A method for preparing boron-doped diamond film on aluminum-based surface based on microwave plasma chemical vapor deposition
By using microwave plasma chemical vapor deposition technology, the problems of difficult nucleation, interfacial stress cracking, and low-temperature doping efficiency of diamond films on aluminum substrates were solved, and high-quality boron-doped diamond films were prepared.
Patent Information
- Application Number
- CN202611412859.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-20
AI Technical Summary
Direct deposition of diamond films on aluminum substrates presents challenges such as nucleation difficulties, interfacial stress cracking, and low-temperature doping efficiency.
Microwave plasma chemical vapor deposition technology was used to remove the oxide layer on the surface of an aluminum substrate and form a nanoscale rough structure through pretreatment. The gas ratio and deposition parameters were controlled in stages, and annealing was combined to eliminate the internal stress of the film, so as to realize the preparation of boron-doped diamond film at low temperature.
This significantly improved the nucleation density and grain uniformity of diamond films, reduced residual stress and boron doping efficiency, and produced high-quality boron-doped diamond films.
Smart Images

Figure CN123132844A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of materials surface engineering and functional thin film preparation technology, and more specifically to a method for preparing boron-doped diamond films on aluminum substrates based on microwave plasma chemical vapor deposition. Background Technology
[0002] Diamond films are considered ideal functional coating materials due to their ultra-high hardness (>90 GPa), extremely high thermal conductivity (>2000 W / m·K), and wide electrochemical window. However, the direct deposition of diamond films on aluminum substrates faces the following technical obstacles:
[0003] 1. Difficulty in nucleation: The natural oxide layer (Al2O3) on the aluminum substrate surface hinders the adsorption of diamond carbon sources, resulting in a nucleation density of <10. 6 cm -2 (Reference: Applied Surface Science, 2020, 512, 145657); The etching capability of hydrogen plasma decreases at low temperatures (<600℃), making it difficult to effectively remove amorphous carbon phases, resulting in a reduction in the size of boron-doped diamond grains (<100nm) and an amorphous component ratio of >40%.
[0004] 2. Interface stress cracking: The coefficient of thermal expansion of aluminum is 24 × 10⁻⁶. -6 / K) and diamond (1×10 -6 The difference in K is significant, and residual stress >1.5 GPa is generated during the cooling process after the film thickness exceeds 20 μm (Reference: Diamond and Related Materials, 2021, 118, 108502). A 30μm thick film prepared by conventional processes has a warpage curvature >5m at room temperature. -1 Interface peeling rate > 80%.
[0005] 3. Low doping efficiency at low temperatures: Conventional MPCVD processes achieve boron doping efficiency <10% and film resistivity >10 Ω·cm at 500℃ (Reference: Journal of Materials Chemistry C, 2019, 7, 12345). Therefore, how to provide a method for preparing boron-doped diamond films on aluminum substrates based on microwave plasma chemical vapor deposition is a technical problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0006] In view of this, the present invention provides a method for preparing boron-doped diamond films on aluminum substrates based on microwave plasma chemical vapor deposition to solve three problems existing in the prior art: 1. The difficulty of diamond nucleation at low temperatures and the weak etching ability of hydrogen atoms on graphite.
[0007] 2. The problem of high internal stress and high internal thermal stress in diamond.
[0008] 3. The difficulty in boron doping and the challenge of achieving low-temperature doping.
[0009] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing boron-doped diamond films on aluminum substrates using microwave plasma chemical vapor deposition includes the following steps: (1) Pretreatment of aluminum substrate: Mechanical grinding or polishing is performed on the aluminum substrate to remove the surface oxide layer, followed by alkaline washing and ultrasonic cleaning; (2) Plasma pretreatment: Under Ar atmosphere, microwave plasma is used to etch the surface of aluminum substrate to remove residual contaminants and form a nanoscale rough structure; At 500℃ and 2.0kW, Ar + Ion bombardment creates pit structures with a depth of 50-200 nm, increasing the specific surface area by 3-5 times and providing mechanical locking anchors.
[0010] (3) Boron-doped diamond nucleation and deposition: methane (CH4), hydrogen (H2), carbon dioxide (CO2) and trimethylborane (TMB) were introduced into the reaction gases, and the diamond was deposited in stages under microwave power of 1.5-3.5kW, temperature of 400-550℃ and pressure of 15-60Torr. (4) Annealing treatment: Slowly cool to room temperature in an inert atmosphere to eliminate internal stress in the film.
[0011] Preferably, the alkaline washing in step (1) uses a mixed alkaline solution of sodium hydroxide and sodium phosphate, and the washing time is 5-10 minutes.
