A refractory alloy surface oxide ceramic-silicide composite oxidation-resistant coating and a method for preparing the same
By preparing an oxide ceramic-silicide composite coating on the surface of refractory alloys, the problem of insufficient oxidation resistance of refractory alloys at high temperatures was solved, and effective protection and mass production at 1800℃ were achieved.
Patent Information
- Application Number
- CN202511849464.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-09
- Publication Date
- 2026-11-20
AI Technical Summary
Existing refractory alloy coatings have insufficient oxidation resistance at high temperatures, leading to performance degradation in oxidizing environments and affecting their application in high-temperature environments.
An oxide ceramic-silicide composite coating structure is adopted, including an outer oxide ceramic layer, an MSi₂ type silicide intermediate layer, and an M₅Si₃ type silicide inner layer. Through gradient design and the addition of modifying elements, an antioxidant protection system of "external heat resistance + internal oxygen barrier" is formed.
It improves the high-temperature oxidation resistance of the coating, enabling it to effectively protect the substrate at 1800℃, reduce the service temperature of the internal silicide coating, and is suitable for mass production of complex components.
Smart Images

Figure CN123132874A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of antioxidant coating technology, and in particular to a composite antioxidant coating of oxide ceramic-silicide on the surface of refractory alloys and its preparation method. Background Technology
[0002] The information disclosed in the background section of this invention is intended only to enhance the understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.
[0003] In the aerospace and nuclear industries, high-temperature metallic structural materials have always held a crucial position and are considered key to leading industry development. Refractory metals (molybdenum, niobium, tantalum, tungsten) and their alloys possess advantages such as high melting points, excellent high-temperature strength, good processing performance, weldability, and excellent dynamic mechanical properties, making them ideal structural materials for operation in environments of 1600-1800 °C. However, the poor oxidation resistance of refractory alloys has always been one of the obstacles to their application in high-temperature aerobic environments. Refractory metals are chemically stable at room temperature, but as the temperature rises (above 500 °C), they undergo severe oxidation in air, with the resulting powdery or volatile oxidation products continuously peeling off or volatilizing, leading to catastrophic oxidation. Therefore, anti-oxidation coating technology is an essential key technology for ensuring the high-temperature service of refractory metals and alloys.
[0004] Among numerous coating systems, silicide coatings have high melting points and good thermal stability. The SiO2 formed on their surface during oxidation can effectively prevent oxygen from diffusing into the interior. In addition, SiO2 has a certain fluidity at high temperatures, giving the coating self-healing ability. Moreover, the process is simple and the cost is low. Therefore, it is currently the most widely used anti-oxidation coating on refractory alloy hot-end components both domestically and internationally.
[0005] However, the temperature resistance of a single silicide coating is insufficient, and modification with active elements is generally required. Common active elements include Al, Cr, Ti, B, Ge, Zr, Hf, and rare earth elements (Y, Ce). However, in existing technologies, the heat resistance of silicide coatings modified with active elements is not high; for example, the operating temperature of Si-Cr-Ti or Si-Cr-Fe silicide coating systems generally does not exceed 1400 ℃. To reduce the thrust chamber wall temperature to a level that the coating can withstand, a combined fuel film / radiation cooling method is used in the design. This cooling accounts for approximately 30% to 40% of the propellant flow. Therefore, measures to further improve the temperature resistance of the silicide coating and thus reduce propellant consumption have significant scientific and engineering value. Summary of the Invention
[0006] In view of this, the present invention provides an oxide ceramic-silicide composite anti-oxidation coating for refractory alloy surfaces and its preparation method, thereby overcoming the shortcomings of the prior art and obtaining an anti-oxidation coating with superior thermal protection capabilities.
[0007] To achieve the above objectives, the present invention is implemented through the following technical solution: In a first aspect, the present invention provides an oxide ceramic-silicide composite anti-oxidation coating for the surface of a refractory alloy, the anti-oxidation coating comprising an oxide ceramic-silicide outer layer, an MSi2 type silicide intermediate layer and an M5Si3 type silicide inner layer.
[0008] Furthermore, M in the silicides of the intermediate and inner layers is a solid solution of Mo, Ti, Cr, Zr and the matrix metal element.
[0009] Furthermore, in the oxide ceramic-silicide outer layer, the oxide ceramic is Al2O3, ZrO2 or HfO2; the silicide is MoSi2; wherein the mass fraction of the oxide ceramic is not less than 30%.
