Horizontal copper plating solution suitable for high speed and low loss material and its application
By using a combination of complexing agents and surfactants in horizontal copper plating solutions, the problem of uneven copper layer formation on high-speed, low-loss materials in traditional horizontal copper plating solutions has been solved, achieving high-speed deposition and high-quality copper layer deposition effects.
Patent Information
- Application Number
- CN202611371077.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-20
AI Technical Summary
Traditional horizontal copper plating solutions struggle to form uniform and robust copper layers on high-speed, low-loss materials such as PTFE, liquid crystal polymers (LCP), and ultra-low Dk/Df modified epoxy resins, often resulting in issues like voids in the hole walls, copper layer peeling, or insufficient adhesion.
A composite complexing agent system consisting of tetrasodium iminodisuccinate, polyethyleneimine, tetramethylethylenediamine, and L-malic acid is used, combined with surfactants Surfynol 465 and propylene glycol block polyether F68. By adjusting the pH value, a horizontal copper deposition solution suitable for high-speed, low-loss materials is formed, which enhances the deposition stability and uniformity.
It significantly improves the speed and uniformity of horizontal copper plating, making it suitable for horizontal copper plating of high-speed, low-loss materials, and ensuring the integrity and reliability of the copper layer.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of copper plating technology, and relates to a horizontal copper plating solution suitable for high-speed, low-loss materials and its application. Background Technology
[0002] Horizontal copper plating, also known as hole metallization (PTH), is a key process in printed circuit board (PCB) manufacturing. Essentially, it's a self-catalyzed redox reaction: a continuous, dense copper layer is deposited on the non-conductive portions of the hole walls (such as resin substrates and glass fiber bundles) through a chemical reduction reaction, thus achieving electrical interconnection between multilayer circuits. Compared to traditional vertical copper plating lines, horizontal copper plating offers significant advantages such as shorter process time, enclosed equipment operation, high automation, and lower water and energy consumption. It has already achieved large-scale industrial applications in high-multilayer boards, high-density interconnect (HDI) boards, and packaging substrates. However, high-speed, low-loss PCB substrates (such as PTFE, liquid crystal polymer LCP, and ultra-low Dk / Df modified epoxy resins) have low surface energy and strong chemical inertness, making it difficult for traditional copper plating solutions to form a uniform and robust copper layer, easily leading to problems such as hole wall voids, copper layer peeling, or insufficient adhesion. Therefore, there is an urgent need to develop a horizontal copper plating solution suitable for high-speed, low-loss materials to adapt to the special surface characteristics and process window requirements of advanced high-frequency substrates. Summary of the Invention
[0003] The purpose of this invention is to provide a horizontal copper plating solution suitable for high-speed, low-loss materials and its application. The horizontal copper plating solution prepared by this invention effectively improves the speed and uniformity of horizontal copper plating and is suitable for horizontal copper plating treatment of high-speed, low-loss materials.
[0004] The objective of this invention can be achieved through the following technical solutions: In a first aspect, the present invention provides a horizontal copper plating solution suitable for high-speed, low-loss materials. The horizontal copper plating solution comprises the following components: copper source, complexing agent, reducing agent, accelerator, stabilizer, surfactant, and pH adjuster. The complexing agent is obtained by mixing tetrasodium iminodisuccinate, polyethyleneimine, tetramethylethylenediamine, and L-malic acid. The surfactant is obtained by mixing Surfynol 465 and propylene glycol block polyether F68.
[0005] Preferably, the horizontal copper plating solution comprises the following components: 7.8-9.4 g / L copper source, 28-32 g / L complexing agent, 13-17 g / L reducing agent, 0.01-0.04 g / L accelerator, 0.01-0.04 g / L stabilizer, 0.01-0.014 g / L surfactant, and an appropriate amount of pH adjuster.
[0006] Preferably, the copper source is selected from copper sulfate pentahydrate and / or copper acetate.
[0007] Preferably, the complexing agent is obtained by mixing tetrasodium iminodisuccinate, polyethyleneimine, tetramethylethylenediamine, and L-malic acid in a weight ratio of 4-6:1-2:0.5-1.5:0.5-1.
[0008] Preferably, the reducing agent is selected from formaldehyde and / or glyoxylic acid.
[0009] Preferably, the accelerator is selected from one or more of 2-mercaptobenzimidazole, tetrahydroxypropylethylenediamine, and dimethylaminopropionitrile.
[0010] Preferably, the stabilizer is selected from one or more of 2,2′-bipyridine, o-phenanthroline, and 8-hydroxyquinoline.
[0011] Preferably, the surfactant is obtained by mixing Surfynol 465 and propylene glycol block polyether F68 in a weight ratio of 1.5-2.5:3-5.
