Titanium alloy wire modification method and application
By using laser processing to create a micro-grid pit texture, vacuum annealing, and chemical conversion solution treatment, the problems of irregular surface texture and weak coating adhesion of titanium alloy wires have been solved. This has resulted in multi-layer composite modification with high wear resistance and corrosion resistance, making it suitable for aerospace fasteners.
Patent Information
- Application Number
- CN202611637061.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-22
- Publication Date
- 2026-11-20
AI Technical Summary
Existing titanium alloy wire modification processes suffer from irregular surface texture, high coating porosity, and weak bonding, resulting in uneven wear and corrosion resistance, which makes it difficult to meet the requirements of high-end aerospace fasteners.
Laser processing with wavelengths of 1050–1080 nm and pulse widths of 80–120 ns was used to fabricate micro-grid pit textures. Combined with vacuum annealing, chemical conversion solution treatment, and sealing agent treatment, a multi-layer composite modified structure was formed, including ceramicization and sealing steps, to optimize grain arrangement and interface bonding.
It significantly improves the interfacial bonding strength between the ceramic coating and the wire substrate, optimizes the surface microstructure density, enhances the lubrication and buffering effect and wear and corrosion resistance of the titanium alloy wire, and meets the service requirements of high-end aerospace fasteners.
Smart Images

Figure CN123132869A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal material surface treatment technology, specifically relating to a method for modifying titanium alloy wire and its application. Background Technology
[0002] Titanium alloys have become a core structural material in the aerospace field due to their advantages such as high specific strength, excellent mechanical properties, low density, and good high-temperature stability. Aerospace fasteners made from titanium alloy wire are the core connecting components of key parts such as aircraft fuselage, wings, and aero engines. Their stability directly determines the overall safety and service life of aerospace equipment.
[0003] Currently, conventional titanium alloy wires, without modification, exhibit problems such as a loose oxide film, poor surface smoothness, high coefficient of friction, and weak resistance to acid and alkali corrosion. In the complex service environment of aviation, fasteners are subjected to alternating loads, air oxidation, trace acid and alkali erosion, and friction and wear over long periods, making them highly susceptible to surface wear, pitting, and seizing failures. This significantly shortens the service life of aviation fasteners and increases maintenance costs and safety hazards for aviation equipment.
[0004] Existing titanium alloy wire modification processes mostly employ single methods such as anodic oxidation, ordinary chemical coating, or simple heat treatment, resulting in limited process complexity and poor synergy. Traditional laser modification often uses high-power, long-pulse lasers, which easily cause thermal damage and stress concentration on the wire surface, failing to create a regular and stable surface texture. Conventional chemical conversion coatings have a single composition, high porosity, and limited protective performance. Ordinary pore sealing treatments can only achieve simple pore plugging and cannot impart lubrication and wear resistance to the wire. Furthermore, existing modification processes do not achieve integrated and synergistic processing of surface texture construction, grain optimization, ceramic coating growth, pore sealing, and curing strengthening. The modified titanium alloy wires prepared exhibit defects such as weak coating adhesion, uneven wear and corrosion resistance, and poor stability, making it difficult to meet the stringent requirements of high-end aerospace fasteners.
[0005] To address the comprehensive problems in existing titanium alloy wire modification processes, such as irregular surface texture, high coating porosity, weak film-substrate adhesion, and uneven wear and corrosion resistance, there is an urgent need to develop a synergistic modification method that can comprehensively improve the wear resistance, corrosion resistance, and lubrication performance of titanium alloy wire surfaces. Summary of the Invention
[0006] To overcome the problems of existing titanium alloy wire modification processes being limited, having irregular surface textures, high coating porosity, weak bonding strength, poor wear and corrosion resistance, and insufficient stability, a method for modifying titanium alloy wire and its application are provided.
[0007] To achieve the above objectives, the present invention provides a method for modifying titanium alloy wire, comprising the following steps: S1. Laser scanning is performed on titanium alloy wire with a wavelength of 1050-1080nm and a pulse width of 80-120ns to process a micro-grid pit texture on the surface of the titanium alloy wire, thus obtaining a textured wire.
[0008] S2. The textured filament is placed in a vacuum of ≤1×1 Annealing was performed at 580–620°C for 2–6 minutes, followed by cooling to room temperature to obtain annealed filament.
[0009] S3. Place the annealed wire in a chemical conversion solution and immerse it at 60-80℃ for 10-20 minutes to obtain ceramicized wire.
[0010] S4. Place the ceramicized filament in the sealing agent and ultrasonically impregnate for 10-15 minutes to obtain the sealing filament.
[0011] S5. The sealing wire is heated and cured to obtain modified titanium alloy wire.
[0012] Preferably, in S1, the titanium alloy wire is any one of TC4 (Ti-6Al-4V), TC11 (Ti-6.5Al-3.5Mo-1.5Zr-0.3Si), and TA15 (Ti-6.5Al-2Zr-1Mo-1V).
[0013] Preferably, in step S1, the traction speed of the titanium alloy wire during laser scanning is 1–3 m / min; the laser scanning is performed under an argon inert protective atmosphere with an argon flow rate of 15–25 L / min; and the width of the pits in the micro-grid pit texture is 50–80 μm, the depth is 15–20 μm, and the axial and circumferential spacing is 180–220 μm.