[0012] The present invention removes the oxide layer by alkaline washing: using a mixed solution of 10wt% NaOH and 10wt% Na3PO4, the oxide film is thoroughly removed through the reaction Al2O3 + 2NaOH → 2NaAlO2 + H2O. Preferably, the ultrasonic cleaning time in step (1) is 30 minutes or more.
[0013] Preferably, the volume ratio of methane, hydrogen, carbon dioxide and trimethylborane in step (3) is CH4:H2:CO2:TMB=2-8%:80-96%:0.5-8%:0.5-1.5%.
[0014] Preferably, the staged deposition in step (3) includes: nucleation stage This stage aims to rapidly form a dense diamond nucleus layer on the aluminum substrate surface.
[0015] Process parameters: Gas ratio: methane: hydrogen: carbon dioxide: trimethylborane = 7-10%: 85-90%: 1-1.5%: 0.5-1%; Temperature: 450-550℃; Atmospheric pressure: 15-60 Torr; Microwave power: 1.5-2kW; Deposition time: 1-2 hours.
[0016] Gas function: Methane: Provides a high concentration of carbon source, significantly increasing the nucleation rate of diamond on the aluminum substrate, ensuring that the substrate is quickly covered by crystal nuclei.
[0017] Hydrogen: Creates a high-concentration atomic hydrogen environment, utilizing its strong etching effect on non-diamond carbon (amorphous carbon) to remove unstable carbon phases and improve nucleation purity.
[0018] Carbon dioxide: its decomposition provides oxygen atoms, which on the one hand reduces the binding energy on the diamond surface, and on the other hand helps to increase the concentration of active carbon source, thus synergistically promoting nucleation.
[0019] Trimethylborane: Utilizing its property of easily breaking BC bonds at low temperatures, it promotes the replacement of carbon atoms in the crystal lattice by boron atoms in the early stage of nucleation, thus achieving initial doping at low temperatures.
[0020] 2. Transitional growth stage This stage aims to transform the nucleation layer into a continuous crystalline thin film and control the crystal orientation.
[0021] Process parameters: Gas ratio: Adjusted to methane:hydrogen:carbon dioxide:trimethylborane = 3-5%:90-95%:0.5-1.5%:0.5-1%; Temperature: 500-540℃; Atmospheric pressure: 25-30 Torr; Microwave power: 3.0kW; Deposition time: 2-3 hours.
[0022] Gas function: Reducing the methane ratio: This reduces the carbon supersaturation in the system, effectively suppressing secondary nucleation (i.e. preventing the formation of new disordered nuclei between already grown grains), and ensuring the compactness and crystal quality of the film.
[0023] Increased microwave power (3.0kW): Significantly increases plasma density and the energy of active groups, accelerates the preferential growth of diamond crystals, and promotes grain merging and growth.
[0024] Hydrogen and carbon dioxide: Maintain a high-hydrogen environment to etch the non-diamond phase, while using oxygen atoms to further purify the growth surface.
[0025] Trimethylborane: Maintains a high proportion of boron source to ensure the continuity of doping concentration during rapid crystal growth.
[0026] 3. Thick film deposition stage This stage aims to grow high-quality, uniformly thick, and stably doped diamond films.
[0027] Process parameters: Gas ratio: Further adjusted to methane:hydrogen:carbon dioxide:trimethylborane = 2-3%:94-97%:0.5-3%:0.3-1%; Temperature: 500-550℃; Atmospheric pressure: 30-60 Torr; Microwave power: 2.5kW.
[0028] Deposition time: 38-40 minutes.
[0029] Gas function: Ultra-low methane ratio: Extremely low carbon source concentration minimizes the non-diamond phase (graphite phase / sp). 2 The formation of carbon improves the purity and thermal conductivity of the thin film.
[0030] Trimethylborane: By appropriately reducing the proportion of boron source and matching the growth rate, the stability of the film thickness doping is maintained, and doping unevenness caused by excessively rapid growth is prevented.
[0031] Carbon dioxide: continuously provides oxygen atoms and selectively removes sp2+ generated during growth. 2 Hybridized carbon bonds ensure the crystal quality of thick films.
[0032] The deposition process of this invention features a gradient pressurization: the gas pressure is gradually increased from 40 Torr during the nucleation stage to 60 Torr during the thick film stage, thereby reducing the thermal shock of the plasma to the film layer.
[0033] Preferably, the cooling rate of the annealing process in step (4) is ≤10℃ / min, and the inert gas is argon or nitrogen. Cooling at a rate of ≤10℃ / min allows the diamond lattice to rearrange in an orderly manner and releases the phase transformation stress (thermodynamic simulations show that the stress increases by more than 200% when the cooling rate is >15℃ / min).
