
[0007] Preferably, the metal substrate includes one or more of carbon steel, stainless steel, or alloys.
[0008] Preferably, the amorphous Si compound surface layer includes one or more of the following: an amorphous silicon oxide layer, an amorphous silicon carbide layer, an amorphous silicon nitride layer, or an amorphous silicon-oxygen-carbon layer.
[0009] Preferably, the density of the amorphous Al2O3 intermediate layer is not less than 95%; the density of the amorphous Si compound surface layer is not less than 99%.
[0010] Preferably, the thickness of the amorphous Al2O3 intermediate layer is 2 μm; the thickness of the amorphous Si compound surface layer is 1 μm.
[0011] Secondly, this application provides a method for preparing an amorphous Al2O3 / Si compound layered composite coating, comprising the following steps: An amorphous Al2O3 intermediate layer was prepared on the surface of a smooth, crystalline metal substrate using a thin film preparation method. On the surface of the amorphous Al2O3 intermediate layer, an amorphous Si compound surface layer is formed by liquid phase coating, thus obtaining an amorphous Al2O3 / Si compound layered composite coating.
[0012] Preferably, the thin film preparation method includes one or more of magnetron sputtering, sol-gel method, plasma spraying method, and chemical vapor deposition method; the liquid phase coating method includes one or more of spin coating, dip coating, and spraying method.
[0013] Thirdly, this application provides an application of an amorphous Al2O3 / Si compound layered composite coating in hydrogen / deuterium / tritium barrier.
[0014] Preferably, the application temperature is ≥500℃.
[0015] Preferably, the environmental medium used includes lithium salts.
[0016] The beneficial effects of this application are as follows: This application utilizes the inherent chemical inertness of silicon-based materials to high-temperature active lithium to form a dense physical barrier band at the interface with the amorphous Al2O3 / Si compound layer. This effectively blocks the penetration path of the corrosive medium into the interior, inhibiting the erosion caused by active lithium from the source and suppressing the generation of failure products such as LiAlO2. It overcomes the problems of poor chemical stability, insufficient corrosion resistance, and structural peeling and significant decrease in hydrogen barrier performance caused by active lithium penetration of a single amorphous Al2O3 layer under high-temperature lithium salt corrosion conditions. This application achieves a significant improvement in the lithium salt corrosion resistance and chemical stability of the hydrogen barrier isotope coating. Attached Figure Description
[0017] To more clearly illustrate the technical solutions of this application, the accompanying drawings used in this application will be briefly described below. Obviously, the drawings described below are merely some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without any creative effort.
[0018] Figure 1 This is a structural diagram of the Al2O3-SiO2 composite coating in Example 1; Figure 2 SEM images of the Al2O3-SiO2 composite coating at different corrosion times in Example 1: (a), (a1) 48 hours; (b), (b1) 192 hours; (c), (c1) 384 hours; Figure 3 The deuterium permeation flux and its PRF of the Al2O3-SiO2 composite coating after different corrosion times in Example 1 are shown: (a) deuterium permeation flux; (b) PRF; Figure 4 The graph shows a comparison of the PRF performance of the Al2O3 coating with other coatings in Comparative Example 1. Figure 5 The diagram shows (a) the deuterium permeation current before corrosion and (b) the morphology after 48 hours of corrosion for the pure SiO2 coating in Comparative Example 2. Detailed Implementation
[0019] The embodiments of the technical solution of this application will be described in detail below. The following embodiments are only used to illustrate the technical solution of this application more clearly, and are therefore only examples, and should not be used to limit the scope of protection of this application.
[0020] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.
[0021] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a mutually exclusive, independent, or alternative embodiment. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0022] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. Additionally, the character "" in this document generally indicates that the preceding and following related objects have an "or" relationship.