[0014] Preferably, in step S3, the chemical conversion solution comprises 20–30 g / L of hydrogen peroxide, 10–20 g / L of ammonium fluorozirconate, 0.8–3 g / L of sodium molybdate, 5–15 g / L of boric acid, and 1.2–3.5 g / L of modified tannic acid, and the pH value of the chemical conversion solution is 3.5–4.5.
[0015] Preferably, the modified tannic acid is prepared by dissolving tannic acid in anhydrous ethanol to prepare a tannic acid ethanol solution with a mass fraction of 8-12%; adding KH550 (γ-aminopropyltriethoxysilane) dropwise to the tannic acid ethanol solution, adding glacial acetic acid to adjust the pH of the system to 4.8-5.5, stirring at 55-65°C for 2.5-3.5 h, followed by rotary evaporation and vacuum drying to obtain modified tannic acid; the mass ratio of tannic acid to KH550 is 1:0.18-0.25.
[0016] Preferably, in step S4, the sealing agent includes polyamic acid, nano-lubricating filler, nonionic surfactant, and N-methylpyrrolidone; the mass of the polyamic acid is 15-25% of the total mass of the sealing agent; the mass of the nano-lubricating filler is 8-15% of the total mass of the sealing agent; the mass of the nonionic surfactant is 0.3-0.8% of the total mass of the sealing agent; and the balance is N-methylpyrrolidone.
[0017] Preferably, the nano-lubricating filler is composed of nano-molybdenum disulfide and nano-PTFE (polytetrafluoroethylene) in a mass ratio of 1:2 to 3, wherein the particle size of the nano-molybdenum disulfide is 40 to 60 nm and the particle size of the nano-PTFE is 70 to 90 nm.
[0018] Preferably, the nonionic surfactant is AEO-9 (fatty alcohol polyoxyethylene ether).
[0019] Preferably, in step S4, the vibration frequency of ultrasonic impregnation is 35–45 kHz, and the power of ultrasonic impregnation is 180–220 W.
[0020] Preferably, in step S5, the heating and curing is carried out under a nitrogen atmosphere, and the heating and curing includes three stages: the first stage is to keep the temperature at 110-130℃ for 15-25 minutes, the second stage is to keep the temperature at 240-260℃ for 25-35 minutes, and the third stage is to keep the temperature at 300-320℃ for 50-70 minutes.
[0021] This invention also provides the application of titanium alloy wire prepared by the above method in the field of aerospace fasteners.
[0022] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention uses laser scanning for precise etching to prepare a micro-grid pit texture, which can significantly increase the effective contact area between the substrate and the subsequent coating, forming a mechanically interlocking and anchoring structure. This can significantly improve the interfacial bonding strength between the ceramic coating, the sealing layer and the wire substrate, providing a stable interfacial bearing foundation for multi-layer composite modified structures. At the same time, the micro-grid pit texture can store lubricating media, providing a continuous lubrication and buffering effect on the surface of the titanium alloy wire.
[0023] 2. The annealing process of this invention can eliminate residual tensile stress generated on the surface of the wire during laser etching, avoiding problems such as coating cracking and microcrack propagation in the substrate caused by residual stress during long-term service. Simultaneously, it can optimize the uniformity of surface grain arrangement, improve the density and mechanical uniformity of the titanium alloy wire substrate surface structure, enhance the interfacial compatibility and bonding stability between the substrate and subsequent ceramic coatings, and the low-temperature, short-time process can effectively avoid the problems of coarse grains and overall strength and toughness reduction in the titanium alloy substrate caused by high-temperature heat treatment, thus simultaneously ensuring the structural strength and interfacial performance of the titanium alloy wire.
[0024] 3. The modified tannic acid added to the chemical conversion solution of this invention is grafted with KH550, introducing silanoxy and phenolic hydroxyl groups into its molecular structure. This allows for the formation of chemical bonds between the titanium alloy surface and the ceramic coating, effectively enhancing the adhesion of the ceramic coating to the substrate. Simultaneously, the phenolic hydroxyl and benzene ring structures retained in the modified tannic acid molecule possess a certain complexing ability, enabling coordination with zirconium and molybdate ions in the chemical conversion solution. This promotes the uniform formation of crystal nuclei and the refinement of grain growth, resulting in a denser and more uniform ceramic coating. The introduction of sodium molybdate allows for the in-situ generation of a lubricating molybdate transfer film on the contact surface during friction, reducing the coefficient of friction.
[0025] 4. The polyamic acid in the sealing agent of this invention possesses excellent film-forming properties and adhesion, enabling the formation of a uniform and dense organic protective film on the ceramic coating surface. The nano-molybdenum disulfide and nano-PTFE bicomponent lubricating filler synergistically exert a solid self-lubricating effect, significantly reducing the surface friction coefficient of the wire, weakening wear loss during frictional contact, effectively improving the smoothness of aerospace fastener assembly, and significantly enhancing the wear resistance and anti-galling ability of fasteners under long-term reciprocating friction service conditions. AEO-9 effectively reduces the interfacial tension of the sealing layer, improves the wetting, dispersion, and suspension stability of the nano-lubricating filler in the system, avoids the agglomeration and sedimentation of nano-powders, and ensures the uniform distribution of lubricating components within the sealing layer. Simultaneously, the surfactant enhances the permeability of the sealing liquid, allowing the sealing components to fully penetrate the micropores of the ceramic coating, improving the uniformity of pore sealing, and ensuring the overall uniformity and stability of the sealing layer. Attached Figure Description
[0026] The present invention will be further described with reference to the accompanying drawings, but the embodiments in the drawings do not constitute any limitation on the present invention. For those skilled in the art, other drawings can be obtained based on the following drawings without creative effort.