[0010] Furthermore, the refractory alloy is a niobium alloy, tantalum alloy, molybdenum alloy, or a high-entropy alloy composed of multiple refractory metal elements; wherein, the multiple refractory metal elements include, but are not limited to, Mo, Nb, Ta, Zr, W, Ti, Hf and other metal elements.
[0011] To improve the high-temperature oxidation resistance of silicide coatings, a high-melting-point, high-thermal-stability oxide ceramic phase was introduced for modification. A gradient structure design was adopted to form a composite structure of oxide ceramic-silicide outer layer / MSi2-type silicide intermediate layer / M5Si3-type silicide inner layer, establishing an "external heat resistance + internal oxygen barrier" anti-oxidation protection system. The high-melting-point composite ceramic outer layer provides high temperature resistance and ablation resistance. The MSi2-type silicide intermediate layer is a multi-component modified silicide phase; the addition of modifying elements Ti, Cr, and Zr promotes the selective formation of SiO2 on the silicide surface, improving oxygen barrier capacity. Furthermore, an M5Si3-type silicide inner layer exists at the interface between the coating and the substrate. This compositional gradient structure design, leveraging the continuous and gradual changes in composition, microstructure, and properties, transitions from the ceramic-silicide outer layer to the substrate alloy, further improving the thermophysical property matching between the coating and the substrate.
[0012] This invention proposes using oxide ceramics (Al2O3, ZrO2, or HfO2) to modify silicide coatings. On one hand, when operating in a high-temperature oxygen-containing atmosphere, the oxide ceramics are already the final oxidation product and do not directly participate in the chemical reaction with oxygen, exhibiting good structural thermal stability. These oxide ceramics can act as a "skeleton" for the SiO2 glass phase formed by the oxidation of silicides (MoSi2) in the early stages of oxidation, increasing the viscosity of the SiO2 film, reducing volatilization at high temperatures, and improving its resistance to high-temperature oxidation. On the other hand, compared to boride or carbide ceramics, oxide ceramics are less expensive, offering an economic advantage in mass production applications.
[0013] In a second aspect, the present invention provides a method for preparing a refractory alloy surface oxide ceramic-silicide composite anti-oxidation coating as described in the first aspect, comprising the following steps: (1) Mix Si, Cr, Ti, Mo and Zr elemental powders, ball mill them to obtain mixed powder I; then mix mixed powder I with a binder to obtain silicide coating slurry; (2) The silicide coating slurry is coated on the surface of the refractory alloy substrate, and after the first sintering, the coated alloy part I is obtained; (3) Si, Mo, MoSi2 and oxide ceramic powder are mixed and ball-milled to obtain mixed powder II. Mixed powder II is then mixed with a binder to obtain oxide ceramic-silicified material slurry. The oxide ceramic powder is Al2O3, ZrO2 or HfO2 oxide ceramic powder. (4) The oxide ceramic-silicified material slurry is coated on the coated alloy part I, and after a second sintering, the coated alloy part II is obtained. The surface coating of the refractory alloy part in the coated alloy part II is the refractory alloy surface anti-oxidation coating.
[0014] Furthermore, the method also includes a refractory alloy substrate pretreatment step, wherein the pretreatment operation is as follows: the substrate surface is sandblasted with corundum sand, ultrasonically cleaned with ethanol after sandblasting, etched with a hydrofluoric acid-nitric acid mixed solution, and finally cleaned with deionized water and dried.
[0015] Further, use anhydrous ethanol for ultrasonic cleaning for 10-20 minutes.
[0016] Furthermore, in the hydrofluoric acid-nitric acid mixed solution, the volume ratio of hydrofluoric acid to nitric acid is 1:2-4, and the etching time is 10-20 s.
[0017] Furthermore, the drying process involves drying at 80-100 ℃ for 4-6 hours.
[0018] Furthermore, in step (1), the mass percentage of elemental powders of Si, Cr, Ti, Mo, and Zr is 60-75% Si, 5-10% Cr, 5-10% Ti, 5-10% Mo, and 5-10% Zr.
[0019] Furthermore, in step (1), the purity of the elemental powders of Si, Cr, Ti, Mo, and Zr is higher than 99.5% and the particle size is less than 10 μm.
[0020] Furthermore, in step (1), the ball milling parameters are: ball milling at 300-350 r / min for 8-12 h.