[0034] Preferably, the boron doping concentration of the boron-doped diamond film is 5 × 10⁻⁶. 19 –1×10 20 cm -3 The film thickness is 5-50 μm.
[0035] As can be seen from the above technical solution, compared with the prior art, the present invention has the following technical effects: 1. Nucleation density increased to >10 9 cm -2 ; 2.30μm thick film residual stress <1.5GPa, critical load ≥30N; 3. At 500℃, the boron doping efficiency is >30% and the resistivity is ≤1.5Ω·cm. Attached Figure Description
[0036] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0037] Figure 1 This is a microscopic morphology diagram of Example 1. As shown in the figure, the diamond grains exhibit a fine polycrystalline structure, with small and uniform grain size, and no obvious amorphous carbon or graphite phase impurities in the microstructure.
[0038] Figure 2 The image shows the microstructure of Example 2. As shown, with the adjustment of process parameters, the diamond grains grew larger than in Example 1, but still maintained a uniform polycrystalline structure with no obvious amorphous carbon or graphite phase impurities.
[0039] Figure 3 This is a microscopic morphology diagram of Example 3. As shown in the figure, the diamond grains are significantly larger, exhibiting a coarse polycrystalline structure. The grains are more fully developed and remain pure, without obvious amorphous carbon and graphite phase impurities. Detailed Implementation
[0040] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0041] Example 1: Preparation of 5μm thin films 1. Substrate preprocessing: Base material: 6061 aluminum alloy (size 20×20×2mm) 3 ); Mechanical polishing: Polish with diamond polishing paste (1μm particle size) to a surface roughness Ra=15nm; Alkaline washing: Ultrasonic cleaning with a mixture of 10% NaOH and 10% Na3PO4 for 8 minutes; Solvent cleaning: Sonicate for 10 minutes each in sequence with acetone, anhydrous ethanol, and deionized water.
[0042] 2. Plasma pretreatment: Process parameters: Ar flow rate 200 sccm, gas pressure 20 Torr, microwave power 2.0 kW, temperature 500℃, time 30 minutes; Effect: The surface forms uniform pits.
[0043] 3. Deposition Process: The cleaned substrate is placed on a Mo substrate and placed into the vacuum chamber of the MPCVD equipment. The MPCVD equipment is run and evacuated to achieve a base vacuum. Then, a reactive gas is injected. The volume ratio of the components in the reactive gas (CH4:H2:CO2:TMB) is 8%:90%:1.5%:0.5%. After the vacuum chamber stabilizes and the gas pressure is maintained at 1 torr, the microwave source is turned on at a frequency of 2.45 GHz. The gas pressure is adjusted to 4 torr to excite the plasma. The reactive gas is continuously injected at a flow rate of 100 sccm to maintain the gas pressure at 40 torr. The temperature inside the chamber is maintained at 420°C for deposition. The plasma is kept running normally for 1 hour. The reaction gas ratio (CH4:H2:CO2:TMB) was adjusted to 4%:94%:1.5%:0.5% and the MPCVD equipment was maintained for 30 minutes. The reaction gas ratio (CH4:H2:CO2:TMB) was then adjusted to 2%:94%:3%:1% and the MPCVD equipment was maintained for 40 hours until the reaction was completed. Ar gas was introduced to cool the sample to 60 degrees Celsius at a rate of ≤10℃ / min. The microwave source and plasma were turned off, the injection of reaction gas was stopped, a vacuum was drawn, and after the sample cooled, air was backfilled into the vacuum chamber. The sample was then removed to obtain aluminum-based boron-doped diamond.
[0044] Example 2 Preparation of 20 μm thick boron-doped thin films with resistivity ≤1.5 Ω·cm 1. Substrate preprocessing: Base material: 6061 aluminum alloy (size 20×20×2mm) 3 ); Mechanical polishing: Polish with diamond polishing paste (1μm particle size) to a surface roughness Ra=12nm; Alkaline washing: Ultrasonic cleaning with a mixed alkaline solution of 10% NaOH + 10% Na3PO4 for 8 minutes; Solvent cleaning: Sonicate for 10 minutes each in sequence with acetone, anhydrous ethanol, and deionized water.
[0045] 2. Plasma pretreatment: Process parameters: Ar flow rate: 200 sccm, gas pressure: 20 Torr, microwave power: 2.0 kW, temperature: 500℃, time: 30 minutes; Effect: The surface forms uniform pits.
