A method for preparing a lossless gold plating layer of photoresist and application thereof
By employing electrostatic adsorption of nano-gold particle suspension and cyanide-free chemical gold plating, the problem of photoresist dissolution and corrosion was solved, enabling the preparation of gold plating layers without damage to the photoresist. This method is suitable for high aspect ratio structures, and the plating layer has uniform thickness and good adhesion.
Patent Information
- Application Number
- CN202611275112.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-20
AI Technical Summary
In existing technologies, free cyanide ions can easily dissolve or corrode photoresist films, leading to risks such as electroplating pattern failure and interconnect short circuits. In particular, the problems of uneven coating thickness and process window sensitivity are difficult to solve in high aspect ratio structures.
A gold coating without photoresist damage was prepared by electrostatic adsorption deposition of a suspension of gold nanoparticles combined with a cyanide-free chemical gold plating process. The gold nanoparticle layer was formed on the substrate by electrostatic polarization and then fixed in a cyanide-free chemical gold plating solution.
It achieves non-destructive gold plating of photoresist, with high consistency between the plating structure and the photolithographic pattern. It is suitable for high aspect ratio structures, with uniform plating thickness and good adhesion, avoiding problems such as photoresist corrosion and uneven plating.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of gold plating process technology, specifically relating to a non-destructive gold plating preparation method for photoresist and its application. Background Technology
[0002] In semiconductor manufacturing, microelectromechanical systems (MEMS), and other fields, gold is widely used to fabricate structures such as bumps, pads, and interconnects due to its excellent electrical conductivity, chemical stability, and corrosion resistance. Preparing specific structures at the micron and nanoscale using photoresist and selectively depositing gold into these structures via electroplating is a key technology in micro / nano fabrication. Gold plating solutions generally include cyanide-free and cyanide-containing gold plating solutions.
[0003] Cyanide-free gold plating solutions are less stable and have lower dispersing power than cyanide systems. In high aspect ratio structures, they are prone to uneven coating thickness due to the effect of the electric field at the tip. Furthermore, the process window is quite sensitive to current density and anodic state, making it difficult to achieve both bottom coverage and top flatness in high aspect ratio structures. Therefore, they are not suitable for micro-nano fabrication.
[0004] Cyanide gold plating solutions are currently the most commonly used solution for micro and nano fabrication due to their mature stability, excellent quality, and superior dispersion and coverage. However, the free cyanide ions in cyanide gold plating solutions can easily dissolve or corrode the photoresist film, leading to problems such as plating penetration, coating etching, and photoresist shrinkage at the bottom of the photolithographic pattern. This can result in plating pattern failure and even short circuits in interconnects. Summary of the Invention
[0005] This invention provides a non-destructive method for preparing gold plating with photoresist and its application, in order to solve the problem that free cyanide ions can easily dissolve or corrode the photoresist film when preparing specific structures at the micron or even nanoscale by photoresist and electroplating gold deposition.
[0006] To solve the above-mentioned technical problems, the present invention provides a method for preparing a non-destructive gold plating layer using photoresist, which includes the following steps:
[0007] 1) Prepare a suspension of gold nanoparticles, wherein the surface of the gold nanoparticles is positively or negatively charged;
[0008] 2) Fabrication of micro / nano patterns: First, a seed layer is set on the substrate surface, and then the micro / nano patterns are displayed through a photoresist mask;
[0009] 3) Electrostatic adsorption: The substrate after development in step 2) is immersed in the nano-gold particle suspension in step 1), and a voltage opposite to the surface charge of the nano-gold particles is applied with the substrate as the working electrode. Under the action of the electric field, the nano-gold particles migrate to the substrate and are adsorbed and deposited in the patterned area to form a nano-gold layer.
[0010] 4) Chemical gold plating fixation: The substrate from which the gold nanoparticles were deposited in step 3) is removed, and a stable gold plating layer is formed by chemical gold plating without cyanide.
[0011] The autocatalytic deposition reaction of cyanide-free gold electroless plating has stringent requirements for the catalytic activity and continuity of the seed layer. When the seed layer is not dense or has insufficient activity, it is easy to encounter difficulties in starting the plating process, missed plating, or poor adhesion of the plating layer.
[0012] Optionally, the positively charged gold nanoparticle suspension is obtained by reacting an aqueous solution of chloroauric acid, cetyltrimethylammonium bromide (CTAB), and NaBH4.