[0021] Further, in step (1), the binder is a sodium carboxymethyl cellulose solution; the mass ratio of mixed powder I to binder is 90-95:5-10.
[0022] Furthermore, in step (2), the coating method includes brushing, dipping, or spraying.
[0023] Furthermore, in step (2), the coating thickness is 100-300 μm.
[0024] Further, in step (2), after coating, the coating is dried at 80-100 °C for 6-12 h.
[0025] Furthermore, in step (2), the first sintering temperature is 1450 ℃-1500 ℃, the sintering time is 30-45 min, and the vacuum degree is ≥1.0×10 -1 Pa.
[0026] Furthermore, the method also includes a post-treatment step for the coated alloy part I, specifically: brushing off surface powder, ultrasonically cleaning with ethanol for 10-20 min, and drying at 80-100 ℃ for 4-6 h.
[0027] Further, in step (3), the mass percentage of Si, Mo, MoSi2 and oxide ceramic powder is: 30~40% Si, 5-10% Mo, 10~20% MoSi2 and 30~40% oxide ceramic powder.
[0028] Furthermore, in step (3), the purity of Si, Mo, MoSi2 and oxide ceramic powders is higher than 99.5% and the particle size is less than 10 μm.
[0029] Furthermore, in step (3), the ball milling parameters are: ball milling at 300-350 r / min for 8-12 h.
[0030] Furthermore, in step (3), the binder is a silica sol with a modulus of 3.5, and the mass ratio of mixed powder II to binder is 85-95:5-15.
[0031] Furthermore, in step (4), the coating method includes brushing, dipping, or spraying.
[0032] Furthermore, in step (4), the coating thickness is approximately 50-150 μm.
[0033] Further, in step (4), after coating, the product is dried at 80-100 °C for 3-5 h.
[0034] Furthermore, in step (4), the second sintering temperature is 1600 ℃-1700 ℃, the sintering time is 20-40 min, and the vacuum degree is ≥1.0×10 -1 Pa.
[0035] Thirdly, the present invention provides the application of the composite antioxidant coating described in the first aspect or the composite antioxidant coating prepared by the preparation method described in the second aspect in the preparation of refractory metal alloys.
[0036] Furthermore, the composite antioxidant coating can be applied to environments up to 1800 °C.
[0037] Compared with the prior art, the present invention has achieved the following beneficial effects: (1) The anti-oxidation coating proposed in this invention, which can operate at 1800 ℃, is a composite structure of oxide ceramic-silicide outer layer / MSi2 type silicide intermediate layer / M5Si3 type silicide inner layer, adopting the thermal protection concept of "external heat resistance + internal oxygen barrier". Among them, the oxide ceramic-silicide outer layer has better temperature resistance and anti-oxidation performance, and the ceramic phase also has a certain thermal resistance, which reduces the service temperature of the internal silicide coating to a certain extent; the MSi2 type silicide intermediate layer is a multi-component modified silicide phase, and the addition of modifying elements promotes the selective generation of SiO2 on the silicide surface and improves the oxygen barrier capacity; there is also an M5Si3 type silicide inner layer at the interface between the coating and the substrate. This compositional gradient structure design, with the help of the continuous gradual change of composition, microstructure and physical properties, gradually transitions from the ceramic-silicide outer layer to the substrate alloy, further improving the thermal property matching between the coating and the substrate.
[0038] (2) The coating preparation method proposed in this invention adopts a two-stage slurry melting process. This process has the advantages of simple operation, low cost, and no constraints on the shape and size of the workpiece, and is suitable for the mass production of complex components. Attached Figure Description
[0039] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.
[0040] Figure 1 This is a process flow diagram of the preparation of oxide ceramic-silicide composite coatings using the secondary slurry melting method proposed in this invention; Figure 2 This is a cross-sectional microstructure diagram of the Al2O3 ceramic-silicide composite coating on the surface of the Nb521 niobium alloy provided in Embodiment 1 of the present invention; Figure 3 This is an enlarged morphology image of the outer layer of the Al2O3 ceramic-silicide composite coating on the surface of the Nb521 niobium alloy provided in Embodiment 1 of the present invention. Detailed Implementation
[0041] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0042] The technical solution of the present invention will be further described below with reference to specific embodiments.