[0023] Unless otherwise explicitly defined and specified herein, all technical and scientific terms used in this application shall have the generally accepted meanings understood by one of ordinary skill in the field of chemical and chemical materials technology (including but not limited to polymer chemistry, inorganic chemistry, organic synthesis, catalysis chemistry, materials processing, and chemical unit operations) based on their professional knowledge and conventional practice. The use of any terminology herein is intended to describe the specific embodiments of this application in the clearest and most accurate manner, so as to fully disclose the technical solution. Such use shall not in any way be construed as a limitation on the scope of the claims, nor does it imply the exclusion of equivalent technical solutions that could be reasonably known by one of skill in the art based on the concept of this application.
[0024] The terms "comprising," "including," "having," "containing," and any grammatical variations or similar expressions used in the specification and claims of this application are all open-ended and non-exhaustive descriptive terms. Their purpose is to explicitly describe the existence of technical features, components, steps, or parts, while explicitly allowing and covering the possibility that other features, components, steps, parts, or any combinations thereof not explicitly listed may exist or be added to the technical solution, as long as such additions do not destroy the integrity and inventiveness of the original technical solution.
[0025] When the terms "embodiments," "some embodiments," or "specific embodiments" are mentioned in the specification, they refer to examples that, in conjunction with the specific parameters, materials, steps, and results described in that section, constitute one or a group of examples for implementing the technical solutions of this application. These embodiments are used for full disclosure and illustrative purposes, not for exhaustive enumeration. Those skilled in the art should understand that, without departing from the overall inventive concept of this application, the various technical features disclosed in different embodiments can be combined, substituted, modified, or deleted to form other implementation methods that are not listed one by one in the specification but also fall within the protection scope of this application.
[0026] Unless otherwise expressly specified and limited, all terms related to chemical process operations, material preparation, processing and analytical testing involved in this application shall be interpreted in the broadest sense based on the conventional understanding of those skilled in the art.
[0027] Regarding performance testing and structural characterization, all testing and characterization methods involved in this application, unless otherwise specified, refer to conventional methods known in the art. Specific testing conditions may be selected and adjusted according to the sample properties and relevant national standards, international standards, or industry-standard methods. Test items may include mechanical properties (such as tensile, bending, and impact strength), thermal properties (such as DSC and TGA analysis), and chemical stability (such as solvent resistance and acid / alkali corrosion resistance). Structural characterization methods may include FT-IR, NMR, XRD, SEM, TEM, and BET. All test results should be understood as being within the allowable range of conventional experimental errors.
[0028] Regarding numerical values and ranges, all parameter ranges expressed in this application in the form of "from a certain value to a certain value" should be understood as explicitly disclosing the endpoints of the range, every specific numerical point between the endpoints, and all sub-ranges formed by any two numerical points within the range. For example, "30℃ to 80℃" discloses 30, 31, ..., 80℃, as well as sub-ranges such as 30-50℃, 45-70℃, etc. When a numerical value is preceded by "about," "approximately," or similar words, it indicates that the numerical value is allowed to have reasonable errors recognized in the art under the measurement or control conditions, which can generally be understood as the deviation allowed by relevant standards or a normal fluctuation range of ±5% or ±10%.
[0029] This application provides an amorphous Al2O3 / Si compound layered composite coating, comprising an amorphous Al2O3 intermediate layer and an amorphous Si compound surface layer sequentially stacked on a metal substrate.
[0030] This application introduces a high hydrogen-barrier amorphous Al2O3 interlayer on the surface of a metal substrate to block the penetration of hydrogen and its isotopes. A composite silicon-based functional surface layer with both high density and chemical inertness is then superimposed on top of the interlayer, effectively cutting off the penetration path of active lithium into the internal hydrogen-barrier layer. Specifically, the amorphous Al2O3 interlayer intrinsically traps hydrogen isotopes, reducing their penetration and diffusion. Meanwhile, the amorphous Si compound surface layer physically blocks direct contact between active lithium and the internal hydrogen-barrier layer, preventing the formation of lithium-containing corrosion products in the amorphous Al2O3 interlayer. This maintains the structural stability of the coating and its hydrogen and isotope penetration resistance under extreme environments. This coating not only achieves a synergistic enhancement of hydrogen isotope resistance and lithium salt corrosion resistance but also exhibits self-densification repair, strong chemical inertness, and compatibility with various oxides, providing a foundation for the long-life service of high-performance hydrogen / tritium protective materials in extreme environments.