[0012] Preferably, the pH adjuster is sodium hydroxide.
[0013] In a second aspect, the present invention provides a method for preparing the horizontal copper plating solution suitable for high-speed, low-loss materials as described in the first aspect, comprising the following steps: The accelerator and stabilizer were dissolved in equal amounts of ethanol. Then, under stirring conditions, the copper source, complexing agent, pre-dissolved accelerator, pre-dissolved stabilizer, reducing agent, and surfactant were added to deionized water in sequence. After stirring evenly, the pH was adjusted to 12.5 using a pH adjuster to obtain the horizontal copper precipitation solution.
[0014] The third invention provides the application of the horizontal copper plating solution described in the first aspect in the horizontal copper plating of PCB high-frequency and high-speed boards.
[0015] The beneficial effects of this invention are: (1) This invention provides a horizontal copper plating solution suitable for high-speed, low-loss materials. The copper plating solution includes a composite complexing agent system composed of tetrasodium iminodisuccinate, polyethyleneimine, tetramethylethylenediamine, and L-malic acid. The strong coordination ability provided by tetrasodium iminodisuccinate prevents copper ions from precipitating or oxidizing in the solution, ensuring the stability of the copper plating process. Polyethyleneimine contains abundant primary, secondary, and tertiary amine groups, which can be adsorbed onto the pore wall surface through electrostatic interactions, enhancing adsorption efficiency. The two nitrogen atoms in the tetramethylethylenediamine molecule can act as lone pair electron donors, effectively binding metal ions. L-malic acid forms a stable complex with copper ions through hydroxyl and carboxyl groups, improving the uniformity of the coating. The four complexing agents synergistically enhance the stability of the copper plating solution, the uniformity of the coating, and its adaptability to high-speed substrates.
[0016] (2) The horizontal copper plating solution provided by the present invention includes a surfactant obtained by compounding Surfynol 465 and propylene glycol block polyether F68. Surfynol 465, as an acetylenol nonionic surfactant, has excellent dynamic wetting ability and low foaming characteristics. Under the high-speed movement of the horizontal copper plating line, it can spread rapidly on the low surface energy substrate. F68, as a polyether block copolymer, has both wetting and leveling functions. It forms a uniform adsorption layer in the corner of blind hole and deep hole area, and inhibits local over-deposition. The combination of the two can greatly improve the wettability of the hole wall and the integrity of the coating coverage.
[0017] (3) The horizontal copper plating solution prepared by the present invention can effectively improve the speed and uniformity of horizontal copper plating, and is suitable for horizontal copper plating treatment of high-speed, low-loss materials. Detailed Implementation
[0018] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with embodiments, is provided below.
[0019] Copper sulfate pentahydrate and copper acetate were purchased from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd.; tetrasodium iminodisuccinate, tetramethylethylenediamine, and L-malic acid were purchased from Wuhan Jiyesheng Chemical Co., Ltd.; polyethyleneimine was purchased from Shanghai Youen Chemical Co., Ltd., with a molecular weight of 1800; 2-mercaptobenzimidazole and tetrahydroxypropylethylenediamine were purchased from Zhongshan Dixin Chemical Co., Ltd.; dimethylaminopropionitrile was purchased from Wuhan Maikairui Chemical Co., Ltd.; 2,2′-bipyridine was purchased from Zhongshan Dixin Chemical Co., Ltd.; o-phenanthroline was purchased from Hubei Xinghengye Technology Co., Ltd.; 8-hydroxyquinoline was purchased from Hubei Langbowan Biomedical Co., Ltd.; Surfynol 465 was purchased from Jining Tangyi Chemical Co., Ltd.; and propylene glycol block polyether F68 was purchased from Jiangsu Jufeng Chemical Technology Co., Ltd.
[0020] Unless otherwise specified, all other materials, reagents, etc. used in all embodiments and comparative examples of this invention are commercially available.
[0021] The preparation methods of the horizontal copper plating solution described in Examples 1-3 all include the following steps: The accelerator and stabilizer were dissolved in equal amounts of ethanol. Then, under stirring conditions, the copper source, complexing agent, pre-dissolved accelerator, pre-dissolved stabilizer, reducing agent, and surfactant were added to deionized water in sequence. After stirring evenly, the pH was adjusted to 12.5 using a pH adjuster to obtain the horizontal copper precipitation solution.
