Apparatus, method for preparing aluminum oxide diffusion barrier layer of double-sided superconducting tape, and superconducting tape

By combining medium-frequency reactive sputtering and an oxygen reaction controller, double-sided synchronous sputtering and multiple flipping are achieved, solving the problems of unstable deposition rate and difficulty in double-sided preparation in alumina thin film preparation. This improves film uniformity and deposition efficiency, and is suitable for the industrial production of high-temperature superconducting tapes.

CN123132828APending Publication Date: 2026-11-20SONGSHAN LAKE MATERIALS LAB +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611610727.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In existing technologies, the preparation process window for alumina thin films is narrow, which easily leads to target poisoning, unstable deposition rates, and difficulties in preparing both sides, making it difficult to achieve efficient industrial production of double-sided superconducting tapes.

Method used

By combining a medium-frequency reactive sputtering device and an oxygen reaction controller, and by setting up a flipping component to make the substrate pass through the double-sided alumina diffusion barrier deposition area multiple times, and setting aluminum targets on both sides of the substrate as cathodes and anodes, and cooperating with the oxygen reaction controller to regulate the atmosphere, double-sided synchronous sputtering and multiple flipping are achieved, thereby improving the film growth efficiency.

Benefits of technology

This improved the deposition rate and uniformity of alumina films, reduced the surface roughness of the films, and met the industrial production requirements of high-temperature superconducting tapes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123132828A_ABST
    Figure CN123132828A_ABST
Patent Text Reader

Abstract

This application provides an apparatus, method, and superconducting tape for preparing an alumina diffusion barrier layer on a double-sided superconducting tape, relating to the field of superconducting tape technology. The method includes: a tape feeding device, several guiding components, a double-sided superconducting tape alumina diffusion barrier layer deposition area, and a tape receiving device. In the tape feeding device, the base tape is fed into the tape receiving device via several guiding components. The double-sided superconducting tape alumina diffusion barrier layer deposition area is located between the feeding device and the receiving device. The base tape passes through the double-sided superconducting tape alumina diffusion barrier layer deposition area 2n times. The several guiding components include m flipping components for flipping the base tape, where m = 2n - 1, and n is a non-zero natural number. The double-sided superconducting tape alumina diffusion barrier layer deposition area includes two aluminum targets, a mid-frequency reactive sputtering device, and an oxygen reaction controller. This application can improve the production efficiency and product quality of double-sided superconducting tapes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of superconducting tape technology, and in particular to an apparatus, method, and superconducting tape for preparing a double-sided superconducting tape alumina diffusion barrier layer. Background Technology

[0002] Second-generation high-temperature superconducting tapes using REBCO (Re being a rare earth element) as the superconducting layer material have shown great application potential in fields such as strong magnets, wind power generation, fault current limiters, and high-efficiency power transmission cables due to their excellent current-carrying performance under high fields and relatively low cost.

[0003] High-temperature superconducting tapes mainly consist of an alloy substrate, a diffusion barrier layer, a seed layer, a transition layer, a REBCO superconducting layer, and a protective layer (some institutions collectively refer to the diffusion barrier layer, seed layer, and transition layer as a buffer layer). The diffusion barrier layer prevents element diffusion between the nucleation layer and the alloy substrate. The material typically chosen is alumina, which possesses extremely high chemical stability, good insulation, and relatively low cost. Numerous studies have confirmed that dense, amorphous, or nanocrystalline alumina films can be fabricated on alloy substrates using magnetron sputtering. These films maintain their amorphous state even during subsequent high-temperature processing, effectively blocking element diffusion through the "maze effect."

[0004] However, this method also faces some challenges: First, the process window is narrow. Alumina is a typical ceramic insulating material, which is prone to "target poisoning" in DC reactive sputtering, resulting in unstable deposition rate, poor process repeatability, and many film defects. Second, double-sided preparation is difficult, which is a key bottleneck to achieve industrial roll-to-roll continuous production. Existing equipment and technologies are mostly focused on single-sided deposition.

[0005] CN209508401U uses a double-sided deposition method to prepare a buffer layer for high-temperature superconducting tapes, but it does not involve simultaneous sputtering on both sides. Sputtering each side separately would severely affect the uniformity of the film quality on both sides. CN102255040B uses a double-sided synchronous deposition method to prepare Y2O3. It utilizes a stepper motor to drive the baseband to move at a constant speed, combined with an argon-hydrogen and water vapor environment, to achieve off-axis sputtering deposition, ensuring double-sided consistency and high orientation. However, due to the thin yttrium oxide seed layer, a medium-frequency reactive magnetron sputtering process with a high sputtering rate was not used.

[0006] However, alumina thin films are difficult to prepare and the thickness requirement is usually between 50 and 80 nm. The radio frequency sputtering rate is low, and the thin films prepared by the single-pass method are relatively thin. It is necessary to take into account the needs of industrial production efficiency of high-temperature superconducting tapes. Summary of the Invention

[0007] To address the shortcomings of existing technologies, this application aims to provide an apparatus, method, and superconducting tape for preparing a double-sided superconducting tape alumina diffusion barrier layer. By incorporating a reversing component, the substrate can be rotated in both directions, allowing it to pass through the deposition region of the double-sided superconducting tape alumina diffusion barrier layer multiple times, thereby improving film growth efficiency. The deposition region of the double-sided superconducting tape alumina diffusion barrier layer uses a metallic aluminum target, and a combination of a mid-frequency reactive sputtering device and an oxygen reaction controller provides a highly stable and fast-responding alumina thin film process window.

[0008] To achieve this objective, the following technical solution is adopted in this application:

[0009] In a first aspect, this application provides an apparatus for preparing a double-sided superconducting tape alumina diffusion barrier layer, the apparatus comprising: a tape feeding device, several guiding components, a double-sided superconducting tape alumina diffusion barrier layer deposition zone, and a tape receiving device.

[0010] In the tape feeding device, the baseband is fed into the tape receiving device through several guiding components, and the double-sided superconducting tape alumina diffusion barrier deposition area is located between the tape feeding device and the tape receiving device.

[0011] The number of times the baseband passes through the alumina diffusion barrier layer deposition area of ​​the double-sided superconducting tape is 2n. The plurality of guiding components include a flipping component that flips the baseband m times, which is used to flip the baseband once after each passage through the alumina diffusion barrier layer deposition area of ​​the double-sided superconducting tape, where m=2n-1 and n is a natural number.

[0012] The double-sided superconducting tape alumina diffusion barrier layer deposition region includes two aluminum targets arranged opposite each other on both sides of the baseband. The aluminum targets are connected to a mid-frequency reactive sputtering device. The two aluminum targets alternately form cathodes and anodes at zero potential, which are used to generate an alumina diffusion barrier layer on the baseband surface under the action of the mid-frequency reactive sputtering device. It also includes an oxygen reaction controller for regulating the oxygen atmosphere in the double-sided superconducting tape alumina diffusion barrier layer deposition region.

[0013] In some technical solutions of this application, the preparation apparatus further includes a tension sensor and a tension adjustment component. The tension sensor is used to monitor the baseband tension during the baseband transport process and feed it back to the tension adjustment component. The tension adjustment component is used to adjust the baseband tension according to the baseband tension monitored by the tension sensor.

[0014] In some technical solutions of this application, the tension adjusting component includes an actuating component, which includes a magnetic powder brake and / or an independent motor as an auxiliary force to the tension adjusting wheel.