[0031] In some embodiments, the metal substrate includes one or more of carbon steel, stainless steel, or alloys.
[0032] In some embodiments, the amorphous Si compound surface layer includes one or more of the following: an amorphous silicon oxide layer, an amorphous silicon carbide layer, an amorphous silicon nitride layer, or an amorphous silicon-oxygen-carbon layer.
[0033] In this embodiment, the silicon-based material is chemically inert to high-temperature active lithium, forming a dense physical barrier band at the interface, which effectively blocks the penetration path of the corrosive medium into the interior and inhibits the generation of failure products such as LiAlO2.
[0034] In some embodiments, the density of the amorphous Al2O3 intermediate layer is not less than 95%; the density of the amorphous Si compound surface layer is not less than 99%.
[0035] In some embodiments, the thickness of the amorphous Al2O3 intermediate layer is 2 μm; the thickness of the amorphous Si compound surface layer is 1 μm.
[0036] This application provides a method for preparing an amorphous Al2O3 / Si compound layered composite coating, comprising the following steps: An amorphous Al2O3 intermediate layer was prepared on the surface of a smooth, crystalline metal substrate using a thin film preparation method. On the surface of the amorphous Al2O3 intermediate layer, an amorphous Si compound surface layer is formed by liquid phase coating, thus obtaining an amorphous Al2O3 / Si compound layered composite coating.
[0037] This application first pre-treats the metal substrate, including grinding, polishing, ultrasonic cleaning, and drying. Anhydrous ethanol is used as the cleaning solution for ultrasonic cleaning. Then, a dense hydrogen-barrier (deuterium / tritium) intermediate layer is prepared. A silicon-based anti-corrosion surface layer is then superimposed on the surface of the hydrogen-barrier (deuterium / tritium) layer. The prepared amorphous Al2O3 / Si compound layered composite coating has high structural stability under extreme environments and possesses hydrogen-barrier and isotope penetration resistance.
[0038] In some embodiments, the thin film preparation method includes one or more of magnetron sputtering, sol-gel method, plasma spraying method, and chemical vapor deposition method; the liquid phase coating method includes one or more of spin coating, dip coating, and spraying.
[0039] This application provides an application of an amorphous Al2O3 / Si compound layered composite coating in hydrogen / deuterium / tritium barrier.
[0040] This application is applicable to various high-temperature and strong chemical corrosion service environments, including nuclear fusion reactors, fission reactors, nuclear fuel cycle systems, hydrogen and deuterium-tritium energy devices, spacecraft thermal control components, high-energy particle accelerators, advanced electronic devices, and semiconductor manufacturing. It is specifically designed to improve the corrosion resistance of metallic or non-metallic material surfaces and their hydrogen permeation barrier properties in corrosive environments.
[0041] In some embodiments, the application temperature is ≥500°C.
[0042] In some embodiments, the environmental medium used includes lithium salts, such as the solid tritium breeder Li4SiO4.
[0043] Under these conditions, when the amorphous Al2O3 / Si compound layered composite coating is etched for 10 days and then subjected to a hydrogen isotope permeation test at 500℃, its hydrogen isotope permeation inhibition factor (PRF) can reach the order of 10 to the power of 3.
[0044] The following specific embodiments further illustrate this solution.
[0045] Example 1 An amorphous Al2O3 / Si compound layered composite coating comprises an amorphous Al2O3 intermediate layer and an amorphous Si compound surface layer sequentially stacked on a metal substrate.