[0027] Figure 1 This is a schematic flowchart of the titanium alloy wire modification method of the present invention; Figure 2 The graph shows the corrosion current density test results of the titanium alloy wire of this invention. Figure 3 The figure shows the results of the oxidation weight gain test of the titanium alloy wire of this invention. Detailed Implementation
[0028] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0029] All raw materials used in this invention are commercially available.
[0030] Example 1: This embodiment provides a method for modifying titanium alloy wire, including the following steps: S1. A TC4 titanium alloy wire with a diameter of 2.5 mm is fed to the laser processing area at a traction speed of 2 m / min. Under an argon protective atmosphere (argon flow rate of 20 L / min), laser scanning is performed with a laser wavelength of 1064 nm and a pulse width of 100 ns. A micro-grid pit texture is processed on the surface of the wire. The width of the pits in the micro-grid pit texture is 65 μm, the depth is 18 μm, and the axial spacing and circumferential spacing are both 200 μm, thus obtaining a textured wire.
[0031] S2. Place the textured filament in a vacuum heat treatment furnace with a vacuum degree of 5×1 Pa, heated to 600℃, held for 4 minutes for annealing, and then cooled to room temperature to obtain annealed filament.
[0032] S3. Prepare the chemical conversion solution: 25 g / L hydrogen peroxide, 15 g / L ammonium fluorozirconate, 1.8 g / L sodium molybdate, 10 g / L boric acid, and 2.2 g / L modified tannic acid. Adjust the pH to 4.0 with ammonia. Immerse the annealed wire in the chemical conversion solution at 70°C for 15 minutes, then rinse with deionized water to obtain the ceramicized wire.
[0033] The modified tannic acid is prepared by dissolving tannic acid in anhydrous ethanol to prepare a 10% solution, adding KH550 (the mass ratio of tannic acid to KH550 is 1:0.22), adjusting the pH value to 5.0 with glacial acetic acid, stirring at 60℃ for 3 hours, and then drying under vacuum after rotary evaporation to obtain modified tannic acid.
[0034] S4. Preparation of sealing agent: Polyamic acid accounts for 20% of the total mass of the sealing agent, nano-lubricating filler (a mixture of molybdenum disulfide with a particle size of 50 nm and PTFE with a particle size of 80 nm in a mass ratio of 1:2.5) accounts for 12% of the total mass of the sealing agent, AEO-9 accounts for 0.5% of the total mass of the sealing agent, and the balance is N-methylpyrrolidone. The ceramicized filament is placed in the sealing agent and ultrasonically impregnated for 12 minutes at 40 kHz and 200 W. After removal and draining, the sealing filament is obtained.
[0035] S5. Place the sealing wire in a nitrogen atmosphere tube furnace for heating and curing: the first stage is 120℃ for 20 min, the second stage is 250℃ for 30 min, the third stage is 310℃ for 60 min, and then naturally cool to room temperature to obtain the modified titanium alloy wire.
[0036] Example 2: This embodiment provides a method for modifying titanium alloy wire, including the following steps: S1. A TC11 titanium alloy wire with a diameter of 2.5 mm is fed to the laser processing area at a traction speed of 3 m / min. Laser scanning is performed under an argon protective atmosphere (argon flow rate of 25 L / min). The laser wavelength is 1080 nm and the pulse width is 120 ns. A micro-grid pit texture is processed on the surface of the wire. The pit width in the micro-grid pit texture is 80 μm, the depth is 20 μm, and the axial spacing and circumferential spacing are both 220 μm, thus obtaining a textured wire.
[0037] S2. Place the textured filament in a vacuum heat treatment furnace with a vacuum level of 1×1 Pa, heated to 620℃, held for 6 minutes for annealing, and then cooled to room temperature to obtain annealed filament.
[0038] S3. Prepare the chemical conversion solution: 30 g / L hydrogen peroxide, 20 g / L ammonium fluorozirconate, 3 g / L sodium molybdate, 15 g / L boric acid, and 3.5 g / L modified tannic acid. Adjust the pH to 4.5 with ammonia. Immerse the annealed filament in the chemical conversion solution at 70°C for 15 minutes, then rinse with deionized water to obtain the ceramicized filament.
[0039] The modified tannic acid is prepared by dissolving tannic acid in anhydrous ethanol to prepare a 12% mass fraction solution, adding KH550 dropwise (the mass ratio of tannic acid to KH550 is 1:0.25), adding glacial acetic acid to adjust the pH value to 5.5, stirring at 65℃ for 3.5h, and then drying under vacuum after rotary evaporation to obtain modified tannic acid.
[0040] S4. Preparation of sealing agent: Polyamic acid accounts for 25% of the total mass of the sealing agent, nano-lubricating filler (a mixture of molybdenum disulfide with a particle size of 60 nm and PTFE with a particle size of 90 nm in a mass ratio of 1:3) accounts for 15% of the total mass of the sealing agent, AEO-9 accounts for 0.8% of the total mass of the sealing agent, and the balance is N-methylpyrrolidone. The ceramicized filament is placed in the sealing agent and ultrasonically impregnated for 15 min at 45 kHz and 220 W. After removal and draining, the sealing filament is obtained.
[0041] S5. Place the sealing wire in a nitrogen atmosphere tube furnace for heating and curing: hold at 130℃ for 25 minutes in the first stage, at 260℃ for 35 minutes in the second stage, and at 320℃ for 70 minutes in the third stage. Then, allow it to cool naturally to room temperature to obtain the modified titanium alloy wire.