[0043] Example 1 An oxide ceramic-silicide composite coating was prepared on the surface of Nb521 niobium alloy using the secondary slurry melting process proposed in this invention. The specific preparation steps are as follows: (1) Pretreatment of Nb521 niobium alloy substrate: The surface of the alloy substrate was sandblasted with corundum sand to obtain a roughness of Ra 3.2 μm; after sandblasting, it was ultrasonically cleaned with anhydrous ethanol for 15 min to remove residual sand particles and oil stains; then it was etched with a mixed solution of hydrofluoric acid and nitric acid (volume ratio 1:3) for 10 s to expose the fresh metal surface; finally, it was rinsed with deionized water and dried in a vacuum drying oven at 100 ℃ for 4 h.
[0044] (2) Weigh 68% Si, 8% Cr, 8% Ti, 8% Mo and 8% Zr powders according to mass percentage, wherein the purity of each powder is higher than 99.5% and the particle size is less than 10 μm. They are ball-milled for 10 hours in an agate ball mill jar at 300 r / min to obtain mixed powder I. Then mix mixed powder I with sodium carboxymethyl cellulose solution in a mass ratio of 92:8 to obtain silicide coating slurry.
[0045] (3) The silicide coating slurry was brushed onto the pretreated substrate alloy surface, with a coating thickness of approximately 200 μm. After vacuum drying at 80 ℃ for 12 h, it was placed in a vacuum high-temperature sintering furnace at a sintering temperature of 1450 ℃ and a vacuum degree of 1.0 × 10⁻⁶. 1 Pa, sintering time of 45 min, to obtain coated alloy part I.
[0046] (4) Use a soft brush to brush off the floating powder on the surface of the coated alloy part I, then use anhydrous ethanol for ultrasonic cleaning for 15 min, and then dry it in a vacuum drying oven at 100 ℃ for 4 h. (5) Weigh each powder according to the mass percentage, which is 40% Si, 5% Mo, 15% MoSi2 and 40% Al2O3. The purity of each powder is higher than 99.5% and the particle size is less than 10 μm. The powder is ball-milled in an agate ball mill jar at 350 r / min for 8 h to obtain mixed powder II. Then, mix mixed powder II with silica sol with a modulus of 3.5 at a mass ratio of 90:10 to obtain oxide ceramic-silicified material slurry. (6) The oxide ceramic-silicide slurry was brushed onto the surface of the pretreated silicide coating sample. The coating thickness was 100 μm. After drying at 80 ℃ for 5 h, the sample was placed in a vacuum high-temperature sintering furnace. The sintering temperature was 1600 ℃ and the vacuum degree was 1.0 × 10⁻⁶. 1 Pa, sintering time of 30 min, that is, an Al2O3 ceramic-silicide composite coating is obtained on the surface of niobium alloy.
[0047] The process flow diagram for preparing oxide ceramic-silicide composite coatings using a two-stage slurry sintering method proposed in this invention is shown below. Figure 1 As shown. The coated sample was wire-cut, and the cross-sectional microstructure of the coating was analyzed using scanning electron microscopy, as shown in the image. Figure 2 As shown, the coating thickness is approximately 200 μm, exhibiting a distinct layered structure. From the outside in, it consists of a 60 μm thick Al₂O₃-MoSi₂ outer layer, a 130 μm thick (Nb,Ti,Cr,Zr,Mo)Si₂ intermediate layer, and a 10 μm thick Nb₅Si₃ inner layer. The layers and interfaces with the substrate are metallurgically bonded, exhibiting high bonding strength and a relatively dense overall microstructure. No macroscopic defects such as cracks were observed. Figure 3 This is a magnified morphology image of the outer layer of the Al2O3 ceramic-silicide composite coating on the surface of the Nb521 niobium alloy provided in Embodiment 1 of the present invention, as shown below. Figure 3 As shown, the Al2O3 ceramic phase accounts for a relatively high proportion in this layer and has good interfacial compatibility with the MoSi2 silicide phase.
[0048] Example 2 An oxide ceramic-silicide composite coating was prepared on the surface of Ta10W tantalum alloy using the secondary slurry melting process proposed in this invention. The specific preparation steps are as follows: (1) The substrate surface was sandblasted with corundum sand to obtain a roughness of not less than Ra 3.2 μm; after sandblasting, it was ultrasonically cleaned with anhydrous ethanol for 15 min to remove residual sand particles and oil stains; then it was etched with a mixed solution of hydrofluoric acid and nitric acid (volume ratio 1:3) for 20 s to expose a fresh metal surface; finally, it was rinsed with deionized water and dried in a vacuum drying oven at 100 ℃ for 5 h.