[0046] A method for preparing an amorphous Al2O3 / Si compound layered composite coating includes the following steps: 321 stainless steel was selected as the base material. The 321 stainless steel base was progressively ground and polished using sandpaper of different grits from 400# to 2000# to ensure a smooth and flat surface, removing the oxide layer and oil stains. The treated metal base was then placed in anhydrous ethanol and ultrasonically treated in an ultrasonic cleaner for 10 minutes, ensuring complete removal of contaminants and fine particles from the base surface. After ultrasonic cleaning, the base was dried at 60℃ to ensure no moisture residue remained on the base surface. Aluminum isopropoxide was added to deionized water and heated in a water bath to prepare a 10% precursor solution. The solution was heated and stirred until a clear and transparent Al2O3 sol was obtained. A coating was prepared by spin coating. The spin-coated sample was dried on a heating plate at 200 °C to remove the solvent and form a gel film. Finally, it was heat-treated at 700 °C to prepare a 2 μm thick Al2O3 oxide hydrogen barrier (deuterium / tritium) coating with a density of 95% on the substrate surface, which is the Al2O3 intermediate layer. A 10% silicone resin precursor solution was prepared. The substrate with the hydrogen barrier (deuterium / tritium) coating was placed on a spin coater, and the silicone resin was evenly spread on the substrate surface. The spin coater was rotated at 3000 rpm to evenly coat the Al2O3 coating surface. The wet film sample was placed in a muffle furnace and heat-treated at 550℃ for 1 hour. The silicone resin was transformed into an amorphous SiO2 protective layer through dehydrogenation and decarburization reactions, thus obtaining an amorphous Al2O3 / Si compound layered composite coating.
[0047] Example 2 An amorphous Al2O3 / Si compound layered composite coating comprises an amorphous Al2O3 intermediate layer and an amorphous Si compound surface layer sequentially stacked on a metal substrate.
[0048] A method for preparing an amorphous Al2O3 / Si compound layered composite coating includes the following steps: 321 stainless steel was selected as the base material. The 321 stainless steel base was progressively ground and polished using sandpaper of different grits from 400# to 2000# to ensure a smooth and flat surface, removing the oxide layer and oil stains. The treated base was then placed in anhydrous ethanol and ultrasonically treated in an ultrasonic cleaner for 10 minutes, ensuring complete removal of contaminants and fine particles from the base surface. After ultrasonic cleaning, the base was dried at 60℃ to ensure no moisture residue remained on the surface. Aluminum isopropoxide was added to deionized water and heated in a water bath to prepare a 10% precursor solution. The solution was heated and stirred until a clear and transparent Al2O3 sol was obtained. The coating was prepared by the dip-coating method at a dip-coating speed of 300 μm / s. The dip-coated sample was dried on a heating plate at 200 °C to remove the solvent and form a gel film. Finally, it was heat-treated at 700 °C to prepare a 2 μm thick Al2O3 oxide hydrogen barrier (deuterium / tritium) coating with a density of 95% on the substrate surface, which is an amorphous Al2O3 intermediate layer. Using 10% polycarbosilane as a precursor, the substrate with the hydrogen barrier (deuterium / tritium) coating was placed on a spin coater, and the precursor solution was sprayed onto the surface of amorphous Al2O3 using a spraying process. The wet film sample was placed in a muffle furnace and heat-treated at 600℃ for 2 hours under argon protection to form a SiC protective layer, thus obtaining an amorphous Al2O3 / Si compound layered composite coating.
[0049] Comparative Example 1 A coating, otherwise identical to that of Example 1, except that it does not include an amorphous Si compound surface layer.
[0050] Comparative Example 2 A coating, otherwise identical to that in Example 1, except that it does not include an amorphous Al2O3 intermediate layer.
[0051] Testing and Evaluation The coatings obtained from different embodiments and comparative examples were subjected to corrosion tests in Li4SiO4 solid lithium salt at 550°C, and their hydrogen barrier isotope performance was tested after different corrosion times.