[0046] 3. Deposition Process: The cleaned substrate is placed on a Mo substrate and placed into the vacuum chamber of the MPCVD equipment. The MPCVD equipment is run and evacuated to achieve a base vacuum. Then, a reactive gas is injected. The volume ratio of the components in the reactive gas (CH4:H2:CO2:TMB) is 8%:90%:1%:1%. After the vacuum chamber stabilizes and the gas pressure is maintained at 1 torr, the microwave source is turned on at a frequency of 1.8 kW. The gas pressure is adjusted to 40 Torr to excite the plasma. The reactive gas is continuously injected at a flow rate of 100 sccm to maintain the gas pressure at 40 torr. The temperature inside the chamber is maintained at 520°C for deposition. The plasma is kept in normal operation for 1.5 hours. The reaction gas ratio (CH4:H2:CO2:TMB) was adjusted to 3%:95%:0.5%:1%, the microwave frequency was 3 kW, the gas pressure was adjusted to 28 Torr, and the cavity temperature was maintained at 530℃ for deposition. The MPCVD equipment was maintained for 2.5 hours. The reaction gas ratio (CH4:H2:CO2:TMB) was then adjusted to 2%:96%:0.5%:0.5%, the microwave frequency was 2.5 kW, the gas pressure was adjusted to 50 Torr, and the cavity temperature was maintained at 540℃ for deposition. The MPCVD equipment was maintained for 38 hours until the reaction was completed. Ar gas was introduced to cool the sample to room temperature at a rate of ≤8℃ / min. The microwave source and plasma were turned off, the injection of reaction gas was stopped, a vacuum was drawn, and after the sample cooled, air was backfilled into the vacuum cavity. The sample was then removed to obtain aluminum-based boron-doped diamond.
[0047] Example 3 20 μm thick boron-doped thin film with resistivity ≤3 Ω·cm: 1. Substrate preprocessing: Base material: 6061 aluminum alloy (size 20×20×2mm³); Mechanical polishing: Polish with diamond polishing paste (1μm particle size) to a surface roughness Ra=12nm; Alkaline washing: Ultrasonic cleaning with a mixed alkaline solution of 10% NaOH + 10% Na3PO4 for 8 minutes; Solvent cleaning: Sonicate for 10 minutes each in sequence with acetone, anhydrous ethanol, and deionized water.
[0048] 2. Plasma pretreatment: Process parameters: Ar flow rate: 200 sccm, gas pressure: 20 Torr, microwave power: 2.0 kW, temperature: 500 ℃, time: 30 minutes; Effect: The surface forms uniform pits.
[0049] 3. Deposition Process: The cleaned substrate is placed on a Mo substrate and placed into the vacuum chamber of the MPCVD equipment. The MPCVD equipment is run and evacuated to achieve a base vacuum. Then, a reactive gas is injected. The volume ratio of the components in the reactive gas (CH4:H2:CO2:TMB) is 8%:90%:1.4%:0.6%. After the vacuum chamber stabilizes and the gas pressure is maintained at 1 torr, the microwave source is turned on at a frequency of 1.8 kW. The gas pressure is adjusted to 40 Torr to excite the plasma. The reactive gas is continuously injected at a flow rate of 100 sccm to maintain the gas pressure at 40 torr. The temperature inside the chamber is maintained at 520°C for deposition. The plasma is kept running normally for 1 hour. The reaction gas ratio (CH4:H2:CO2:TMB) was adjusted to 3%:95%:0.5%:1%, the microwave frequency was 3 kW, the gas pressure was adjusted to 28 Torr, and the cavity temperature was maintained at 530℃ for deposition. The MPCVD equipment was maintained for 2 hours. The reaction gas ratio (CH4:H2:CO2:TMB) was then adjusted to 2%:96%:0.8%:0.3%, the microwave frequency was 2.5 kW, the gas pressure was adjusted to 50 Torr, and the cavity temperature was maintained at 540℃ for deposition. The MPCVD equipment was maintained for 40 hours until the reaction was completed. Ar gas was introduced to cool the sample to room temperature at a rate of ≤8℃ / min. The microwave source and plasma were turned off, the injection of reaction gas was stopped, a vacuum was drawn, and after the sample cooled, air was backfilled into the vacuum cavity. The sample was then removed to obtain aluminum-based boron-doped diamond.