[0042] Example 3: S1. A TA15 titanium alloy wire with a diameter of 2.5 mm is fed to the laser processing area at a traction speed of 1 m / min. Under an argon protective atmosphere (argon flow rate of 15 L / min), laser scanning is performed with a laser wavelength of 1050 nm and a pulse width of 80 ns. A micro-grid pit texture is processed on the surface of the wire. The width of the pits in the micro-grid pit texture is 50 μm, the depth is 15 μm, and the axial spacing and circumferential spacing are both 180 μm, thus obtaining a textured wire.
[0043] S2. Place the textured filament in a vacuum heat treatment furnace with a vacuum level of 1×1 Pa, heated to 580℃, held for 2 minutes for annealing, and then cooled to room temperature to obtain annealed filament.
[0044] S3. Prepare the chemical conversion solution: 20 g / L hydrogen peroxide, 10 g / L ammonium fluorozirconate, 0.8 g / L sodium molybdate, 5 g / L boric acid, and 1.2 g / L modified tannic acid. Adjust the pH to 3.5 with ammonia. Immerse the annealed filament in the chemical conversion solution at 60°C for 10 minutes, then rinse with deionized water to obtain the ceramicized filament.
[0045] The modified tannic acid is prepared by dissolving tannic acid in anhydrous ethanol to prepare a solution with a mass fraction of 8%, adding KH550 dropwise (the mass ratio of tannic acid to KH550 is 1:0.18), adding glacial acetic acid to adjust the pH value to 4.8, stirring at 55℃ for 2.5 h, and then drying under vacuum after rotary evaporation to obtain modified tannic acid.
[0046] S4. Preparation of sealing agent: Polyamic acid accounts for 15% of the total mass of the sealing agent, nano-lubricating filler (a mixture of molybdenum disulfide with a particle size of 60 nm and PTFE with a particle size of 90 nm in a mass ratio of 1:2) accounts for 8% of the total mass of the sealing agent, AEO-9 accounts for 0.3% of the total mass of the sealing agent, and the balance is N-methylpyrrolidone. The ceramicized filament is placed in the sealing agent and ultrasonically impregnated for 10 min at 35 kHz and 180 W. After removal, it is drained to obtain the sealing filament.
[0047] S5. Place the sealing wire in a nitrogen atmosphere tube furnace for heating and curing: the first stage is 110℃ for 15 min, the second stage is 240℃ for 25 min, the third stage is 300℃ for 50 min, and then naturally cool to room temperature to obtain the modified titanium alloy wire.
[0048] Comparative Example 1: The difference between this comparative example and Example 1 is that the laser scanning process is removed, and the titanium alloy wire is directly annealed. All other parameters and processes are completely consistent with Example 1.
[0049] Comparative Example 2: The difference between this comparative example and Example 1 is that the modified tannic acid in the chemical conversion solution is replaced with unmodified tannic acid. All other parameters and processes are completely consistent with Example 1.
[0050] Comparative Example 3: The difference between this comparative example and Example 1 is that the nano-lubricating filler in the sealing agent is removed, and only polyamic acid, AEO-9, and N-methylpyrrolidone are used to formulate the sealing agent. All other parameters and processes are completely consistent with Example 1.
[0051] The titanium alloy wires prepared in the various embodiments and comparative examples of this invention were tested according to the following methods: 1. Surface roughness measurement: The surface roughness of the titanium alloy wire was measured at multiple points using a surface roughness meter. Six different test points were selected in the axial and circumferential directions for each sample to measure the surface roughness. The arithmetic mean of the six test data was taken as the surface roughness result.
[0052] 2. Film Thickness Measurement: The thickness of the ceramic coating on the surface of the titanium alloy wire was measured using an eddy current thickness gauge. Ten measurement points were evenly marked along the length of each sample. Each measurement point was measured three times at 120° intervals along the circumference, resulting in a total of 30 thickness data points. The arithmetic mean was taken as the film thickness of that sample. For samples where the eddy current method was insufficient, a metallographic section method was used for verification: the wire was inlaid, ground, and polished, and the film thickness was observed and measured under a metallographic microscope at 500x magnification.
[0053] 3. Film Adhesion Test: The film adhesion test was conducted using the cross-cut test method. A special cross-cut tool was used to cut a 1mm grid on the sample surface, penetrating the surface film to the titanium alloy substrate. Special adhesive tape was then tightly adhered to the grid area, and the tape was quickly and vertically peeled off. The film peeling in the grid area was observed under a microscope, and the adhesion grade was determined according to the grading rules for the cross-cut test specified in GB / T9286-2021 "Paints and Varnishes - Cross-cut Test". GB / T9286-2021 classifies the film bonding strength into levels 0 to 5 based on the proportion of the area of film peeling off within the grid area to the total area of the grid area: Level 0: The cut edge is completely smooth, and there is no film peeling off at the grid intersections or within the squares; Level 1: A small amount of film peeling off at the cut intersections, with the affected area not exceeding 5%; Level 2: Significant film peeling off at the cut edge and / or intersections, with the affected area greater than 5% but not exceeding 15%; Level 3: The film peeling off partially or completely along the cut edge in large fragments, with the affected area greater than 15% but not exceeding 35%; Level 4: The film peeling off along the cut edge in large fragments or partially or completely in a square, with the affected area greater than 35% but not exceeding 65%; Level 5: The area of film peeling off is greater than 65%. The smaller the level number, the stronger the bonding strength between the film and the fiber matrix, with level 0 being the best.