[0015] In some technical solutions of this application, the direction from the self-releasing tape device to the retracting tape device includes, in sequence, a tape-releasing guide wheel, a front guide component located before the alumina diffusion barrier layer deposition area of ​​the double-sided superconducting tape, a rear guide component located after the alumina diffusion barrier layer deposition area of ​​the double-sided superconducting tape, and a retracting guide wheel. The flipping component is located at the end of the rear guide component and / or the front end of the front guide component, and is used to flip the base tape.

[0016] In some technical solutions of this application, the front guide component has 2n sets of front guide paths arranged in parallel.

[0017] In some technical solutions of this application, the rear guide component has 2n sets of rear guide paths arranged in parallel.

[0018] In some technical solutions of this application, the tape feeding guide wheel and the tape take-up guide wheel are each independently equipped with a meter counting component. In some technical solutions of this application, the number of n is 1 to 4.

[0019] In some technical solutions of this application, the preparation apparatus further includes a baseband baking device, which is located before the deposition area of ​​the alumina diffusion barrier layer of the double-sided superconducting tape along the baseband conveying direction.

[0020] In some technical solutions of this application, the tape take-up device includes a tape take-up servo motor.

[0021] In some technical solutions of this application, the tape feeding device includes a tape feeding torque motor or a tape feeding servo motor.

[0022] In some technical solutions of this application, the oxygen reaction controller includes a voltage sensor for monitoring the target surface voltage; and an oxygen regulator for adjusting the oxygen flow rate according to the monitored target surface voltage.

[0023] In some technical solutions of this application, the preparation device further includes a chamber and a vacuum pumping device for evacuating the chamber, and the plurality of guiding components and the double-sided superconducting tape alumina diffusion barrier deposition area are all disposed in the chamber.

[0024] Secondly, this application provides a method for preparing an alumina diffusion barrier layer for double-sided superconducting tapes, wherein the preparation method is performed using the apparatus for preparing an alumina diffusion barrier layer for double-sided superconducting tapes described in the first aspect.

[0025] In some technical solutions of this application, the preparation method includes: the baseband is fed into the double-sided superconducting tape alumina diffusion barrier deposition area by a self-releasing device to perform the first double-sided alumina diffusion barrier deposition, and then the baseband is flipped m times. After each flip, it is fed back into the same double-sided superconducting tape alumina diffusion barrier deposition area to perform m double-sided alumina diffusion barrier depositions. The first double-sided alumina diffusion barrier deposition and the m double-sided alumina diffusion barrier depositions are performed simultaneously. After the deposition is completed, the baseband is fed into a tape-retrieving device for tape-retrieving.

[0026] In some technical solutions of this application, m is an odd number between 1 and 7.

[0027] In some technical solutions of this application, the preparation method further includes: real-time monitoring of the baseband tension, and adjusting the tension adjustment wheel using a magnetic powder brake and / or an independent motor according to the monitoring results, so as to adjust the baseband tension.

[0028] In some technical solutions of this application, the baseband transmission speed is 1~50mm / s.

[0029] In some technical solutions of this application, the baseband transmission speed is 5~20mm / s.

[0030] In some technical solutions of this application, the preparation method further includes baking the baseband before depositing the alumina diffusion barrier layer in the double-sided superconducting tape.

[0031] In some technical solutions of this application, the baking temperature is 150~200℃.

[0032] In some technical solutions of this application, the process before depositing the double-sided alumina diffusion barrier layer includes: pre-sputtering before the baseband is fed in, and then depositing the double-sided alumina diffusion barrier layer when the baseband is fed in.

[0033] In some technical solutions of this application, the pre-sputtering includes: first evacuating the chamber to 0.0001~0.001 Pa, then introducing a protective gas, and then turning on the medium-frequency reactive sputtering device to perform pre-sputtering to clean the oxide layer and impurities on the surface of the aluminum target.

[0034] In some technical solutions of this application, the protective gas includes argon.

[0035] In some technical solutions of this application, the pressure after the protective gas is introduced is 1~3 Pa.

[0036] In some technical solutions of this application, the pre-sputtering process parameters are the same as the sputtering parameters during the deposition of the double-sided alumina diffusion barrier layer.

[0037] In some technical solutions of this application, the pre-sputtering time is 3 to 10 minutes.

[0038] In some technical solutions of this application, the deposition of the double-sided alumina diffusion barrier layer includes: simultaneously turning on the intermediate frequency reactive sputtering device and the oxygen reaction controller, and sputtering and depositing an alumina film on the substrate surface that is being transported through the double-sided alumina diffusion barrier layer deposition area.

[0039] In some technical solutions of this application, the power of the sputtering deposition is 1~10kW.

[0040] In some technical solutions of this application, the current of sputtering deposition is 1~15A.

[0041] In some technical solutions of this application, the working pressure of sputtering deposition is 0.5~3.5 Pa.

[0042] In some technical solutions of this application, the flow rate ratio of argon to oxygen in the sputtering deposition is (0.5~1.5):1.

[0043] In some technical solutions of this application, the flow rate of argon gas in the sputtering deposition ranges from 0 to 200 sccm.

[0044] In some technical solutions of this application, the oxygen flow rate in the sputtering deposition ranges from 0 to 200 sccm.

[0045] In some technical solutions of this application, the target surface voltage is monitored during the sputtering deposition process; then, the oxygen flow rate is adjusted by an oxygen regulator based on the monitored target surface voltage.

[0046] Thirdly, this application provides a superconducting tape, the superconducting tape comprising a base tape and an alumina diffusion barrier layer disposed on two surfaces of the base tape; the absolute value of the thickness difference between the alumina diffusion barrier layers on both sides of the base tape is ≤2nm, and / or the absolute value of the roughness Rq difference between the alumina diffusion barrier layers on both sides of the base tape in a 5*5μm2 sampling area is ≤0.7nm.

[0047] In some technical solutions of this application, the baseband includes a Hastelloy baseband.

[0048] In some technical solutions of this application, the thickness of the alumina diffusion barrier layer on one side is 25~100nm.

[0049] In some technical solutions of this application, the roughness Rq of the single-sided alumina diffusion barrier layer is 0.5~3.0nm in a sampling area of ​​5*5μm2.

[0050] In some technical solutions of this application, the absolute value of the difference in thickness between the alumina diffusion barrier layers on both sides of the baseband is ≤1nm.

[0051] In some technical solutions of this application, the absolute value of the difference in roughness Rq between the alumina diffusion barrier layers on both sides of the baseband under a sampling area of ​​5*5μm2 is ≤0.1nm.

[0052] Compared with the prior art, this application has at least the following beneficial effects:

[0053] (1) The apparatus and method for preparing double-sided superconducting tape alumina diffusion barrier layer provided in this application can simultaneously achieve double-sided sputtering (meaning that both sides of the same tape are sputtered synchronously during a single tape-carrying process) + multiple sputtering of the tape + reversal of the sputtering faces after flipping, thereby improving the uniformity of the two sides of the tape; multiple flipping of the tape can increase the tape-carrying rate several times, thereby reducing the temperature rise of the tape surface, thus reducing the roughness of the alumina film surface, and providing a good template for the subsequent growth of the texture layer.