[0050] Sample performance testing The performance of the aluminum-based boron-doped diamond film prepared in Example 3 was tested, and the test results are as follows: 1. Film thickness: 20.2 μm, thickness uniformity: 5%; 2. Boron atom doping concentration: 6.2 × 10⁻⁶ 17 cm -3 , in 5×10 15 –1×10 18 cm -3 Within the design scope; 3. Film resistivity: 2.9 Ω·cm, low-temperature boron doping efficiency approximately 33%; 4. Residual stress: No cracking or peeling observed; 5. Surface morphology: The diamond grains have a uniform polycrystalline structure and no obvious amorphous carbon and graphite phase impurities.
[0051] This embodiment successfully solved the technical bottlenecks of difficult diamond film nucleation on aluminum-based surfaces, interface stress cracking, and low-temperature doping efficiency by pretreatment synergistic optimization, staged gas process design, and stress control technology. The boron-doped diamond film prepared has excellent comprehensive performance and can be applied to high-end application scenarios such as high-power electronic heat dissipation and electrodes in highly corrosive environments.
[0052] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on its differences from other embodiments. Similar or identical parts between embodiments can be referred to interchangeably. For the apparatus disclosed in the embodiments, since they correspond to the methods disclosed in the embodiments, the description is relatively simple; relevant parts can be referred to the method section.
[0053] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing boron-doped diamond films on aluminum substrates based on microwave plasma chemical vapor deposition, characterized in that, Includes the following steps: (1) Pretreatment of aluminum substrate: Mechanical grinding or polishing is performed on the aluminum substrate to remove the surface oxide layer, followed by alkaline washing and ultrasonic cleaning; (2) Plasma pretreatment: Under Ar atmosphere, microwave plasma is used to etch the surface of aluminum substrate to remove residual contaminants and form a nanoscale rough structure; (3) Boron-doped diamond nucleation and deposition: methane, hydrogen, carbon dioxide and trimethylborane were introduced as reaction gases, and the diamond was deposited in stages under microwave power of 1.5-3.5kW, temperature of 400-550℃ and pressure of 15-60Torr. (4) Annealing treatment: Slowly cool to room temperature in an inert atmosphere to eliminate internal stress in the film.
2. The method for preparing boron-doped diamond films on aluminum substrates based on microwave plasma chemical vapor deposition according to claim 1, characterized in that, The alkaline washing in step (1) uses a mixed alkaline solution of sodium hydroxide and sodium phosphate, and the washing time is 5-10 minutes.
3. The method for preparing boron-doped diamond films on aluminum substrates based on microwave plasma chemical vapor deposition according to claim 1, characterized in that, The ultrasonic cleaning time in step (1) is more than 30 minutes.
4. The method for preparing boron-doped diamond films on aluminum substrates based on microwave plasma chemical vapor deposition according to claim 1, characterized in that, In step (2), etching is performed at 500°C and 2.0 kW using Ar. + Ion bombardment creates pit structures with a depth of 50-200 nm.
5. The method for preparing boron-doped diamond films on aluminum substrates based on microwave plasma chemical vapor deposition according to claim 1, characterized in that, The volume ratio of methane, hydrogen, carbon dioxide and trimethylborane in step (3) is methane: hydrogen: carbon dioxide: trimethylborane = 2-8%: 80-96%: 0.5-8%: 0.5-1.5%.
6. The method for preparing boron-doped diamond films on aluminum substrates based on microwave plasma chemical vapor deposition according to claim 5, characterized in that, The staged deposition described in step (3) includes: Nucleation stage: gas ratio methane:hydrogen:carbon dioxide:trimethylborane = 7-10%:85-90%:1-1.5%:0.5-1%, temperature 450-550℃, gas pressure 15-60 Torr, microwave power 1.5-2kW, deposition time 1-2 hours; Transitional growth stage: The gas ratio is adjusted to methane:hydrogen:carbon dioxide:trimethylborane = 3-5%:90-95%:0.5-1.5%:0.5-1%, temperature 500-540℃, gas pressure 25-30 Torr, microwave power 3.0kW, deposition time 2-3 hours; Thick film deposition stage: The gas ratio is further adjusted to methane:hydrogen:carbon dioxide:trimethylborane = 2-3%:94-97%:0.5-3%:0.3-1%, temperature 500-550℃, gas pressure 30-60 Torr, microwave power 2.5kW.
7. The method for preparing boron-doped diamond films on aluminum substrates based on microwave plasma chemical vapor deposition according to claim 1, characterized in that, The cooling rate of the annealing process in step (4) is ≤10℃ / min, and the inert gas is argon or nitrogen.
8. The method for preparing boron-doped diamond films on aluminum substrates based on microwave plasma chemical vapor deposition according to claim 1, characterized in that, The boron doping concentration of the boron-doped diamond film is 5 × 10⁻⁶. 19 –1×10 20 cm -3 The film thickness is 5-50 μm.