[0054] 4. Tribological Performance Testing: The tribological properties of the film layer on the wire surface were tested under dry friction conditions using a tribological testing machine. The wire was straightened and fixed to the test platform using a special fixture. A reciprocating friction test was conducted by sliding the friction pair along the axial direction of the wire. The test parameters were set as follows: normal load 5N, reciprocating frequency 5Hz, sliding stroke 5mm, and total friction time 30min. The testing machine automatically recorded the real-time friction coefficient, and the average value during the stable phase (last 25min) was taken as the average friction coefficient. After the test, the cross-sectional area of the wear track on the wire surface was measured using a three-dimensional profilometer, and the wear rate was calculated using the following formula: Wear rate = Wear track volume / (Normal load × Sliding distance). The test was repeated at three different locations for each sample, and the average value was taken.
[0055] 5. Corrosion resistance was evaluated using potentiodynamic polarization curve testing on an electrochemical workstation. A three-electrode system was employed: the sample as the working electrode, a platinum sheet as the auxiliary electrode, and a saturated calomel electrode as the reference electrode. The electrolyte was a 3.5 wt% NaCl solution. Before testing, the sample was immersed in the solution, and scanning began after the open-circuit potential stabilized. The potentiodynamic scanning range was set to -250 mV to +250 mV relative to the open-circuit potential, with a scan rate of 0.5 mV / s. IR downcorrection was applied to the test data. Among them, IR drop refers to the ohmic potential drop (valued as I×Rs) generated when the polarization current I flows through the electrolyte resistance Rs between the reference electrode and the working electrode during the potentiodynamic polarization test. This potential drop causes the instrument's measured potential Emeasured to deviate from the true potential Etrue on the surface of the working electrode. IR drop correction involves first measuring the solution resistance Rs using positive feedback compensation, current interruption method, or high-frequency intercept method of electrochemical impedance spectroscopy at an electrochemical workstation, and then subtracting this ohmic potential drop point by point from the potential value of each data point on the polarization curve according to Etrue = Emeasured - I×Rs. Based on the sample exposure area (1c... The current was converted into current density, and a linear segment of the strongly polarized region was selected for linear fitting. The corrosion current density was obtained by Tafel extrapolation.
[0056] 6. Microhardness Measurement: The surface hardness of the film was measured using a microhardness tester. HV0.05 (load 0.49N) was used when the film thickness was greater than 15μm, and HV0.025 (load 0.245N) was used when the film thickness was less than 15μm. The holding time was set to 15s for both. Ten test points were evenly selected on the surface of each sample, with the center-to-center distance between adjacent indentations not less than three times the diagonal length of the indentation. After testing, the diagonal length of the indentation was measured and the Vickers hardness value was calculated. The maximum and minimum values were discarded, and the average value was taken.
[0057] 7. Tensile mechanical property determination: The titanium alloy wires of each group were subjected to room temperature tensile tests using an electronic universal testing machine. A fixed tensile rate was set, and the tensile strength and elongation after fracture of the specimens were tested. Each group of tests was repeated 3 times, and the average value was taken.
[0058] 8. Determination of High-Temperature Oxidation Resistance: The wire was cut into 50mm lengths, cleaned and dried, and its initial mass was measured using an analytical balance with an accuracy of 0.01mg. The sample was placed in an alumina crucible preheated to constant weight and oxidized at 500℃ in air atmosphere with a temperature control accuracy of ±3℃. The crucible was removed after 24h, 48h, 72h, and 100h of oxidation, cooled to room temperature in a desiccator, and weighed. The weight gain per unit area (mg / cm²) was calculated. The area is calculated based on the geometric area of the outer surface of the titanium alloy wire. The average value of three parallel samples is taken at each time point.
[0059] The test results of the above embodiments and comparative examples are shown in Tables 1-3 and Figures 2-3 As shown.
[0060] Table 1: Test results of physical properties of surface film layer of titanium alloy wire Table 1 shows the test results of the physical properties of the surface film of the titanium alloy wire. Examples 1-3 of this invention, through the micro-grid pit texture combined with the filling and leveling effect of the modified composite film, effectively controlled the surface roughness of the titanium alloy wire within the range of 0.88–1.12 μm. Comparative Example 1, lacking the laser scanning process, resulted in insufficient substrate anchoring sites, a slight decrease in film uniformity, and a surface roughness of 1.05 μm. In Comparative Example 2, the unmodified tannic acid without silane grafting modification had poor interfacial compatibility with the titanium alloy wire, failing to form effective chemical bonding and cross-linking. This significantly reduced the film-forming reaction activity of the chemical conversion solution, leading to uneven film deposition, numerous micropores, cracks, and localized film defects, ultimately resulting in a surface roughness as high as 2.86 μm and poor surface smoothness. In Comparative Example 3, after removing the nano-lubricating filler, the sealing layer could not effectively fill the micropores and pits in the film, deteriorating the surface micro-smoothness and achieving a roughness of 1.53 μm.