[0054] (2) The apparatus and method for preparing the alumina diffusion barrier layer of the double-sided superconducting tape provided in this application adopts a scheme that combines medium-frequency reactive sputtering with an oxygen reaction controller to regulate the target surface voltage and optimize the ratio of oxide deposition to metal deposition. This scheme is beneficial for controlling the composition of the alumina film and can increase the deposition rate of the film on the substrate surface by one or even several times, thus enabling the industrial-grade production of double-sided superconducting tape. Attached Figure Description

[0055] Figure 1 This is a schematic diagram of the apparatus for preparing the double-sided superconducting tape alumina diffusion barrier layer provided in Embodiment 1 of this application.

[0056] Figure 2 This is a schematic diagram of the apparatus for preparing the double-sided superconducting tape alumina diffusion barrier layer provided in Embodiment 2 of this application.

[0057] In the figure: 1. Tape feeding device; 2. Base tape; 3. Tape feeding guide wheel; 4. Baking device guide wheel; 5. Base tape baking device; 6. First front guide wheel; 7. Deposition area of ​​alumina diffusion barrier layer of double-sided superconducting tape; 8. First rear guide wheel; 9. Second rear guide wheel; 10. Tilting wheel; 11. Tape take-up guide wheel; 12. Tape take-up device. Detailed Implementation

[0058] To facilitate understanding of this application, the following embodiments are provided. Those skilled in the art should understand that these embodiments are merely illustrative and should not be construed as limiting the scope of this application.

[0059] It should be understood that in the description of this application, the terms "center," "longitudinal," "lateral," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. These terms are used solely for the convenience of describing this application and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application. Furthermore, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined with "first," "second," etc., may explicitly or implicitly include one or more of that feature. In the description of this application, unless otherwise stated, "a plurality of" means two or more.

[0060] It should be noted that, in the description of this application, unless otherwise expressly specified and limited, the terms "set up," "connected," and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this application based on the specific circumstances.

[0061] Those skilled in the art should understand that this application necessarily includes the necessary pipelines, conventional valves and general pump equipment for achieving process integrity, but the above content is not the main inventive point of this application. Those skilled in the art can add layouts based on the process flow and equipment structure selection. This application does not make any special requirements or specific limitations in this regard.

[0062] The technologies for achieving double-sided coating of superconducting basebands can be broadly classified into two categories: two-pass single-sided deposition and double-sided simultaneous deposition.

[0063] (1) Two-pass single-sided deposition refers to the substrate passing through the coating system once to complete the deposition of the first side; then the substrate passes through the same coating system a second time to complete the deposition of the second side by switching the side sequence through the take-up and unwinding system. This technology is simple and convenient to operate, requiring only one set of sputtering target material, but it also has certain limitations. First, the total deposition length is doubled, and the production efficiency is halved; second, due to the fluctuation of the process during sputtering, it is difficult to ensure that the process parameters (such as vacuum degree, temperature, plasma state) during the two depositions are completely consistent, which ultimately leads to differences in the film performance and thickness of the two sides of the substrate; moreover, during the take-up and unwinding process after the first deposition, the coated first side may rub against the guide roller or other contact surfaces, causing contamination or damage.

[0064] (2) Double-sided synchronous deposition refers to the symmetrical arrangement of two sputtering targets (top and bottom or left and right) in a vacuum chamber, with the substrate passing through the middle, thereby achieving double-sided synchronous deposition. The advantage of this method is that it can significantly improve production efficiency and film thickness consistency. The disadvantage is that the plasma will interfere with each other. When the two sputtering sources work simultaneously in a small space, their plasma regions will overlap and couple, leading to unstable discharge, which will aggravate the target poisoning phenomenon and make the process uncontrollable. In addition, even if the two coating systems are exactly the same, there will inevitably be some differences (power supply, process gas flow rate, etc.), making it difficult to achieve complete consistency of the double-sided film. In addition, in terms of target selection and sputtering method, the use of alumina target requires the use of magnetron radio frequency sputtering process. The alumina film prepared by this method has a low growth rate, which is not conducive to industrial production. The use of metallic aluminum target usually adopts magnetron DC reactive sputtering process. Although this method can greatly improve the sputtering rate, it cannot guarantee the complete oxidation state of the alumina film. The presence of metallic aluminum impurities will seriously affect the anti-diffusion effect of the alumina layer, and the target surface is prone to poisoning, which seriously affects the stability of long strip preparation.

[0065] In this regard, as a specific embodiment of this application, a fabrication apparatus for a double-sided superconducting tape alumina diffusion barrier layer is provided. The fabrication apparatus includes: a tape feeding device, several guiding components, a double-sided superconducting tape alumina diffusion barrier layer deposition area, and a tape receiving device.

[0066] In the tape feeding device, the baseband is fed into the tape receiving device through several guiding components, and the double-sided superconducting tape alumina diffusion barrier deposition area is located between the tape feeding device and the tape receiving device.

[0067] The number of times the baseband passes through the alumina diffusion barrier layer deposition area of ​​the double-sided superconducting tape is 2n. The plurality of guiding components include a flipping component that flips the baseband m times, which is used to flip the baseband once after each passage through the alumina diffusion barrier layer deposition area of ​​the double-sided superconducting tape, where m=2n-1 and n is a natural number.

[0068] The double-sided superconducting tape alumina diffusion barrier layer deposition region includes two aluminum targets arranged opposite each other on both sides of the baseband. The aluminum targets are connected to a mid-frequency reactive sputtering device. The two aluminum targets alternately form cathodes and anodes at zero potential, which are used to generate an alumina diffusion barrier layer on the baseband surface under the action of the mid-frequency reactive sputtering device. It also includes an oxygen reaction controller for regulating the oxygen atmosphere in the double-sided superconducting tape alumina diffusion barrier layer deposition region.

[0069] Those skilled in the art will know that the zero potential is generally ground.

[0070] The apparatus for preparing the double-sided superconducting tape alumina diffusion barrier layer provided in this application has the following ingenious design:

[0071] A. This application does not use an alumina target, but instead uses an aluminum target, and is equipped with an oxygen reaction controller, thereby enabling high-speed deposition of alumina on the substrate surface, solving the problem of high surface roughness caused by excessively high temperature during the deposition process when a thick alumina diffusion barrier layer needs to be deposited on the substrate surface.

[0072] B. This application adopts a simultaneous double-sided + multiple deposition method, that is, the substrate is deposited on both sides and multiple segments at the same time, and after each delivery into the double-sided superconducting tape alumina diffusion barrier deposition area, it is flipped once. This can improve the film growth rate and reduce the temperature rise of the tape surface, thereby reducing the roughness of the alumina film surface. On the other hand, it can significantly improve the uniformity of the double sides of the tape.

[0073] C. This application uses a medium-frequency reactive sputtering device and sets up a pair of aluminum targets for sputtering. The two aluminum targets alternately form the cathode and anode at zero potential, which can reduce the problem of unevenness of the double-sided film and solve the problem of unstable discharge.

[0074] In some specific embodiments, the preparation apparatus further includes a tension sensor and a tension adjustment component. The tension sensor monitors the baseband tension during the baseband transport process and feeds it back to the tension adjustment component. The tension adjustment component adjusts the baseband tension based on the baseband tension monitored by the tension sensor.

[0075] When the belt speed is increased, problems such as unstable belt feeding and excessive base belt tension leading to belt breakage may occur. This application addresses these issues by setting up a tension sensor and a tension adjustment component. Tension feedback adjustment is achieved by using servo motors for the unloading and take-up rollers, adding tension wheels at the belt outlet of the unloading device and the inlet of the take-up device, and adjusting the magnetic powder.