[0013] Optionally, the molar ratio of NaBH4 to chloroauric acid is 2:1 to 4:1.
[0014] Optionally, the preparation method of the positively charged gold nanoparticle suspension is as follows: prepare a 0.25-1 mM (millimoles per liter) aqueous solution of chloroauric acid, add 0.1-5 wt% of CTAB aqueous solution, and then add 10 mM of NaBH4 aqueous solution under an ice-water bath, and continue stirring for 0.5-2 hours to prepare the gold nanoparticle suspension.
[0015] Optionally, the negatively charged gold nanoparticle suspension is obtained by reacting an aqueous solution of chloroauric acid with sodium citrate.
[0016] Optionally, the molar ratio of sodium citrate to chloroauric acid is 2:1 to 4:1.
[0017] Optionally, the preparation method of the negatively charged gold nanoparticle suspension is as follows: prepare a 0.25-1 mM chloroauric acid aqueous solution, add a 40 mM sodium citrate aqueous solution while heating to boiling, stop heating, and continue stirring for 0.5-2 hours to obtain the gold nanoparticle suspension.
[0018] Optionally, the particle size of the gold nanoparticles is 3-500 nm.
[0019] Optionally, the concentration of the gold nanoparticle suspension in step 3) is 0.1-1.0 mg / mL.
[0020] Optionally, in step 2), the seed layer on the substrate surface is formed sequentially by physical vapor deposition of a titanium metal layer and a copper metal layer.
[0021] Optionally, in step 3), when the surface of the gold nanoparticles is positively charged, a voltage of -0.5 to -2V is applied between the substrate and the counter electrode; when the surface of the gold nanoparticles is negatively charged, a voltage of 0.5 to 2V is applied between the substrate and the counter electrode.
[0022] Optionally, in step 3), the electrostatic adsorption deposition time is 10-120 minutes, until the deposition thickness reaches 70-90% of the final coating target thickness.
[0023] Optionally, in step 4), the gold plating solution used for chemical gold plating is selected from a sulfite system, a thiosulfate system, or a hydantoin system.
[0024] The present invention also provides a MEMS processing method, which uses the above-mentioned photoresist non-destructive gold plating preparation method to form bumps, pads or interconnects made of gold on a substrate.
[0025] The technical solution provided by this invention first prepares charged gold nanoparticles, then uses electrochemical polarization to electrostatically deposit and adsorb the gold nanoparticles onto a substrate with a seed layer and a photoresist mask. Finally, a cyanide-free electroless gold plating solution is used to allow the gold nanoparticle layers to intergrow and form a stable gold plating structure. The above technical solution is non-corrosive to the photoresist film, ensuring high selectivity and consistency between the plating structure and the photolithographic pattern; it can achieve submicron-level precise positioning and deposition; by adjusting the electric field strength and suspension concentration, it can promote the entry of gold nanoparticles into deep holes, making it suitable for high aspect ratio structures; in addition, the electrostatic deposition results in a uniform plating thickness. Detailed Implementation
[0026] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0027] Example 1:
[0028] 1. Preparation of gold nanoparticle suspension:
[0029] Preparation of positively charged gold nanoparticles: Prepare a 1 mM aqueous solution of chloroauric acid, add 3 wt% aqueous solution of CTAB and stir to dissolve. Under ice-water bath and vigorous stirring, add 10 mM aqueous solution of NaBH4, with a molar ratio of NaBH4 to chloroauric acid of 3:1. Stir continuously for 1 hour to prepare a suspension of positively charged gold nanoparticles with a particle size of 20 nm.
[0030] After the reaction was completed, the gold nanoparticles were concentrated to 0.5 mg / mL by centrifugation and washing with water three times.
[0031] 2. Photolithography and development:
[0032] Ti and Cu metal layers were sequentially deposited on a silicon substrate using physical vapor deposition as seed layers. Then, a 20×20μm square block pattern was obtained through photolithography. The photoresist used was AZ4620, a positive photoresist.
[0033] 3. Electrostatic adsorption deposition:
[0034] The substrate was immersed in a gold nanoparticle suspension and used as the working electrode. A voltage of -1V was applied, and the suspension was stirred at a certain speed for 10 minutes. Finally, a gold nanoparticle layer with a thickness of 500nm was deposited in the square block pattern area.