[0049] (2) Weigh out 65% Si, 8% Cr, 10% Ti, 10% Mo and 7% Zr powders by mass percentage, wherein the purity of each powder is higher than 99.5% and the particle size is less than 10 μm. Use an agate ball mill jar to ball mill the powders at 300 r / min for 10 h to obtain mixed powder I. Then mix mixed powder I with sodium carboxymethyl cellulose solution at a mass ratio of 92:8 to obtain silicide coating slurry.
[0050] (3) The silicide coating slurry was brushed onto the pretreated substrate alloy surface, with a coating thickness of 200 μm. After vacuum drying at 100 ℃ for 6 h, it was placed in a vacuum high-temperature sintering furnace at a sintering temperature of 1500 ℃ and a vacuum degree of 1.0×10 1 Pa, sintering time of 45 min, to obtain coated alloy part I.
[0051] (4) First, use a soft brush to brush off the floating powder on the surface of the coated alloy part I, then use anhydrous ethanol for ultrasonic cleaning for 15 min, and then dry it in a vacuum drying oven at 80 ℃ for 6 h.
[0052] (5) Weigh each powder according to the mass percentage, which is 40% Si, 5% Mo, 20% MoSi2 and 35% HfO2. The purity of each powder is higher than 99.5% and the particle size is less than 10 μm. The powder is ball-milled in an agate ball mill jar at 350 r / min for 8 hours to obtain mixed powder II. Then, mix mixed powder II with silica sol with a modulus of 3.5 at a mass ratio of 95:5 to obtain oxide ceramic-silicified material slurry. (6) The oxide ceramic-silicide slurry was brushed onto the surface of the pretreated silicide coating sample. The thickness of the second coating was 150 μm. After drying at 80 ℃ for 5 h, the sample was placed in a vacuum high-temperature sintering furnace at a sintering temperature of 1700 ℃ and a vacuum degree of 1.0 × 10⁻⁶. 1Pa, sintering time of 40 min, that is, HfO2 ceramic-silicide composite coating is obtained on the surface of tantalum alloy.
[0053] Example 3 An oxide ceramic-silicide composite coating was prepared on the surface of TZM molybdenum alloy using the secondary slurry melting process proposed in this invention. The specific preparation steps are as follows: (1) The substrate surface was sandblasted with corundum sand to obtain a roughness of not less than Ra 3.2 μm; after sandblasting, it was ultrasonically cleaned with anhydrous ethanol for 15 min to remove residual sand particles and oil stains; then it was etched with a mixed solution of hydrofluoric acid and nitric acid (volume ratio 1:3) for 15 s to expose a fresh metal surface; finally, it was rinsed with deionized water and dried in a vacuum drying oven at 80 ℃ for 6 h.
[0054] (2) Weigh 70% Si, 10% Cr, 10% Ti, 5% Mo and 5% Zr powders according to mass percentage, wherein the purity of each powder is higher than 99.5% and the particle size is less than 10 μm. They are ball-milled for 8 hours in an agate ball mill at 300 r / min to obtain mixed powder I. Then, mix mixed powder I with sodium carboxymethyl cellulose solution at a mass ratio of 90:10 to obtain silicide coating slurry.
[0055] (3) The silicide coating slurry was brushed onto the pretreated substrate alloy surface, with a coating thickness of 300 μm. After vacuum drying at 80 ℃ for 12 h, it was placed in a vacuum high-temperature sintering furnace at a sintering temperature of 1480 ℃ and a vacuum degree of 1.0×10⁻⁶. 1 Pa, sintering time of 30 min, to obtain coated alloy part I.
[0056] (4) Use a soft brush to brush off the floating powder on the surface of the coated alloy part I, then use anhydrous ethanol for ultrasonic cleaning for 15 min, and then dry it in a vacuum drying oven at 80 ℃ for 6 h.