[0076] In some specific embodiments, the tension adjusting component includes an actuating component, which includes a magnetic powder brake and / or an independent motor as an auxiliary force to the tension adjusting wheel.

[0077] In some specific embodiments, in the direction from the tape feeding device to the tape take-up device, the plurality of guiding components sequentially include a tape feeding guide wheel, a front guide component located before the alumina diffusion barrier layer deposition area of ​​the double-sided superconducting tape, a rear guide component located after the alumina diffusion barrier layer deposition area of ​​the double-sided superconducting tape, and a tape take-up guide wheel. The flipping component is located at the end of the rear guide component and / or the front end of the front guide component, and is used to flip the base tape.

[0078] In this application, the guide wheel serves to guide, adjust, and constrain the movement direction of the superconducting tape, ensuring that the superconducting tape maintains tension and runs stably along a predetermined path, while also distributing the load and reducing single-point stress.

[0079] In some specific embodiments, the front guide component has 2n sets of front guide paths arranged in parallel.

[0080] In this application, the front guide path can be a front guide path composed of 2n sets of front guide wheels arranged in parallel, or it can be composed of several sets of front guide wheels arranged in parallel. Each front guide wheel can be provided with multiple guide grooves, thereby forming 2n sets of front guide paths arranged in parallel.

[0081] In some specific embodiments, the rear guide component includes 2n sets of rear guide paths arranged in parallel.

[0082] In this application, the rear guide path can be composed of 2n sets of rear guide wheels arranged in parallel, or it can be composed of several sets of rear guide wheels arranged in parallel. Each rear guide wheel can be provided with multiple guide grooves, thereby forming 2n sets of rear guide paths arranged in parallel.

[0083] This application does not have any special requirements on the number of guide wheels in the front guide wheel path and the rear guide wheel path, but the specific requirement is to achieve effective baseband delivery.

[0084] In some specific embodiments, the unloading guide wheel and the take-up guide wheel are each independently equipped with a meter-counting component. This component is typically located on the take-up guide wheel. It can monitor and record the length of the tape with the prepared alumina diffusion barrier layer in real time.

[0085] In some specific implementations, the number of n is 1 to 4, for example, it can be 1, 2, 3 or 4.

[0086] This application allows for 2-pass, 4-pass, 6-pass, or 8-pass deposition, meaning the substrate passes through the deposition zone 2, 4, 6, or 8 times consecutively in a single experiment. Theoretically, this increases the film deposition rate on the substrate by 100%, 300%, 500%, or 700%, respectively. Furthermore, the higher transport rate significantly shortens the substrate's dwell time in the deposition zone per pass, resulting in lower temperature rise on the substrate, which is more conducive to the growth of amorphous alumina and lower surface roughness. The increased transport rate also facilitates the preparation of amorphous alumina layers with superior performance at lower temperatures.

[0087] In some specific embodiments, the flipping component includes m flipping wheels, or the flipping component includes m flipping guide grooves, or the flipping component includes several flipping wheels, each flipping wheel having several flipping guide grooves, so that the baseband can be flipped m times in total.

[0088] In some specific embodiments, the preparation apparatus further includes a baseband baking device, which is positioned before the deposition area of ​​the alumina barrier diffusion layer of the double-sided superconducting tape along the baseband conveying direction.

[0089] This application includes a baseband baking device, which can remove moisture and gas adsorbed in the baseband.

[0090] In some specific embodiments, the baseband baking device is equipped with a heating resistance wire.

[0091] In some specific embodiments, the take-up device includes a take-up servo motor.

[0092] In some specific embodiments, the tape feeding device includes a tape feeding torque motor or a tape feeding servo motor.

[0093] This ensures that the tension of the superconducting tape is moderate and continuously adjustable during the preparation process, avoiding tape curling or breakage failure.

[0094] In some embodiments, the oxygen reaction controller includes a voltage sensor for monitoring target surface voltage and an oxygen regulator for adjusting the oxygen flow rate based on the monitored target surface voltage.

[0095] This application utilizes an oxygen reaction controller to regulate the reaction state on the surface of an aluminum target, enabling the deposition of an alumina film on the substrate as it passes through the thin film deposition zone. Generally, the oxygen reaction controller incorporates a voltage sensor as a feedback signal and uses a PID controller to control the start and stop of the oxygen flow meter, dynamically adjusting the surface state of the aluminum target from an oxygen-rich or oxygen-deficient state to a low-oxygen state and maintaining it within this ideal window. The feedback delay and the type of intelligent algorithm can be optimized and adjusted according to the actual needs of the field, and will not be elaborated further here.

[0096] In some specific embodiments, the preparation apparatus further includes a chamber and a vacuum pumping device for evacuating the chamber, wherein the plurality of guiding components and the double-sided superconducting tape alumina diffusion barrier deposition area are all disposed within the chamber.

[0097] As a specific embodiment of this application, a method for preparing an alumina diffusion barrier layer for a double-sided superconducting tape is provided, wherein the preparation method is performed using the apparatus for preparing an alumina diffusion barrier layer for a double-sided superconducting tape described in the first aspect.

[0098] In some specific embodiments, the preparation method includes: the baseband is fed into the double-sided superconducting tape alumina diffusion barrier deposition area by a self-releasing device to perform the first double-sided alumina diffusion barrier deposition, and then the baseband is flipped m times. After each flip, it is fed back into the same double-sided superconducting tape alumina diffusion barrier deposition area to perform m double-sided alumina diffusion barrier depositions. The first double-sided alumina diffusion barrier deposition and the m double-sided alumina diffusion barrier depositions are performed simultaneously. After the deposition is completed, the baseband is sent to a tape-retrieving device for tape-retrieving.

[0099] This application enables simultaneous double-sided sputtering (meaning that both sides of the same strip are sputtered simultaneously during a single tape run) + multiple sputtering of the strip + reversal of the sputtering faces after flipping, ensuring higher uniformity of both sides of the strip; multiple flipping of the strip can increase the tape run rate several times, thereby reducing the temperature rise of the strip surface, thus reducing the surface roughness of the alumina film and providing a good template for the subsequent growth of the texture layer.

[0100] In some specific implementations, m is an odd number between 1 and 7, for example, it can be 1, 3, 5 or 7.

[0101] In some specific embodiments, the preparation method further includes: monitoring the baseband tension in real time, and adjusting the tension adjustment wheel using a magnetic powder brake and / or an independent motor to adjust the baseband tension based on the monitoring results.

[0102] In some specific embodiments, the baseband transmission speed is 1~50mm / s, for example, it can be 1mm / s, 7mm / s, 12mm / s, 18mm / s, 23mm / s, 29mm / s, 34mm / s, 40mm / s, 45mm / s or 50mm / s, etc., but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0103] In some specific embodiments, the baseband transmission speed is 5~20mm / s.

[0104] In some specific embodiments, the preparation method further includes baking the baseband before feeding it into the alumina diffusion barrier layer deposition region of the double-sided superconducting tape.

[0105] In some specific embodiments, the baking temperature is 150~200℃, for example, it can be 150℃, 156℃, 160℃, 165℃, 170℃, 175℃, 180℃, 185℃, 195℃ or 200℃, but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0106] In some specific embodiments, the deposition of the double-sided alumina diffusion barrier layer includes: pre-sputtering before the substrate is fed in, and then depositing the double-sided alumina diffusion barrier layer when the substrate is fed in.