[0035] 4. Post-processing: Remove the substrate with the deposited gold nanolayer, gently rinse it with ultrapure water and dry it with nitrogen gas, then immerse the substrate in a cyanide-free electroless gold plating solution of thiosulfate system at 65℃ for 15 minutes, and then rinse it with water.
[0036] The preparation method of the cyanide-free electroless gold plating solution of the thiosulfate system is as follows: 30 g of sodium thiosulfate, 12 g of anhydrous sodium sulfite, 18 g of disodium hydrogen phosphate, and 2.5 g of sodium dihydrogen phosphate are added sequentially to 800 mL of deionized water under stirring in a water bath at 30-40 ℃, and stirred until completely dissolved to form a colorless and transparent base solution. Separately, a small amount of deionized water is used to pre-dissolve approximately 3.5 g of chloroauric acid, which is then slowly added dropwise to the above base solution under continuous stirring to obtain a light yellow transparent gold plating solution stock solution. After the stock solution cools to room temperature, 15 g of sodium hypophosphite is added, stirred until dissolved, and then diluted to 1 L with deionized water. The pH is then finely adjusted to 8.0±0.2 using 1 mol / L sodium hydroxide solution or 1 mol / L phosphoric acid to complete the preparation.
[0037] 5. After removing the adhesive, a gold plating layer is obtained. The gold plating layer is uniform and bright, and there is no plating penetration at the edges. The plating pattern is consistent with the photolithography pattern. The critical load Lc of the nano-scratch test is ≥1.5N, indicating that it has good adhesion to the seed layer. The plating layer thickness is about 680nm.
[0038] Example 2:
[0039] 1. Preparation of gold nanoparticle suspension:
[0040] Preparation of negatively charged gold nanoparticles: Prepare a 1 mM aqueous solution of chloroauric acid, add a 40 mM aqueous solution of sodium citrate while stirring vigorously and heating to boiling, and then stop heating. The molar ratio of sodium citrate to chloroauric acid is 3:1. Continue stirring for 1 hour to obtain a suspension of negatively charged gold nanoparticles with a particle size of 30 nm.
[0041] After the reaction was completed, the gold nanoparticles were concentrated to 0.5 mg / mL by centrifugation and washing with water three times.
[0042] 2. Photolithography and development:
[0043] Ti and Cu metal layers were sequentially deposited on a silicon substrate using physical vapor deposition as seed layers. Then, a circular pattern with a diameter of 50 μm was obtained through photolithography. The photoresist used was NR26-12000P, a negative photoresist.
[0044] 3. Electrostatic adsorption deposition:
[0045] The substrate was immersed in a gold nanoparticle suspension and used as the working electrode. A voltage of +1V was applied, and the suspension was stirred at a certain speed for 10 minutes. Finally, a gold nanoparticle layer with a thickness of 800nm was deposited in the circular pattern area.
[0046] 4. Post-processing: Remove the substrate with the deposited gold nanolayer, rinse it gently with ultrapure water and dry it with nitrogen gas, and then immerse the substrate in the cyanide-free electroless gold plating solution of the thiosulfate system prepared in Example 1 at 65°C for 15 min.
[0047] 5. After removing the adhesive, a gold plating layer is obtained. The gold plating layer is uniform and bright, and there is no plating penetration at the edges. The plating pattern is consistent with the photolithography pattern. The critical load Lc of the nano-scratch test is ≥2.0N, indicating that it has good adhesion to the seed layer. The plating thickness is about 1μm.
[0048] Example 3:
[0049] 1. Preparation of gold nanoparticle suspension:
[0050] Preparation of positively charged gold nanoparticles: A 1 mM aqueous solution of chloroauric acid was prepared, and 3 wt% CTAB aqueous solution was added and stirred to dissolve. Under ice-water bath and vigorous stirring, a 10 mM aqueous solution of NaBH4 (molar ratio of NaBH4 to chloroauric acid 3:1) was added, and stirring continued for 1 hour to prepare a suspension of positively charged gold nanoparticles with a particle size of 20 nm.
[0051] After the reaction was completed, the gold nanoparticles were concentrated to 0.5 mg / mL by centrifugation and washing with water three times.
[0052] 2. Photolithography and development:
[0053] Ti and Cu metal layers were sequentially deposited as seed layers on an aluminum substrate with a 45μm deep hole and an opening of 30μm×30μm. Then, a 50×50μm circular pattern was obtained by photolithography. The deep hole was located at the center of the circular pattern. The photoresist was NR26-12000P, a negative photoresist.