[0061] Examples 1-3 demonstrate sufficient film thickness and continuous, complete formation, creating a uniform and stable physical protective barrier on the surface of titanium alloy wires, effectively blocking external corrosion, friction, and high-temperature environments from eroding the titanium alloy wires. Example 1 exhibits the optimal process parameters, resulting in the largest film thickness and the fullest protective layer. Comparative Example 1, lacking the laser scanning process, has few reactive sites on the titanium alloy wire surface, leading to low chemical conversion film deposition efficiency, discontinuous film formation, insufficient sealing layer adhesion, and a film thickness of only 12.3 μm, failing to form a complete protective system. Comparative Example 2 uses unmodified tannic acid, resulting in insufficient cross-linking reaction activity, reduced ceramic coating deposition, and a lower overall film thickness of 16.1 μm. Comparative Example 3 removes the nano-lubricating filler, resulting in no particle-filled thickening effect in the sealing layer, and a decrease in film density and fullness, demonstrating that the process components of this invention have a significant synergistic effect on increasing film thickness and ensuring protective integrity.
[0062] The surface hardness of Examples 1-3 of this invention reaches 412-438 HV, and the film layer exhibits excellent resistance to extrusion, scratches, and deformation. Comparative Example 1, due to the removal of the laser scanning process, has a thin and porous film layer with extremely low ceramic coating phase content, resulting in a surface hardness of only 365 HV and a significant decrease in surface deformation resistance. Comparative Example 2, with its unmodified tannic acid film uniformity and low crystallinity of the ceramic coating, suffers from insufficient hardening effect, resulting in a surface hardness of 401 HV. Comparative Example 3, lacking nano-lubricating filler, shows a decrease in the overall structural toughness and strength of the film layer, as well as a decrease in surface hardness, demonstrating that the nano-lubricating filler not only possesses lubrication function but also effectively improves the surface hardness and structural stability of the film layer. In the modified system of this invention, the ceramic coating and the nano-lubricating filler work synergistically to enhance the surface film layer's density and structural strength, achieving a surface strengthening effect.
[0063] In Examples 1 and 2 of this invention, the modified titanium alloy wire film adhesion strength reaches Grade 0, indicating a tight bond between the film and the substrate. In Example 3, due to relatively mild process parameters, the film adhesion strength is Grade 1, still meeting the requirements for high-end industrial applications. In Comparative Example 1, without the laser scanning process, the film adheres to the substrate surface solely through physical adsorption, resulting in weak interfacial bonding strength. Significant film detachment occurs during cross-cut adhesion testing, with an adhesion strength of only Grade 2. In Comparative Example 2, the lack of interfacial chemical bonding leads to poor film-substrate bonding stability, resulting in large-area film detachment and peeling during cross-cut adhesion testing, with an adhesion strength of only Grade 2. In Comparative Example 3, lacking the toughening and reinforcing effect and interfacial filling of nano-lubricating fillers, the internal stress of the sealing layer cannot be effectively released, leading to decreased interfacial stability. This fully verifies the advantages of the process of this invention in improving film adhesion stability. This invention employs a micro-grid pit texture pretreatment, modified tannic acid chemical conversion, and nano-lubricating filler synergistic modification process to construct a composite protective film layer with excellent comprehensive physical properties on the surface of titanium alloy wire. It can stably obtain high-quality modified titanium alloy wire with regular morphology, dense structure, strong bonding, and strong deformation resistance, significantly improving the physical protection performance and stability of the titanium alloy wire surface.
[0064] Table 2: Test results of tribological properties of titanium alloy wire As can be seen from the test results of the tribological properties of titanium alloy wire in Table 2, the present invention, through the synergistic modification system of micro-grid pit texture pretreatment, modified tannic acid ceramic coating, and nano-lubricating filler composite sealing, enabled the samples of Examples 1-3 to obtain excellent friction reduction and wear resistance. The average friction coefficient of each group of examples was only 0.16-0.21, and the wear rate was controlled between 1.85 and 2.46 × 10⁻⁶. m Within the range of / (N·m). In Comparative Example 1, without the laser scanning process, the titanium alloy wire surface exhibits irregular micro-pit structures, and the film layer is thin and loosely formed, failing to form an effective hard support and lubrication bearing system. This results in high interfacial frictional resistance, with the average friction coefficient increasing to 0.35 and the wear rate reaching 4.89 × 10⁻⁶. m / (N·m), the wear resistance and friction reduction properties are basically lost. Comparative Example 2 uses unmodified tannic acid, and the prepared ceramic coating is loose and porous, with low crystallinity and poor structural stability. During friction, the film layer is prone to problems such as microcrack propagation, large-scale peeling, and local damage. It cannot provide a stable hard support carrier for the friction interface, the lubrication sealing layer loses its adhesion basis, and the interfacial friction resistance increases; at the same time, the protective barrier of the film layer fails, the substrate is directly exposed to the friction interface, and the wear loss is greatly aggravated, with a wear rate as high as 5.16×1 m / (N·m), the wear-resistant and friction-reducing properties failed. Comparative Example 3, by removing the nano-lubricating filler and relying solely on a single ceramic coating to achieve wear resistance, failed to reduce friction, resulting in a lack of lubrication compensation at the friction interface and a significant increase in wear loss.
[0065] This invention constructs a wear-resistant and friction-reducing system on the surface of titanium alloy wire through multi-process synergistic modification, effectively solving the technical problems of high friction coefficient, large wear, poor friction interface stability, and easy wear failure of traditional titanium alloy wire. By rationally matching the micro-grid pit texture parameters, modified tannic acid film-forming formula, and nano-lubricating filler system, low-friction, high-wear-resistant modified titanium alloy wire can be stably obtained, which can significantly extend the service life of titanium alloy wire under reciprocating friction and dynamic wear conditions, and is suitable for various industrial applications with high precision and high wear resistance requirements.