[0107] In some specific embodiments, the pre-sputtering includes: first evacuating the chamber to 0.0001~0.001 Pa, then introducing a protective gas, and then turning on the medium-frequency reactive sputtering device to perform pre-sputtering to clean the oxide layer and impurities on the surface of the aluminum target.

[0108] In some specific embodiments, the protective gas includes argon.

[0109] In some specific embodiments, the pressure after the protective gas is introduced is 1~3 Pa, for example, it can be 1 Pa, 1.3 Pa, 1.5 Pa, 1.7 Pa, 1.9 Pa, 2.2 Pa, 2.4 Pa, 2.6 Pa, 2.8 Pa or 3 Pa, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0110] In some specific embodiments, the pre-sputtering process parameters are the same as the sputtering parameters during the deposition of the double-sided alumina diffusion barrier layer.

[0111] In some specific embodiments, the pre-sputtering time is 3 to 10 minutes, for example, it can be 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0112] In some specific embodiments, the deposition of the double-sided alumina barrier layer includes: simultaneously turning on the intermediate frequency reactive sputtering device and the oxygen reaction controller, and sputtering and depositing an alumina film on the substrate surface that is being transported through the double-sided alumina barrier layer deposition area.

[0113] The combination of the intermediate frequency reactive sputtering device and the oxygen reaction controller in this application solves the problem of alumina target surface poisoning. This application can maintain the sputtering process in metal mode or transition mode at all times, and the deposition rate can be increased by several times or even an order of magnitude compared with DC reactive sputtering or radio frequency sputtering. This is a decisive advantage for industrial applications that need to deposit strips hundreds of meters or even kilometers long. In addition, the oxygen reaction controller can quickly adjust for slight fluctuations in the chamber environment caused by plasma interference, pull the process back to the set point, and thus ensure the synchronicity and consistency of deposition on both sides.

[0114] In some specific embodiments, the power of the sputtering deposition is 1 to 10 kW, for example, it can be 1 kW, 2 kW, 3 kW, 4 kW, 5 kW, 6 kW, 7 kW, 8 kW, 9 kW or 10 kW, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0115] In some specific embodiments, the sputtering deposition current is 1~15A, for example, it can be 1A, 3A, 5A, 6A, 8A, 9A, 11A, 12A, 14A or 15A, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0116] In some specific embodiments, the working pressure of the sputtering deposition is 0.5~3.5 Pa, for example, it can be 0.5 Pa, 0.9 Pa, 1.2 Pa, 1.5 Pa, 1.9 Pa, 2.2 Pa, 2.5 Pa, 2.9 Pa, 3.2 Pa or 3.5 Pa, etc., but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0117] In some specific embodiments, the flow rate ratio of argon to oxygen in the sputtering deposition is (0.5~1.5):1, for example, it can be 0.5:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1 or 1.5:1, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0118] In some specific embodiments, the flow rate of argon gas in the sputtering deposition ranges from 50 to 200 sccm, for example, it can be 50 sccm, 65 sccm, 80 sccm, 100 sccm, 110 sccm, 130 sccm, 150 sccm, 160 sccm, 180 sccm or 200 sccm, but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0119] In some specific embodiments, the oxygen flow rate in the sputtering deposition ranges from 50 to 200 sccm, for example, it can be 50 sccm, 65 sccm, 80 sccm, 100 sccm, 110 sccm, 130 sccm, 150 sccm, 160 sccm, 180 sccm or 200 sccm, but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0120] In some specific embodiments, the target surface voltage is monitored during the sputtering deposition process, and the oxygen flow rate is adjusted according to the monitored target surface voltage value.

[0121] As a specific embodiment of this application, a superconducting tape is provided, the superconducting tape comprising a base tape and alumina diffusion barrier layers disposed on two surfaces of the base tape; the absolute value of the thickness difference between the alumina diffusion barrier layers on both sides of the base tape is ≤2nm, for example, it can be 0.01nm, 0.24nm, 0.46nm, 0.68nm, 0.9nm, 1.12nm, 1.34nm, 1.56nm, 1.78nm or 2nm, etc., but is not limited to the listed values, and other unlisted values ​​within this range are also applicable. The absolute value of the roughness Rq difference between the alumina diffusion barrier layers on both sides of the base tape in a 5*5μm2 sampling area is ≤0.7nm, for example, it can be 0.01nm, 0.09nm, 0.17nm, 0.24nm, 0.32nm, 0.4nm, 0.47nm, 0.55nm, 0.63nm or 0.7nm, etc., but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0122] In some specific embodiments, the absolute value of the difference in thickness between the alumina diffusion barrier layers on both sides of the baseband is ≤1nm.

[0123] In some embodiments, the absolute value of the difference in roughness Rq between the alumina diffusion barrier layers on both sides of the baseband in a 5*5μm² sampling area is ≤0.1nm. In some embodiments, the baseband includes a Hastelloy baseband.

[0124] In some specific embodiments, the thickness of the alumina diffusion barrier layer on one side is 25~100nm, for example, it can be 25nm, 34nm, 40nm, 50nm, 55nm, 60nm, 75nm, 85nm, 90nm or 100nm, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0125] In some specific embodiments, the roughness Rq of the single-sided alumina diffusion barrier layer under a sampling area of ​​5*5μm2 is 0.5~3.0nm, for example, it can be 0.5nm, 0.8nm, 1.1nm, 1.4nm, 1.7nm, 1.9nm, 2.2nm, 2.5nm, 2.8nm or 3.0nm, etc., but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0126] This application has the following advantages:

[0127] (1) The scheme of combining medium-frequency reactive sputtering with oxygen reaction controller to regulate the target surface voltage and optimize the ratio of oxide deposition to metal deposition is beneficial to control the composition of alumina film and increase the deposition rate of film on the substrate surface by one or even several times, which can realize the industrial-grade production of double-sided superconducting tape.

[0128] (2) In this application, the baseband is heated and baked at 150~200℃ before entering the deposition zone, which can effectively remove the gas and moisture adsorbed on the surface of the baseband and improve the quality of the prepared film.

[0129] (3) The process of simultaneously depositing the baseband on both sides in the same preparation environment in this application can ensure the consistency of the growth of the thin film on both sides.

[0130] (4) The solution of adding a flipping component in the cavity can realize the flipping of the substrate during one tape transport process, so that at least two thin film depositions can be carried out on the substrate, which effectively improves the efficiency of thin film deposition, and saves experimental time by eliminating the need for additional vacuuming and other repetitive operations. The increased tape transport rate brought about by multiple flipping will also significantly reduce the temperature rise of the tape, which is obviously beneficial to reducing the roughness of the alumina layer and providing a better growth substrate for subsequent processes.

[0131] (5) In this application, the baseband sputtering surfaces are swapped after flipping, which means that either side of the baseband will undergo two or more identical target deposition processes, greatly ensuring the consistency of the two sides of the baseband.

[0132] The apparatus and method for preparing alumina diffusion barrier layers on double-sided superconducting tapes provided in this application enable the efficient and uniform preparation of high-quality alumina barrier layers on double-sided metal substrates, regardless of substrate width, thickness, or type. This technology effectively suppresses the high-temperature diffusion of substrate elements into the superconducting layer, significantly improving the overall interface quality and current-carrying capacity of the double-sided tape. This method is not only suitable for the large-scale, continuous production of second-generation high-temperature superconducting tapes (such as REBCO), meeting the stringent requirements for material consistency and stability in high-end applications such as high-field magnets and superconducting cables, but also provides a new technical pathway for the preparation of high-performance double-sided thin films in other flexible electronic devices.