[0022] Example 1 A horizontal copper plating solution suitable for high-speed, low-loss materials, comprising the following components: 8.6 g / L copper source (copper sulfate pentahydrate), 30 g / L complexing agent, 15 g / L reducing agent (formaldehyde), 0.025 g / L accelerator (2-mercaptobenzimidazole), 0.025 g / L stabilizer (2,2′-bipyridine), 0.012 g / L surfactant, and an appropriate amount of pH adjuster (sodium hydroxide). The complexing agent is obtained by mixing tetrasodium iminodisuccinate, polyethyleneimine, tetramethylethylenediamine, and L-malic acid in a weight ratio of 5:1.5:1:0.75. The surfactant is obtained by mixing Surfynol 465 and propylene glycol block polyether F68 in a weight ratio of 2:3.5.
[0023] Example 2 A horizontal copper plating solution suitable for high-speed, low-loss materials, wherein the raw materials of the horizontal copper plating solution include the following components: 7.8 g / L copper source (copper acetate), 28 g / L complexing agent, 13 g / L reducing agent (glyoxylic acid), 0.01 g / L accelerator (tetrahydroxypropylethylenediamine), 0.01 g / L stabilizer (o-phenanthroline), 0.01 g / L surfactant, and an appropriate amount of pH adjuster (sodium hydroxide). The complexing agent is obtained by mixing tetrasodium iminodisuccinate, polyethyleneimine, tetramethylethylenediamine, and L-malic acid in a weight ratio of 4:1:0.5:0.5. The surfactant is obtained by mixing Surfynol 465 and propylene glycol block polyether F68 in a weight ratio of 1.5:3.
[0024] Example 3 A horizontal copper plating solution suitable for high-speed, low-loss materials, wherein the raw materials of the horizontal copper plating solution include the following components: 9.4 g / L copper source (copper sulfate pentahydrate), 32 g / L complexing agent, 17 g / L reducing agent (formaldehyde and glyoxylic acid in a mass ratio of 1:1), 0.04 g / L accelerator (dimethylaminopropionitrile), 0.04 g / L stabilizer (8-hydroxyquinoline), 0.014 g / L surfactant, and an appropriate amount of pH adjuster (sodium hydroxide). The complexing agent is obtained by mixing tetrasodium iminodisuccinate, polyethyleneimine, tetramethylethylenediamine, and L-malic acid in a weight ratio of 6:2:1.5:1. The surfactant is obtained by mixing Surfynol 465 and propylene glycol block polyether F68 in a weight ratio of 2.5:5.
[0025] Comparative Example 1 Based on Example 1, in Comparative Example 1, tetrasodium iminodisuccinate was removed from the complexing agent, and the missing amount was made up with an equal weight of polyethyleneimine. Other conditions remained the same as in Example 1.
[0026] Comparative Example 2 Based on Example 1, Comparative Example 2 removed polyethyleneimine from the complexing agent, and the missing amount was made up with an equal weight of tetramethylethylenediamine, while other conditions remained the same as in Example 1.
[0027] Comparative Example 3 Based on Example 1, Comparative Example 3 removed tetramethylethylenediamine from the complexing agent, and the missing amount was made up with an equal weight of L-malic acid, while other conditions remained the same as in Example 1.
[0028] Comparative Example 4 Based on Example 1, Comparative Example 4 removed L-malic acid from the complexing agent, and the missing amount was made up with an equal weight of tetrasodium iminodisuccinate, while other conditions remained the same as in Example 1.
[0029] Comparative Example 5 Based on Example 1, the complexing agent of Comparative Example 5 was obtained by mixing tetrasodium iminodisuccinate, polyethyleneimine, tetramethylethylenediamine, and L-malic acid in a weight ratio of 0.75:1:5:1.5, with other conditions remaining the same as in Example 1.
[0030] Comparative Example 6 Based on Example 1, Surfynol 465 was removed from the surfactant in Comparative Example 6, and the missing amount was made up with an equal weight of propylene glycol block polyether F68. Other conditions remained the same as in Example 1.
[0031] Comparative Example 7 Based on Example 1, Comparative Example 7 removed propylene glycol block polyether F68 from the surfactant, and the missing amount was made up with an equal weight of Surfynol 465. Other conditions remained the same as in Example 1.
[0032] Comparative Example 8 Based on Example 1, the surfactant in Comparative Example 8 was obtained by mixing Surfynol 465 and propylene glycol block polyether F68 in a weight ratio of 3.5:2, with other conditions remaining the same as in Example 1.
[0033] Test Example 1: Deposition Rate Using the horizontal copper plating solutions prepared in Examples 1-3 and Comparative Examples 1-8 as samples, the substrates (15cm×15cm FR4 material) that had undergone expansion, desmearing, neutralization, adjustment, activation, and reduction were immersed in the samples for copper plating treatment. The samples were chemically plated at 30°C for 5 minutes, and the plating thickness was measured using an X-ray fluorescence thickness gauge. The deposition rate was calculated. Three parallel tests were performed on each group of samples, and the average test results were recorded as shown in Table 1 below.