[0057] (5) Weigh each powder according to the mass percentage, which is 40% Si, 5% Mo, 20% MoSi2 and 35% ZrO2. The purity of each powder is higher than 99.5% and the particle size is less than 10 μm. The powder is ball-milled in an agate ball mill jar at 350 r / min for 8 hours to obtain mixed powder II. Then, mix mixed powder II with silica sol with a modulus of 3.5 at a mass ratio of 95:5 to obtain oxide ceramic-silicified material slurry. (6) The oxide ceramic-silicide slurry was brushed onto the surface of the pretreated silicide coating sample. The thickness of the second coating was 150 μm. After drying at 80 ℃ for 5 h, the sample was placed in a vacuum high-temperature sintering furnace at a sintering temperature of 1650 ℃ and a vacuum degree of 1.0 × 10⁻⁶. 1 Pa, sintering time of 30 min, that is, a ZrO2 ceramic-silicide composite coating is obtained on the surface of molybdenum alloy.
[0058] Comparative Example 1 The difference between this comparative example and Example 1 is that a silicide coating was prepared on the surface of Nb521 niobium alloy using only a single melting process. The specific preparation steps and slurry composition are shown in (1)-(3) of Example 1. The coating structure in Comparative Example 1 is a two-layer structure, consisting of a thicker (Nb,Ti,Cr,Zr,Mo)Si2 outer layer and a thinner Nb5Si3 inner layer, from the outside to the inside.
[0059] Comparative Example 2 The difference between this comparative example and Example 1 is that the oxide ceramic-silicide slurry was directly coated onto the alloy surface, dried, and then vacuum sintered at 1600 ℃ for 30 min to prepare the oxide ceramic-silicide coating. The specific preparation steps and slurry composition are shown in (1), (5)-(6) of Example 1. The coating structure in Comparative Example 2 is a three-layer structure, consisting of a loose and porous Al2O3-MoSi2-Mo5Si3 outer layer, a dense NbSi2 intermediate layer, and an Nb5Si3 inner layer, from the outside to the inside.
[0060] Comparative Example 3 The difference between this comparative example and Example 1 is that the oxide ceramic (Al2O3) phase in the coating is removed, that is, Al2O3 is removed from the oxide ceramic-silicified material slurry in step (5), and the powder ratio of the slurry is 60% Si, 15% Mo and 25% MoSi2. The coating structure in Comparative Example 3 is a three-layer structure, from the outside to the inside, namely the outer layer of MoSi2-Mo5Si3, the middle layer of (Nb,Ti,Cr,Zr,Mo)Si2 and the inner layer of Nb5Si3.
[0061] The high-temperature oxidation resistance of the coating samples prepared in Examples 1-3 and Comparative Examples 1-3 was tested. The oxidation resistance test was conducted using a self-made ultra-high temperature oxidation testing platform. The sample size was 60 mm × 4 mm × 2 mm. The coating sample was clamped onto the two electrodes of the testing instrument, and a low voltage and high current were applied to the electrodes for heating. A Raytek infrared thermometer was connected. The temperature was controlled by adjusting the current and voltage. The sample was raised to the test temperature in an atmospheric environment and held at that temperature for a period of time. After this period, the current and voltage were turned off, and the sample was removed after the temperature dropped to room temperature to evaluate the high-temperature oxidation resistance of the coating. The coating lifetime was defined as the time during which the surface oxide film remained dense and intact, without significant peeling, and effectively protected the substrate from oxidation. The results are shown in Table 1.
[0062] Table 1. High-Temperature Antioxidant Performance Test Data
[0063] As can be seen from Table 1, the composite coating prepared in the embodiments of the present invention exhibits excellent oxidation resistance in a static atmospheric environment at 1800℃. Comparative Examples 1 and 2 used a single-melting process, and the resulting composite coatings oxidized severely and could not be used at 1800℃. Comparative Example 3 omitted alumina compared to Example 1, i.e., it did not use oxide ceramic powder, and similarly could not be used at 1800℃.
[0064] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A composite anti-oxidation coating of oxide ceramic-silicide on the surface of a refractory alloy, characterized in that, The antioxidant coating consists of an oxide ceramic-silicide outer layer, an MSi2 type silicide intermediate layer, and an M5Si3 type silicide inner layer; M in the silicides of the intermediate and inner layers is a solid solution of Mo, Ti, Cr, Zr and the base metal element; In the oxide ceramic-silicide outer layer, the oxide ceramic is Al2O3, ZrO2 or HfO2; the silicide is MoSi2.
2. The composite antioxidant coating as described in claim 1, characterized in that, The oxide ceramic-silicide outer layer has an oxide ceramic mass fraction of not less than 30%; and / or the refractory alloy is a niobium alloy, tantalum alloy, molybdenum alloy or a high-entropy alloy composed of multiple refractory metal elements.