[0054] 3. Electrostatic adsorption deposition:
[0055] The substrate was immersed in a gold nanoparticle suspension and used as the working electrode. A voltage of -1V was applied, and the suspension was stirred at a certain speed for 30 minutes. Finally, a gold nanoparticle layer was deposited in the circular pattern area. The gold nanoparticle layer filled the deep pore and rose 1.8 μm.
[0056] 4. Post-processing: Remove the substrate with deposited gold nanoparticles, gently rinse with ultrapure water and dry with nitrogen, and then immerse the substrate in the cyanide-free electroless gold plating solution of the thiosulfate system prepared in Example 1 at 65°C for 15 min.
[0057] 5. After removing the adhesive, a gold plating layer is obtained. The gold plating layer is uniform and bright, and there is no plating penetration at the edges. The plating pattern is consistent with the photolithography pattern. The critical load Lc of the nano-scratch test at the top of the deep hole is ≥2.5N, indicating that it has good adhesion to the seed layer. The thickness of the gold plating layer at the bottom of the deep hole is about 2μm, and the thickness of the gold plating layer at the top of the deep hole is about 2.1μm. The plating thickness is uniform.
[0058] Example 3 demonstrates the feasibility of using a suspension of positively charged gold nanoparticles for gold plating in deep-pore structures.
[0059] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein, and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a non-destructive gold plating layer using photoresist, characterized in that, Includes the following steps: 1) Prepare a suspension of gold nanoparticles, wherein the surface of the gold nanoparticles is positively or negatively charged; 2) Fabrication of micro / nano patterns: First, a seed layer is set on the substrate surface, and then the micro / nano patterns are displayed through a photoresist mask; 3) Electrostatic adsorption: The substrate after development in step 2) is immersed in the nano-gold particle suspension in step 1), and a voltage opposite to the surface charge of the nano-gold particles is applied with the substrate as the working electrode. Under the action of the electric field, the nano-gold particles migrate to the substrate and are adsorbed and deposited in the patterned area to form a nano-gold layer. 4) Chemical gold plating fixation: Take out the substrate from step 3) where gold nanoparticles were deposited, and use a cyanide-free chemical gold plating process to form a stable gold plating layer for the gold nanoparticles.
2. The method for preparing a non-destructive gold plating layer using photoresist according to claim 1, characterized in that, The positively charged gold nanoparticle suspension was obtained by reacting chloroauric acid aqueous solution, CTAB and NaBH4.
3. The method for preparing a non-destructive gold plating layer using photoresist according to claim 2, characterized in that, The molar ratio of NaBH4 to chloroauric acid is 2:1 to 4:
1.
4. The method for preparing a non-destructive gold plating layer using photoresist according to claim 1, characterized in that, The suspension of negatively charged gold nanoparticles was obtained by reacting an aqueous solution of chloroauric acid with sodium citrate.
5. The method for preparing a non-destructive gold plating layer using photoresist according to claim 4, characterized in that, The molar ratio of sodium citrate to chloroauric acid is 2:1 to 4:
1.
6. The method for preparing a non-destructive gold plating layer using photoresist according to claim 1, characterized in that, The concentration of the gold nanoparticle suspension mentioned in step 3) is 0.1-1.0 mg / mL.
7. The method for preparing a non-destructive gold plating layer using photoresist according to claim 1, characterized in that, The particle size of the gold nanoparticles is 3-500 nm.
8. The method for preparing a non-destructive gold plating layer using photoresist according to claim 1, characterized in that, In step 3), when the surface of the gold nanoparticles is positively charged, a voltage of -0.5 to -2V is applied between the substrate and the counter electrode; when the surface of the gold nanoparticles is negatively charged, a voltage of 0.5 to 2V is applied between the substrate and the counter electrode.
9. The method for preparing a non-destructive gold plating layer using photoresist according to claim 1, characterized in that, In step 3), the electrostatic adsorption deposition time is 10-120 minutes, until the deposition thickness reaches 70-90% of the final coating target thickness.
10. A MEMS fabrication method, characterized in that, The gold plating layer preparation method of photoresist without damage as described in any of claims 1-9 is used to form bumps, pads or interconnects made of gold on a substrate.