[0066] Table 3: Test results of tensile mechanical properties of titanium alloy wire As shown in Table 3, the tensile mechanical properties of the titanium alloy wires in Examples 1-3, after being treated with the modified process of this invention, exhibit excellent and balanced tensile mechanical properties. The tensile strength of each group of samples is stable between 985 and 1060 MPa, and the elongation after fracture is maintained between 13.8% and 15.1%, indicating a good match between the strength and plasticity of the matrix. In Comparative Example 1, the removal of the laser scanning process slightly reduced the plasticity of the titanium alloy wire matrix, decreasing the elongation after fracture to 13.5% and the tensile strength to 1010 MPa. The overall mechanical properties were less balanced than those of the example samples. Comparative Example 2 used unmodified tannic acid, which could not form a stable chemical bond with the titanium alloy wire matrix. The membrane-matrix interface had numerous micro-gaps and structural defects, easily leading to stress concentration. Under tensile load, the membrane layer was prone to cracking and peeling, resulting in local stress imbalance in the titanium alloy wire matrix. Ultimately, this caused the tensile strength to drop to 972 MPa and the elongation after fracture to only 12.8%, with both tensile strength and elongation after fracture decreasing significantly. In Comparative Example 3, the tensile strength of the titanium alloy wire slightly improved after removing the nano-lubricating filler, but the plasticity index showed no significant advantage, and the overall strength-plasticity matching degree was not as good as that of the titanium alloy wire prepared by the modification process of this invention. The composite modification process adopted in this invention can construct a high-performance protective film layer on the surface of the titanium alloy wire while completely preserving and optimizing the tensile mechanical properties of the wire matrix. This allows the modified titanium alloy wire to have both high tensile strength and good plasticity, effectively ensuring the structural integrity and dimensional stability of aerospace fasteners under harsh service conditions such as high-altitude complex loads, alternating tension, vibration and impact. It can stably withstand tensile loads during the assembly and operation of aerospace equipment, and is not prone to fracture or deformation failure, greatly improving the service reliability and service life of aerospace fasteners, and can meet the usage requirements of high-end fasteners in the aerospace field.
[0067] Depend on Figure 2 The corrosion current density measurements show that this invention, through a multi-layered synergistic protection mechanism—including micro-grid pit texture activation of the substrate, efficient complexation film formation with modified tannic acid, and synergistic pore sealing with nano-lubricating fillers—can form a dense, continuous, and defect-free composite protective film on the surface of titanium alloy wire. This effectively seals micropores, blocks the penetration channels of corrosive media, and significantly reduces the corrosion reaction kinetic rate. The corrosion current densities in Examples 1-3 are only 0.42-0.62 μA / c. The overall corrosion level was low. In Comparative Example 1, the micro-grid pit texture pretreatment process was omitted, resulting in a lack of microscopic anchoring and activation sites in the substrate. The chemical conversion film deposition was uneven, the film layer was loose and porous, and numerous penetrating corrosion channels existed, allowing corrosive media to easily penetrate the substrate. The corrosion current density was 1.48 μA / c. The corrosion resistance was significantly deteriorated. Comparative Example 2, using unmodified tannic acid, showed low cross-linking, resulting in a porous film with numerous penetrating corrosion channels. This allowed the corrosive medium to rapidly penetrate the substrate, leading to a substantial increase in corrosion current density to 1.86 μA / c. Comparative Example 3, after removing the nano-lubricating filler, showed that the sealing layer could not completely fill the micropores of the ceramic coating, resulting in insufficient film sealing and residual trace corrosion diffusion channels. The corrosion current density was 0.68 μA / c. The results are slightly higher than those of the modified embodiment of the present invention, which fully demonstrates that the synergistic effect of laser scanning, modified tannic acid and nano-lubricating filler is the key to achieving high corrosion resistance of titanium alloy wire.
[0068] pass Figure 3 High-temperature weight gain test data under different oxidation durations show that, under a high-temperature air environment of 500℃ and a long-term constant-temperature oxidation condition of 24h to 100h, the oxidation weight gain of the titanium alloy wires in each group of examples remained at a low level throughout the entire process, and the weight gain rate was slow and stable with the extension of oxidation time. Comparative Example 1, without the laser scanning process, has weak anchoring bond between the film layer and the substrate, and the film layer is loose and porous. At high temperatures, it is prone to micropore expansion, film layer cracking and detachment, and increased oxygen molecule permeation rate, resulting in increased oxidation weight gain at all time points and decreased high-temperature protection capability. Comparative Example 2 uses unmodified tannic acid to form a film. The film layer has insufficient cross-linking density and many micro-defects, failing to form a long-term high-temperature shielding barrier. With the extension of oxidation time, the oxidation weight gain continues to increase, reaching as high as 1.38 mg / cm² after 100h. The high-temperature oxidation resistance of the sample in Comparative Example 3 was far inferior to that of the sample in the example. With the removal of the nano-lubricating filler, the stability of the sealing layer structure was insufficient, failing to effectively seal the micropores in the film layer. Under long-term high-temperature conditions, the pores gradually expanded, allowing oxygen molecules to continuously permeate, resulting in a significant shortcoming in long-term high-temperature protection performance. This invention, through a micro-grid pit texture synergistically modified tannic acid to form a dense film, combined with a nano-lubricating filler system, forms a continuous and highly dense composite protective film on the surface of the filament. This film can stably block the diffusion of high-temperature oxygen molecules into the matrix, effectively inhibiting the high-temperature oxidation reaction of the titanium alloy matrix and significantly delaying the high-temperature oxidation process. This invention can significantly improve the structural stability of aerospace fasteners under harsh conditions such as high altitude, high temperature, continuous thermal cycling, and long-term service, effectively delaying high-temperature oxidation failure, dimensional degradation, and performance decline of fasteners. It ensures the assembly accuracy, connection reliability, and structural safety of aerospace fasteners during long-term service, effectively extending the high-temperature service life of aerospace fasteners and meeting the long-term stable assembly and use requirements of aerospace equipment under high-temperature conditions.