[0034] Table 1 Deposition rate (μm / h) Example 1 14.1 Example 2 12.7 Example 3 13.6 Comparative Example 1 7.2 Comparative Example 2 8.5 Comparative Example 3 7.9 Comparative Example 4 8.8 Comparative Example 5 11.1 Comparative Example 6 9.5 Comparative Example 7 9.9 Comparative Example 8 10.4 As shown in Table 1, the horizontal copper plating solutions prepared in Examples 1-3 of this invention have good deposition rates and are suitable for horizontal copper plating treatment of high-speed PCBs and high-frequency and high-speed materials.
[0035] Test Example 2: Backlight Test The copper-plated samples were prepared according to the method in Test Example 1. The copper-plated samples were cut and ground in a slicing machine. The slicing hole was ground to half the diameter of the hole, and the other side of the slice was ground to 2 mm away from the edge of the hole. After grinding, copper shavings and other impurities in the hole were wiped clean. The hole was examined under a microscope at 50x magnification. The uniformity of the copper deposited layer in the hole was detected using the backlight principle. The backlight level was divided into 10 levels. The higher the backlight level, the better the backlight effect of the sample. The specific test results are recorded in Table 2 below.
[0036] Table 2 Backlight level / grade Example 1 10 Example 2 10 Example 3 10 Comparative Example 1 5 Comparative Example 2 6 Comparative Example 3 5 Comparative Example 4 6 Comparative Example 5 8 Comparative Example 6 7 Comparative Example 7 7 Comparative Example 8 8 As shown in Table 1, the horizontal copper plating solution prepared in Examples 1-3 of the present invention has good hole wettability and coverage, and the copper plating layer obtained by the treatment has good uniformity and stability, good backlight effect, and good reliability and application prospects.
[0037] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any indirect modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A horizontal copper plating solution suitable for high-speed, low-loss materials, characterized in that, The horizontal copper immersion solution comprises the following components: copper source, complexing agent, reducing agent, accelerator, stabilizer, surfactant, and pH adjuster. The complexing agent is obtained by mixing tetrasodium iminodisuccinate, polyethyleneimine, tetramethylethylenediamine, and L-malic acid. The surfactant is obtained by mixing Surfynol 465 and propylene glycol block polyether F68.
2. The horizontal copper immersion solution according to claim 1, characterized in that, The horizontal copper plating solution comprises the following components: 7.8-9.4 g / L copper source, 28-32 g / L complexing agent, 13-17 g / L reducing agent, 0.01-0.04 g / L accelerator, 0.01-0.04 g / L stabilizer, 0.01-0.014 g / L surfactant, and an appropriate amount of pH adjuster.
3. The horizontal copper immersion solution according to claim 1, characterized in that, The copper source is selected from copper sulfate pentahydrate and / or copper acetate.
4. The horizontal copper immersion solution according to claim 1, characterized in that, The complexing agent is obtained by mixing tetrasodium iminodisuccinate, polyethyleneimine, tetramethylethylenediamine, and L-malic acid in a weight ratio of 4-6:1-2:0.5-1.5:0.5-1.
5. The horizontal copper immersion solution according to claim 1, characterized in that, The reducing agent is selected from formaldehyde and / or glyoxylic acid.
6. The horizontal copper plating solution according to claim 1, characterized in that, The accelerator is selected from one or more of 2-mercaptobenzimidazole, tetrahydroxypropylethylenediamine, and dimethylaminopropionitrile.
7. The horizontal copper plating solution according to claim 1, characterized in that, The stabilizer is selected from one or more of 2,2′-bipyridine, o-phenanthroline, and 8-hydroxyquinoline.
8. The horizontal copper plating solution according to claim 1, characterized in that, The surfactant is obtained by mixing Surfynol 465 and propylene glycol block polyether F68 in a weight ratio of 1.5-2.5:3-5.
9. The method for preparing the horizontal copper immersion solution according to any one of claims 1-8, characterized in that, Includes the following steps: The accelerator and stabilizer are dissolved in equal amounts of ethanol. Then, under stirring conditions, the copper source, complexing agent, pre-dissolved accelerator, pre-dissolved stabilizer, reducing agent, and surfactant are added to deionized water in sequence. After stirring evenly, the pH is adjusted to 12.2-12.8 using a pH adjuster to obtain the horizontal copper precipitation solution.
10. The application of the horizontal copper plating solution according to any one of claims 1-8 in horizontal copper plating of PCB high-frequency and high-speed boards.