[0052] In Example 1, an Al2O3-SiO2 composite coating was constructed by using an Al2O3 coating obtained by heat treatment in an argon atmosphere as a hydrogen-barrier (deuterium / tritium) intermediate layer and a SiO2 coating as an anti-corrosion surface layer. The structural schematic diagram is shown below. Figure 1 As shown. The surface morphology after different etching times in Example 1 is as follows. Figure 2 As shown. By Figure 2 As can be seen from (a) and (a1) (a is high magnification, a1 is low magnification, the same below), after 48 hours of corrosion, the surface of the composite coating remains relatively intact and dense, with only a small number of fine particles and slight surface undulations; as the corrosion time is extended to 192 hours, as Figure 2 As shown in (b) and (b1), the overall structure of the coating remains continuous and dense, with no obvious through cracks or large-area peeling observed, indicating that the SiO2 anti-corrosion layer can effectively slow down the erosion of the internal Al2O3 tritium barrier layer by the corrosive medium; when the corrosion time is further extended to 384 hours, as Figure 2 As shown in (c) and (c1), although the surface roughness of the coating has increased and is accompanied by local particle agglomeration, the composite coating still maintains a relatively complete coverage structure, exhibiting good structural stability and corrosion resistance.
[0053] Deuterium permeation tests were performed on the coating samples from Example 1 at different corrosion times. The deuterium permeation performance results after different corrosion times are as follows: Figure 3 As shown. Among them, Figure 3 (a) shows the curve of deuterium permeation flux variation. Figure 3 (b) shows the corresponding PRF change results. Tables 1 and 2 below show the deuterium permeation flux and PRF results of the Al2O3-SiO2 composite coating in Example 1 at different corrosion times.
[0054] Table 1. Deuterium permeation flux (mol / m³) of the coating after different corrosion times in Example 1 -2 s -1 )
[0055] Table 2 PRF after different corrosion times of the coating in Example 1
[0056] It should be noted that 550℃ is the temperature for corrosion testing (early service stage), while the hydrogen isotope testing temperatures are 400 / 450℃ and 450℃ (later testing temperatures).
[0057] It can be seen that under the initial uncorroded condition at 500℃, the Al2O3-SiO2 layered composite coating exhibits a high PRF of 4710, demonstrating excellent hydrogen isotope blocking performance. With prolonged corrosion time, the deuterium permeation flux of the coating generally shows a gradual increasing trend, while the PRF gradually decreases, but the decrease is relatively limited. After 192 hours of corrosion, the composite coating still exhibits excellent performance, with a deuterium permeation flux of 1.4 × 10⁻⁶. -10 mol m -2 s -1 The corresponding PRF (Potential Resistance Factor) is 3235. This extremely high PRF value significantly outperforms the protective performance of conventional single hydrogen barrier coatings under the same high-temperature lithium salt environment. Conventional coatings often experience a precipitous drop in PRF when facing active lithium corrosion due to structural phase transformation. However, the Al2O3-SiO2 layered composite coating in Example 1 maintained a stable PRF of over 3000 after 192 hours of long-term extreme corrosion at a test temperature of 500°C, without experiencing catastrophic failure. This strongly demonstrates that the layered structure possesses extremely high hydrogen barrier efficiency and excellent service stability. Furthermore, even after 384 hours of corrosion, the coating still maintained a high barrier capacity, indicating its excellent long-term service stability. This further illustrates that SiO2 can, to a certain extent, prevent direct contact between the Li source and the Al2O3 coating, preventing the formation of Li-containing corrosion products, thus significantly enhancing the structural and performance stability of the coating.
[0058] Figure 4 The diagram shows a comparison of the PRF performance of the single-layer Al2O3 coating with other protective systems in Comparative Example 1. Experimental data show that, before the introduction of high-temperature lithium salt corrosion, this single Al2O3 coating exhibits extremely excellent intrinsic hydrogen isotope penetration barrier performance, with an initial PRF value as high as 4710. Figure 5 The images show (a) the deuterium permeation current before corrosion and (b) the morphology after 48 hours of corrosion for the pure SiO2 coating in Comparative Example 2. Figure 5 (a) As can be seen, due to the lack of a hydrogen-blocking intermediate layer, its PRF is only 800 at the test temperature of 500°C, which is far lower than the level of the layered composite structure in Example 1 of this invention. This indicates that the single SiO2 coating is insufficient in its hydrogen isotope blocking effect and cannot independently meet the high hydrogen-blocking requirements. However, due to Figure 5 (b) It can be seen that after 48 hours of corrosion, the surface of the SiO2 coating remains uniform and dense, without cracks or peeling, which confirms that silicon-based materials have excellent corrosion resistance to high-temperature lithium salts.