[0069] In summary, this invention, through a surface modification process that combines micro-grid pit texture pretreatment, modified tannic acid-assisted chemical conversion, and nano-lubricating fillers, effectively improves the film thickness, density, and film-substrate bonding strength without compromising the mechanical properties of titanium alloy wire. It significantly reduces the coefficient of friction and wear rate, greatly enhances the electrochemical corrosion resistance and long-term high-temperature oxidation resistance of the titanium alloy wire, and enables the modified titanium alloy wire to possess excellent tensile strength, surface hardness, wear resistance, corrosion resistance, and high-temperature stability. This fully meets the high-precision, high-reliability, and long-life service requirements of aerospace fasteners under complex, harsh, and long-term service conditions.
[0070] The above are merely specific embodiments of the present invention, but the technical features of the present invention are not limited thereto. Any simple changes, equivalent substitutions, or modifications made based on the present invention to solve essentially the same technical problems and achieve essentially the same technical effects are all covered within the protection scope of the present invention.
Claims
1. A method for modifying titanium alloy wire, characterized in that, Includes the following steps: S1. Laser scanning is performed on titanium alloy wire with a wavelength of 1050-1080nm and a pulse width of 80-120ns to process a micro-grid pit texture on the surface of the titanium alloy wire, thus obtaining a textured wire. S2. The textured filaments are placed in a vacuum of ≤1×1 Annealing was performed at 580–620℃ for 2–6 minutes, followed by cooling to room temperature to obtain annealed filament. S3. Place the annealed wire in a chemical conversion solution and immerse it at 60-80℃ for 10-20 minutes to obtain ceramicized wire; S4. Place the ceramicized filament in the sealing agent and ultrasonically impregnate for 10-15 minutes to obtain the sealing filament; S5. The sealing wire is heated and cured to obtain modified titanium alloy wire.
2. The method for modifying titanium alloy wire according to claim 1, characterized in that, In S1, the titanium alloy wire is any one of TC4, TC11, and TA15.
3. The method for modifying titanium alloy wire according to claim 1, characterized in that, In step S1, the traction speed of the titanium alloy wire during laser scanning is 1–3 m / min; the laser scanning is performed under an argon inert protective atmosphere with an argon flow rate of 15–25 L / min; the width of the pits in the micro-grid pit texture is 50–80 μm, the depth is 15–20 μm, and the axial and circumferential spacing is 180–220 μm.
4. The method for modifying titanium alloy wire according to claim 1, characterized in that, In step S3, the chemical conversion solution comprises 20–30 g / L of hydrogen peroxide, 10–20 g / L of ammonium fluorozirconate, 0.8–3 g / L of sodium molybdate, 5–15 g / L of boric acid, and 1.2–3.5 g / L of modified tannic acid, and the pH value of the chemical conversion solution is 3.5–4.
5.
5. The method for modifying titanium alloy wire according to claim 4, characterized in that, The modified tannic acid is prepared by dissolving tannic acid in anhydrous ethanol to prepare a tannic acid ethanol solution with a mass fraction of 8-12%; adding KH550 dropwise to the tannic acid ethanol solution, adding glacial acetic acid to adjust the pH of the system to 4.8-5.5, stirring at 55-65℃ for 2.5-3.5 h, followed by rotary evaporation and vacuum drying to obtain modified tannic acid; the mass ratio of tannic acid to KH550 is 1:0.18-0.
25.
6. The method for modifying titanium alloy wire according to claim 1, characterized in that, In S4, the sealing agent includes polyamic acid, nano-lubricating filler, nonionic surfactant, and N-methylpyrrolidone; The mass of the polyamic acid is 15-25% of the total mass of the sealing agent; the mass of the nano-lubricating filler is 8-15% of the total mass of the sealing agent; the mass of the nonionic surfactant is 0.3-0.8% of the total mass of the sealing agent; and the balance is N-methylpyrrolidone. The nano-lubricating filler is composed of nano-molybdenum disulfide and nano-PTFE in a mass ratio of 1:2 to 3, with the nano-molybdenum disulfide having a particle size of 40 to 60 nm and the nano-PTFE having a particle size of 70 to 90 nm. The nonionic surfactant is AEO-9.
7. The method for modifying titanium alloy wire according to claim 1, characterized in that, In step S4, the vibration frequency of ultrasonic impregnation is 35–45 kHz, and the power of ultrasonic impregnation is 180–220 W.
8. The method for modifying titanium alloy wire according to claim 1, characterized in that, In step S5, the heating and curing is carried out under a nitrogen atmosphere and includes three stages: the first stage is to keep the temperature at 110-130℃ for 15-25 minutes, the second stage is to keep the temperature at 240-260℃ for 25-35 minutes, and the third stage is to keep the temperature at 300-320℃ for 50-70 minutes.
9. The application of titanium alloy wire prepared by the method according to any one of claims 1 to 8 in the field of aerospace fasteners.