[0133] Example 1

[0134] This embodiment provides a device for preparing a double-sided superconducting tape alumina diffusion barrier layer, such as... Figure 1 As shown, the preparation apparatus includes a tape feeding device 1, several guiding components, a double-sided superconducting tape alumina diffusion barrier layer deposition region 7, and a tape receiving device 12.

[0135] In the tape feeding device 1, the base tape 2 is fed into the tape taking device 12 through several guiding components. The double-sided superconducting tape alumina diffusion barrier layer deposition area 7 is located between the tape feeding device 1 and the tape taking device 12. The base tape 2 passes through the double-sided superconducting tape alumina diffusion barrier layer deposition area 7 twice. The several guiding components include a flipping wheel 10 for flipping the base tape 2.

[0136] The double-sided superconducting tape alumina diffusion barrier layer deposition region 7 includes two aluminum targets disposed opposite each other on both sides of the base tape 2. The aluminum targets are connected to a mid-frequency reactive sputtering device. The two aluminum targets alternately form a cathode and an anode at zero potential, which are used to generate an alumina diffusion barrier layer on the surface of the base tape 2 under the action of the mid-frequency reactive sputtering device. An oxygen reaction controller is also included to regulate the oxygen atmosphere in the double-sided superconducting tape alumina diffusion barrier layer deposition region 7. From the direction of the self-releasing tape device 1 to the retracting tape device 12, the plurality of guiding components sequentially include a tape-releasing guide wheel 3, a front guide component located before the double-sided superconducting tape alumina diffusion barrier layer deposition area 7, a rear guide component located after the double-sided superconducting tape alumina diffusion barrier layer deposition area 7, and a retracting guide wheel 11. The flipping wheel 10 is located at the end of the rear guide component and / or the front end of the front guide component, and is used to flip the base tape 2 once after passing through the double-sided superconducting tape alumina diffusion barrier layer deposition area each time. The front guide component includes two sets of front guide wheels arranged in parallel. The rear guide component includes two sets of rear guide wheels arranged in parallel. The tape-releasing guide wheel 3 and the retracting guide wheel 11 are each independently provided with a meter counting component.

[0137] Specifically, the front guide wheel assembly includes a first front guide wheel 6; the rear guide wheel assembly includes a first rear guide wheel 8 and a second rear guide wheel 9 arranged sequentially.

[0138] The preparation device further includes a tension sensor and a tension adjustment component. The tension sensor is used to monitor the tension of the baseband 2 during the baseband 2 conveying process and feed it back to the tension adjustment component. The tension adjustment component adjusts the tension of the baseband 2 based on the monitored tension of the baseband 2, with a magnetic powder brake as the actuating component and a tension adjustment wheel as the auxiliary component.

[0139] The preparation device also includes a base belt baking device 5, which is arranged between the belt feeding guide wheel 3 and the front guide component along the conveying direction of the base belt 2; and a baking device guide wheel 4 is also arranged in front of the base belt baking device 5.

[0140] The tape take-up device 12 includes a tape take-up servo motor;

[0141] The oxygen reaction controller includes a voltage sensor for monitoring the target surface voltage and an oxygen regulator for adjusting the oxygen flow rate based on the monitored target surface voltage value.

[0142] The preparation apparatus also includes a chamber and a vacuum pumping device for evacuating the chamber. The plurality of guiding components and the double-sided superconducting tape alumina diffusion barrier deposition region 7 are all disposed in the chamber.

[0143] Example 2

[0144] This embodiment provides a device for preparing a double-sided superconducting tape alumina diffusion barrier layer, such as... Figure 2 As shown, the preparation device is the same as that in Example 1, except that some of the guiding components are different from those in Example 1.

[0145] Specifically, the baseband 2 passes through the double-sided superconducting tape alumina diffusion barrier layer deposition region 7 4 times, and the plurality of guiding components include 3 flipping wheels 10 for flipping the baseband 2.

[0146] From the tape feeding device 1 to the tape take-up device 12, the plurality of guiding components sequentially include a tape feeding guide wheel 3, a front guide component located before the double-sided superconducting tape alumina diffusion barrier layer deposition area 7, a rear guide component located after the double-sided superconducting tape alumina diffusion barrier layer deposition area 7, and a tape take-up guide wheel 11. The flipping wheel 10 is located at the end of the rear guide component and / or the front end of the front guide component, and is used to flip the base tape 2 after each passage through the double-sided superconducting tape alumina diffusion barrier layer deposition area. The front guide component includes four sets of front guide wheels arranged in parallel. The rear guide component includes four sets of rear guide wheels arranged in parallel. Each of the tape feeding guide wheel 3 and the tape take-up guide wheel 11 is independently equipped with a meter counting component.

[0147] Specifically, the front guide wheel assembly includes a first front guide wheel 6; the rear guide wheel assembly includes a first rear guide wheel 8 and a second rear guide wheel 9 arranged sequentially.

[0148] Comparative Example 1

[0149] This comparative example provides a device for preparing a double-sided superconducting tape alumina diffusion barrier layer. The device is the same as in Example 1 except that it does not have a turning wheel, and the front guide component includes a set of front guide wheels and the rear guide component includes a set of rear guide wheels.

[0150] Comparative Example 2

[0151] This comparative example provides a device for preparing alumina diffusion barrier layer on a double-sided superconducting tape. The device is the same as in Example 1 except that it does not have an oxygen reaction controller, uses an alumina target, does not require a rotating wheel, and only has one deposition stage.

[0152] Comparative Example 3

[0153] This comparative example provides a device for preparing a double-sided superconducting tape alumina diffusion barrier layer. The device is the same as that in Comparative Example 1, except that it does not use double-sided deposition but instead uses single-sided deposition.

[0154] Application Example 1

[0155] This application example provides a method for preparing a double-sided superconducting tape alumina diffusion barrier layer. The preparation method uses the apparatus provided in Example 1. Specifically, the preparation method includes:

[0156] The baseband is fed into a baseband baking device at 150-200°C for baking treatment, and then into a double-sided superconducting tape alumina diffusion barrier deposition zone for the first double-sided alumina diffusion barrier deposition. The baseband is then flipped once by a turning wheel. After each flip, it is fed back into the same double-sided superconducting tape alumina diffusion barrier deposition zone for the second double-sided alumina diffusion barrier deposition. The first and second double-sided alumina diffusion barrier depositions are performed simultaneously. After deposition, the baseband is fed into a take-up device for take-up. The baseband tension is monitored in real time, and based on the monitoring results, a magnetic powder brake is used as the actuator, with a tension adjustment wheel assisting in adjusting the baseband tension.