[0059] This application uses an amorphous Al2O3 material with high hydrogen permeation resistance as an intermediate layer to prevent hydrogen isotope diffusion and permeation. A chemically inert composite silicon compound is then deposited in situ on the surface of the intermediate layer as a top layer. The amorphous Al2O3 hydrogen-resistant intermediate layer reduces hydrogen isotope permeation and diffusion, while the surface silicon-based material's chemical inertness to lithium salts at high temperatures effectively blocks active lithium ions from penetrating into the inner hydrogen-resistant layer. This simultaneously achieves high hydrogen / deuterium / tritium resistance and high corrosion resistance. This novel layered composite structure, through the synergistic function of the outer corrosion-resistant layer and the inner hydrogen (deuterium / tritium) barrier, ensures that the coating system possesses both high hydrogen permeation resistance and structural integrity and efficient long-life operation under extreme multi-field coupling service environments. After ten days of lithium salt corrosion at 550°C, the amorphous Al2O3 / Si compound layered composite coating prepared in this invention still maintains a hydrogen isotope permeation inhibition factor (PRF) on the order of 10³. This coating improves the structural and performance stability of the material surface in corrosive environments and can be applied to hydrogen embrittlement protection in extreme environments such as nuclear energy and hydrogen energy.
[0060] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. An amorphous Al2O3 / Si compound layered composite coating, characterized in that, It includes an amorphous Al2O3 intermediate layer and an amorphous Si compound surface layer sequentially stacked on a metal substrate.
2. The amorphous Al2O3 / Si compound layered composite coating according to claim 1, characterized in that, The metal substrate includes one or more of carbon steel, stainless steel, or alloys.
3. The amorphous Al₂O₃ / Si compound layered composite coating according to claim 1, characterized in that, The amorphous Si compound surface layer includes one or more of the following: an amorphous silicon oxide layer, an amorphous silicon carbide layer, an amorphous silicon nitride layer, or an amorphous silicon-oxygen-carbon layer.
4. The amorphous Al₂O₃ / Si compound layered composite coating according to claim 1, characterized in that, The density of the amorphous Al2O3 intermediate layer is not less than 95%; the density of the amorphous Si compound surface layer is not less than 99%.
5. The amorphous Al₂O₃ / Si compound layered composite coating according to claim 1, characterized in that, The thickness of the amorphous Al2O3 intermediate layer is 2 μm; the thickness of the amorphous Si compound surface layer is 1 μm.
6. A method for preparing an amorphous Al2O3 / Si compound layered composite coating as described in any one of claims 1-5, characterized in that, Includes the following steps: An amorphous Al2O3 intermediate layer was prepared on the surface of a smooth, crystalline metal substrate using a thin film preparation method. On the surface of the amorphous Al2O3 intermediate layer, an amorphous Si compound surface layer is formed by liquid phase coating, thus obtaining the amorphous Al2O3 / Si compound layered composite coating.
7. The method for preparing the amorphous Al2O3 / Si compound layered composite coating according to claim 6, characterized in that, The thin film preparation method includes one or more of magnetron sputtering, sol-gel method, plasma spraying method, and chemical vapor deposition method; the liquid phase coating method includes one or more of spin coating, dip coating, and spraying method.
8. The application of an amorphous Al2O3 / Si compound layered composite coating as described in any one of claims 1-5 in hydrogen / deuterium / tritium barrier.
9. The application according to claim 8, characterized in that, The application temperature is ≥500℃.
10. The application according to claim 8, characterized in that, The environmental medium for this application includes lithium salts.