3. The method for preparing the composite antioxidant coating as described in claim 1, characterized in that, Includes the following steps: (1) Mix Si, Cr, Ti, Mo and Zr elemental powders, ball mill them to obtain mixed powder I; then mix mixed powder I with a binder to obtain silicide coating slurry; (2) The silicide coating slurry is coated on the surface of the refractory alloy substrate, and after the first sintering, the coated alloy part I is obtained; (3) Si, Mo, MoSi2 and oxide ceramic powder are mixed and ball-milled to obtain mixed powder II. Mixed powder II is then mixed with a binder to obtain oxide ceramic-silicified material slurry. The oxide ceramic powder is Al2O3, ZrO2 or HfO2 oxide ceramic powder. (4) The oxide ceramic-silicified material slurry is coated on the coated alloy part I, and after a second sintering, the coated alloy part II is obtained. The surface coating of the refractory alloy part in the coated alloy part II is the refractory alloy surface anti-oxidation coating. In step (1), the mass percentage of elemental powders of Si, Cr, Ti, Mo, and Zr is 60-75% Si, 5-10% Cr, 5-10% Ti, 5-10% Mo, and 5-10% Zr. In step (3), the mass percentages of Si, Mo, MoSi2 and oxide ceramic powder are: 30-40% Si, 5-10% Mo, 10-20% MoSi2 and 30-40% oxide ceramic powder.
4. The preparation method according to claim 3, characterized in that, The method further includes a refractory alloy substrate pretreatment step, wherein the pretreatment operation is as follows: the substrate surface is sandblasted with corundum sand, ultrasonically cleaned with ethanol after sandblasting, etched with a hydrofluoric acid-nitric acid mixed solution, and finally cleaned with deionized water and dried. Preferably, ultrasonic cleaning with anhydrous ethanol is performed for 10-20 minutes; Preferably, in the hydrofluoric acid-nitric acid mixed solution, the volume ratio of hydrofluoric acid to nitric acid is 1:2-4, and the etching time is 10-20s; Preferably, the drying operation is carried out at 80-100 ℃ for 4-6 h.
5. The preparation method according to claim 3, characterized in that, In step (1), the purity of Si, Cr, Ti, Mo, and Zr elemental powders is higher than 99.5% and the particle size is less than 10 μm; And / or, in step (1), the ball milling parameters are: ball milling at 300-350 r / min for 8-12 h; And / or, in step (1), the binder is a sodium carboxymethyl cellulose solution; the mass ratio of mixed powder I to binder is 90-95:5-10.
6. The preparation method according to claim 3, characterized in that, In step (2), the coating method includes brushing, dipping, or spraying; And / or, in step (2), the coating thickness is 100-300 μm; And / or, in step (2), after coating, dry at 80-100 °C for 6-12 h; And / or, in step (2), the first sintering temperature is 1450 ℃-1500 ℃, the sintering time is 30-45 min, and the vacuum degree is ≥1.0×10 -1 Pa.
7. The preparation method according to claim 3, characterized in that, The method also includes a post-treatment step for the coated alloy part I, specifically: brushing off the surface powder, ultrasonically cleaning with ethanol for 10-20 min, and drying at 80-100 ℃ for 4-6 h.
8. The preparation method according to claim 3, characterized in that, In step (3), the purity of Si, Mo, MoSi2 and oxide ceramic powders is higher than 99.5% and the particle size is less than 10 μm; And / or, in step (3), the ball milling parameters are: ball milling at 300-350 r / min for 8-12 h; And / or, in step (3), the binder is a silica sol with a modulus of 3.5, and the mass ratio of mixed powder II to binder is 85-95:5-15.
9. The preparation method according to claim 3, characterized in that, In step (4), the coating method includes brushing, dipping, or spraying; And / or, in step (4), the coating thickness is approximately 50-150 μm; And / or, in step (4), after coating, dry at 80-100 °C for 3-5 h; And / or, in step (4), the second sintering temperature is 1600 ℃-1700 ℃, the sintering time is 20-40 min, and the vacuum degree is ≥1.0×10 -1 Pa.
10. The application of the composite antioxidant coating as described in any one of claims 1-2 or the composite antioxidant coating prepared by the preparation method as described in any one of claims 3-9 in the preparation of refractory metal alloys.