[0157] Before depositing the double-sided alumina diffusion barrier layer, the process includes: first, evacuating the chamber to 0.0001~0.001 Pa, then introducing argon gas and controlling the pressure to 1~3 Pa; then, turning on the intermediate frequency reactive sputtering device for pre-sputtering for 3~10 minutes to clean the oxide layer and impurities on the surface of the aluminum target. The process parameters for the pre-sputtering are the same as the sputtering parameters for the deposition of the double-sided alumina diffusion barrier layer. Then, during the substrate feed, the double-sided alumina diffusion barrier layer is deposited, which includes: simultaneously turning on the intermediate frequency reactive sputtering device and... An oxygen reaction controller is used to sputter-deposit an alumina thin film on the surface of a substrate that is conveyed through a double-sided alumina diffusion barrier deposition zone. The sputtering deposition power is 1~10kW, the current is 1~15A, the working pressure is 0.5~3.5Pa, the argon to oxygen flow ratio is (0.5~1.5):1, the argon flow rate range is 50~200sccm, and the oxygen flow rate range is 50~200sccm. During the sputtering deposition process, the oxygen concentration is monitored, and the oxygen flow rate is adjusted according to the monitored oxygen concentration.

[0158] Application Example 2

[0159] This application example provides a method for preparing an alumina diffusion barrier layer on a double-sided superconducting tape. The preparation method uses the apparatus provided in Example 2. The only difference from Application Example 1 is that the base tape is flipped three times by three flipping wheels. After each flip, it is fed back into the same double-sided superconducting tape alumina diffusion barrier layer deposition area for a second, third, and fourth double-sided alumina diffusion barrier layer deposition, respectively. The first double-sided alumina diffusion barrier layer deposition and the second, third, and fourth double-sided alumina diffusion barrier layer deposition are performed simultaneously.

[0160] For ease of comparison and analysis, the conditions for application examples 1 and 2 were as follows: the baking temperature was 180℃; the chamber was first evacuated to 0.0001 Pa, then argon gas was introduced and the pressure was controlled at 2 Pa; then, the medium-frequency reactive sputtering device was turned on for pre-sputtering for 5 minutes to clean the oxide layer and impurities on the surface of the aluminum target. The working pressure was 1.0 Pa, the argon to oxygen flow ratio was controlled at 1:1, and the argon flow rate was 100 sccm, and the oxygen flow rate was 100 sccm. This control was adjusted in real time during production based on the oxygen concentration. The sputtering deposition voltage was 360 V, and the sputtering deposition current varied accordingly with the power.

[0161] The thickness and roughness data of the alumina anti-diffusion layer on both sides of the baseband were obtained by adjusting the sputtering power and different tape feed rates in Application Example 1 and Application Example 2, as shown in Table 1.

[0162] Table 1

[0163]

[0164] As shown in Table 1, the method for preparing the alumina diffusion barrier layer of the double-sided superconducting tape provided in this application can improve the deposition efficiency by more than 100%, and the thickness difference between the two sides of the tape is small, within 1 nm, and within 5*5 μm. 2 The surface roughness Rq of the sampled area is within 2.6 nm and within 5*5 μm. 2 The difference in roughness Rq between the two sides of the strip within the sampling area is within 0.13 nm. This indicates that the preparation method of the alumina diffusion barrier layer for double-sided superconducting strips provided in this application can not only improve the deposition efficiency, but also improve the surface quality of the alumina diffusion barrier layer deposited on the strip surface, and shorten the quality difference between the two sides, thereby improving the stability of the deposited surface.

[0165] Application Example 3

[0166] This application example provides a method for preparing an alumina diffusion barrier layer for a double-sided superconducting tape. The preparation method uses the apparatus provided in Example 1, and is the same as in Application Example 1-1 except that no baking treatment is performed.

[0167] Application Example 4

[0168] This application example provides a method for preparing an alumina diffusion barrier layer for a double-sided superconducting tape. The preparation method uses the apparatus provided in Example 1, and is the same as in Application Example 1-1 except that the tape speed is 60 mm / s.

[0169] Application Example 5

[0170] This application example provides a method for preparing an alumina diffusion barrier layer for a double-sided superconducting tape. The preparation method uses the apparatus provided in Example 1, and is the same as in Application Example 1-1 except that the tape speed is 5 mm / s.

[0171] Application Comparative Example 1

[0172] This application provides a comparative example of a method for preparing an alumina diffusion barrier layer on a double-sided superconducting tape. The purpose of the preparation method is the same as that of Application Example 1-1, which is to obtain an alumina diffusion barrier layer with a thickness of 62 nm. The only difference from Application Example 1-1 is that the apparatus of Comparative Example 1 is used, and no flipping is performed. The tape feed rate is 5 mm / s. All other aspects are the same as those in Application Example 1-1.

[0173] Application Comparative Example 2

[0174] This application provides a comparative example of a method for preparing an alumina diffusion barrier layer on a double-sided superconducting tape. The purpose of the preparation method is the same as that of Application Example 1-1, which is to obtain an alumina diffusion barrier layer with a thickness of 62 nm. The only difference from Application Example 1-1 is that oxygen is not introduced and an alumina plate target is used directly. The other process parameters are exactly the same as those in Application Example 1-1.

[0175] Application Comparative Example 3

[0176] This application provides a comparative example of a method for preparing an alumina diffusion barrier layer on a double-sided superconducting tape. The purpose of the preparation method is the same as that of Application Example 1-1, in order to obtain an alumina diffusion barrier layer with a thickness of 62 nm. The only difference from Application Example 1-1 is that the first side is deposited first, and then the second side is deposited by flipping. The tape travel rate is 5 mm / s. All other aspects are the same as those in Application Example 1-1.

[0177] Table 2 shows the thickness and roughness data of the alumina diffusion barrier layers on both sides of the baseband obtained from Application Examples 3-5 and Comparative Examples 1-3.

[0178] Table 2

[0179]

[0180] Several points can be observed from Table 2:

[0181] (1) Combining Application Example 1-1 and Application Example 3, it can be seen that baking treatment in Application Example 1 can better improve the surface quality of the alumina diffusion layer deposited on the strip surface.

[0182] (2) Combining Application Examples 1-1 and 4-5, it can be seen that in Application Example 4, the tape carrying rate is too high. Although the surface roughness of the tape decreases, the deposition thickness of the tape is also significantly reduced, and the tape tension is too high, making tape breakage more likely during production. In Application Example 5, the tape carrying rate is too low, and the surface roughness of the tape is improved compared to Application Example 1-1. This shows that by controlling the tape carrying rate within a reasonable range, this application can balance the deposition thickness and the surface quality of the alumina diffusion barrier layer.

[0183] (3) In Comparative Example 1, the apparatus of Comparative Example 1 was used without flipping, resulting in a thickness difference of up to 7.2 nm on both sides of the strip and a surface roughness difference of up to 0.21 nm. This indicates that without the flipping wheel in Comparative Example 1, not only is the time longer and the efficiency lower, but the difference in thickness and surface roughness between the two sides is also larger. In Comparative Example 2, due to the use of alumina target material, only single-sided deposition can be performed each time, resulting in a significant decrease in production efficiency, and the difference in thickness and surface roughness between the two sides is improved compared to Comparative Example 1-1. Compared to Comparative Example 1, Comparative Example 3 does not use double-sided deposition, resulting in a decrease in deposition efficiency. Although the difference between the two sides of the surface is improved compared to Comparative Example 1, the consistency of the thickness and roughness of the two sides of the surface is still lower than that of Comparative Example 1.

[0184] This application illustrates its detailed features through the above embodiments, but it is not limited to these detailed features, meaning that this application does not necessarily rely on them for implementation. Those skilled in the art should understand that any improvements to this application, equivalent substitutions for selected technical features, additions of auxiliary technical features, and selection of specific methods all fall within the protection and disclosure scope of this application.

Claims

1. A device for preparing a double-sided superconducting tape alumina diffusion barrier layer, characterized in that, The preparation apparatus includes: a tape feeding device, several guiding components, a double-sided superconducting tape alumina diffusion barrier layer deposition zone, and a tape receiving device; In the tape feeding device, the base tape is fed into the tape taking device through several guiding components, and the double-sided superconducting tape alumina diffusion barrier layer deposition area is located between the tape feeding device and the tape taking device. The number of times the baseband passes through the alumina barrier diffusion layer deposition region of the double-sided superconducting tape is 2n. The plurality of guiding components include a flipping component that flips the baseband m times, which is used to flip the baseband once after each passage through the alumina barrier diffusion layer deposition region of the double-sided superconducting tape, where m=2n-1 and n is a non-zero natural number. The double-sided superconducting tape alumina diffusion barrier layer deposition region includes: Two aluminum targets are arranged opposite each other on both sides of the baseband. The aluminum targets are connected to the intermediate frequency reactive sputtering device. The two aluminum targets alternately form cathodes and anodes at zero potential, which are used to generate an aluminum oxide diffusion barrier layer on the baseband surface under the action of the intermediate frequency reactive sputtering device. And an oxygen reaction controller, used to regulate the oxygen atmosphere in the deposition zone of the alumina diffusion barrier layer of the double-sided superconducting tape.

2. The preparation apparatus according to claim 1, characterized in that, The preparation device further includes a tension sensor and a tension adjustment component. The tension sensor is used to monitor the baseband tension during the baseband conveying process and feed it back to the tension adjustment component. The tension adjustment component is used to adjust the baseband tension according to the baseband tension monitored by the tension sensor. The tension adjustment component includes an actuation component, which includes a magnetic powder brake and / or an independent motor to assist the tension adjustment wheel.

3. The preparation apparatus according to claim 1 or 2, characterized in that, In the direction from the tape feeding device to the tape take-up device, the plurality of guiding components sequentially include a tape feeding guide wheel, a front guide component located before the alumina diffusion barrier layer deposition area of ​​the double-sided superconducting tape, a rear guide component located after the alumina diffusion barrier layer deposition area of ​​the double-sided superconducting tape, and a tape take-up guide wheel. The flipping component is located at the end of the rear guide component and / or the front end of the front guide component, and is used to flip the base tape. The front guide component has 2n sets of front guide paths arranged in parallel; the number of n is 1 to 4. And / or, the rear guide component has 2n sets of rear guide paths arranged in parallel; the number of n is 1 to 4; And / or, the tape feeding guide wheel and the tape taking guide wheel are each independently equipped with a meter counting component.

4. The preparation apparatus according to claim 1 or 2, characterized in that, The preparation apparatus also includes a baseband baking device, which is a guide component positioned before the deposition area of ​​the double-sided superconducting tape alumina diffusion barrier layer along the baseband conveying direction. And / or, the take-up device includes a take-up servo motor; And / or, the tape feeding device includes a tape feeding torque motor or a tape feeding servo motor; And / or, the oxygen reaction controller includes a voltage sensor for monitoring target surface voltage; and an oxygen regulator for adjusting the oxygen flow rate based on the monitored target surface voltage.

5. The preparation apparatus according to claim 1 or 2, characterized in that, The preparation apparatus also includes a chamber and a vacuum pumping device for evacuating the chamber. The plurality of guiding components and the double-sided superconducting tape alumina diffusion barrier deposition area are all disposed in the chamber.

6. A method for preparing an alumina diffusion barrier layer on a double-sided superconducting tape, characterized in that, The preparation method is carried out using the apparatus for preparing the double-sided superconducting tape alumina diffusion barrier layer as described in any one of claims 1 to 5.

7. The preparation method according to claim 6, characterized in that, The preparation method includes: the baseband is fed into the double-sided superconducting tape alumina diffusion barrier layer deposition area by a self-releasing device to perform the first double-sided alumina diffusion barrier layer deposition, and then the baseband is flipped m times. After each flip, it is fed back into the same double-sided superconducting tape alumina diffusion barrier layer deposition area to perform m double-sided alumina diffusion barrier layer depositions. The first double-sided alumina diffusion barrier layer deposition and the m double-sided alumina diffusion barrier layer depositions are performed simultaneously. After the deposition is completed, the baseband is sent to a tape-retrieving device for tape-retrieving.

8. The preparation method according to claim 7, characterized in that, The m is an odd number between 1 and 7; And / or, the preparation method further includes: monitoring the baseband tension in real time, and adjusting the tension adjustment wheel using a magnetic powder brake and / or an independent motor to adjust the baseband tension based on the monitoring results; And / or, the baseband's transmission speed is 1~50mm / s; And / or, before depositing the alumina diffusion barrier layer in the double-sided superconducting tape, the preparation method further includes baking the base tape; wherein the baking temperature is 150~200℃. And / or, the deposition of the double-sided alumina diffusion barrier layer includes: pre-sputtering before the baseband is fed in, and then depositing the double-sided alumina diffusion barrier layer when the baseband is fed in. The pre-sputtering process includes: first, evacuating the chamber to 0.0001~0.001 Pa, then introducing a protective gas, and then turning on the medium-frequency reactive sputtering device to perform pre-sputtering to clean the oxide layer and impurities on the surface of the aluminum target; the protective gas includes argon; the pressure after introducing the protective gas is 1~3 Pa; the process parameters of the pre-sputtering are the same as the sputtering parameters during the deposition of the double-sided alumina diffusion barrier layer; the pre-sputtering duration is 3~10 min. And / or, the deposition of the double-sided alumina barrier layer includes: simultaneously turning on the intermediate frequency reactive sputtering device and the oxygen reaction controller, and sputtering and depositing an alumina film on the baseband surface that is being transported through the double-sided alumina barrier layer deposition area; Wherein, the power of the sputtering deposition is 1~10kW; and / or, the current of the sputtering deposition is 1~15A; and / or, the working pressure of the sputtering deposition is 0.5~3.5Pa; and / or, the flow ratio of argon to oxygen in the sputtering deposition is (0.5~1.5):1; and / or, the flow rate of argon in the sputtering deposition is 0~200sccm; and / or, the flow rate of oxygen in the sputtering deposition is 0~200sccm; and / or, the target surface voltage is monitored during the sputtering deposition process, and the oxygen flow rate is adjusted according to the monitored voltage value.

9. A superconducting tape, characterized in that, The superconducting tape is prepared by the method for preparing the alumina diffusion barrier layer of the double-sided superconducting tape according to any one of claims 6 to 8; The superconducting tape includes a base tape and an alumina diffusion barrier layer disposed on two surfaces of the base tape; The absolute value of the thickness difference between the alumina diffusion barrier layers on both sides of the baseband is ≤2nm, and / or the alumina diffusion barrier layers on both sides of the baseband are 5*5μm. 2 The absolute value of the difference in roughness Rq across the sampled area is ≤0.7nm.

10. The superconducting tape according to claim 9, characterized in that, The baseband includes a Hastelloy baseband; And / or, the thickness of the alumina diffusion barrier layer on one side is 25~100nm; And / or, the single-sided alumina diffusion barrier layer is 5*5μm 2 The roughness Rq of the sampled area is 0.5~3.0 nm.

Citation Information

Patent Citations

  • Continuous preparing method of double-sided superconductive belt material buffer layer

    CN102255040B

  • Superconducting tape buffer layer double-sided coating device

    CN209508401U