Method for repairing micro-cracks on the tungsten surface of the first wall of the blanket of a nuclear fusion device

By using the controllable remelting technology of plasma arc under inert gas protection, the problems of high equipment cost, large size and secondary cracking of laser cladding method when repairing microcracks on the tungsten surface of the first wall of the blanket of nuclear fusion device have been solved, achieving in-situ repair effect with low cost and low environmental requirements.

CN123132875APending Publication Date: 2026-11-20SHENZHEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610962731.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-30
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing laser cladding methods for repairing microcracks on the tungsten surface of the first wall of the blanket of nuclear fusion devices involve high equipment investment, high operating costs, large equipment size, difficulty in achieving in-situ repair, and improper parameters can easily lead to defects such as deformation, cracks, and porosity, and cannot overcome the problem of secondary cracks.

Method used

The plasma arc is used to controllably remelt microcrack areas under inert gas protection. By controlling the moderate energy density and precise heat input of the plasma arc, and with the preset scanning path, the remelting, spreading and solidification of microcrack areas can be achieved. The powder-free remelting method avoids dust pollution and subsequent cleaning problems.

Benefits of technology

It effectively suppresses the generation of secondary cracks, realizes in-situ repair with low cost and low environmental requirements, and has a small equipment size, which can complete the repair of the first wall without disassembly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123132875A_ABST
    Figure CN123132875A_ABST
Patent Text Reader

Abstract

The application discloses a repairing method for micro-cracks on a tungsten surface of a first wall of a nuclear fusion device, and the method comprises the following steps: providing a first wall of a cladding, wherein the surface of the first wall of the cladding comprises a micro-crack area; pretreating the surface of the first wall of the cladding; placing the pretreated first wall of the cladding on a plasma cladding device; introducing ion gas and protective gas into the plasma cladding device, wherein the ion gas and the protective gas are independently selected from inert gases; generating a plasma arc on the plasma cladding device; controlling the plasma arc to scan the micro-crack area by using a preset scanning path; forming a molten pool to cover the micro-crack area; and causing the micro-crack area to be remelted, spread and solidified to complete the repairing. Thus, the repairing method can controllably remelt the micro-crack area by using the plasma arc under the protection of the inert gas, realizes crack closure and surface reconstruction, and effectively inhibits the generation of secondary cracks.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of material repair technology, and in particular relates to a method for repairing microcracks on the tungsten surface of the first wall of the blanket of a nuclear fusion device. Background Technology

[0002] In existing technologies, laser cladding is commonly used to repair microcracks on the tungsten surface of the first wall of a fusion reactor blanket. However, laser cladding requires a harsh working environment, resulting in high equipment investment and operating costs. Furthermore, the equipment is bulky, making in-situ repair of the first wall within the fusion reactor difficult. In addition, laser cladding parameters significantly affect the quality of the molten pool; improper parameter matching can directly disrupt the stability of the molten pool, interfere with the solidification process and gas expulsion, and cause defects such as deformation, cracks, and porosity. Most importantly, laser heating inherently possesses high heating and rapid cooling rates, and even with highly matched parameters, the problem of secondary cracking caused by these inherent characteristics cannot be overcome. Summary of the Invention

[0003] This application provides a method for repairing microcracks on the tungsten surface of the first wall of the blanket of a nuclear fusion device. This repair method can controllably remelt the microcracked area using a plasma arc under inert gas protection, thereby achieving crack closure and surface reconstruction and effectively suppressing the generation of secondary cracks. It adopts a powder-free remelting method, avoiding dust pollution and subsequent cleaning problems. Moreover, it has low requirements for the working environment, small equipment size, and can achieve in-situ repair without disassembly.

[0004] In a first aspect, this application provides a method for repairing microcracks on the tungsten surface of the first wall of the blanket of a nuclear fusion device, comprising the following steps: A first wall tungsten cladding is provided, the surface of which includes a microcrack region; The surface of the first tungsten cladding wall is pretreated, and the pretreated first tungsten cladding wall is placed on a plasma cladding equipment; Ionizing gas and protective gas are introduced into the plasma cladding equipment. The ionizing gas and the protective gas are each independently selected from inert gases. The plasma cladding equipment generates a plasma arc. The plasma arc is controlled to scan the microcrack area using a preset scanning path, forming a melt channel that covers the microcrack area. This causes the microcrack area to remelt, spread, and solidify, thus completing the repair.

[0005] This application provides a method for repairing microcracks on the surface of tungsten in the first wall of the blanket of a nuclear fusion device. The method involves providing a tungsten first wall blanket, the surface of which includes a microcrack region; pre-treating the surface of the tungsten first wall blanket; placing the pre-treated tungsten first wall blanket on a plasma cladding device; introducing an ionizing gas and a protective gas, each independently selected from inert gases, into the plasma cladding device to generate a plasma arc; controlling the plasma arc to scan the microcrack region using a preset scanning path, forming a melt channel covering the microcrack region, causing the microcrack region to remelt, spread, and solidify, thus completing the repair. Therefore, this repair method utilizes the moderate energy density and strong penetration of the plasma arc, combined with precise heat input control under inert gas protection and synergistic optimization of the preset scanning path, to induce local remelting, spreading, and solidification in the microcrack area. This ensures full fusion of the microcrack area while effectively suppressing the generation of secondary cracks. Furthermore, this repair method employs a powder-free remelting approach, avoiding the dust pollution and subsequent equipment cleaning difficulties that are easily introduced by conventional powder additive repair processes. In addition, compared to laser cladding equipment, this repair method has lower requirements for the working environment, uses smaller equipment, and can achieve in-situ repair without disassembling the first tungsten wall of the nuclear fusion device blanket. Attached Figure Description

[0006] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0007] Figure 1 A flowchart illustrating the steps of a method for repairing microcracks on the tungsten surface of the first wall of a nuclear fusion device blanket, provided in this application embodiment; Figure 2 Comparison of the morphology of the microcracked area on the tungsten surface of the first cladding wall before and after repair; Figure 3 The images show the XRD results of the tungsten surface of the first cladding wall before and after repair. Figure 4 Comparison of the width of the microcrack area on the tungsten surface of the first cladding wall before and after repair. Detailed Implementation

[0008] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0009] The flowchart shown in the attached diagram is for illustrative purposes only and does not necessarily include all content and operations / steps, nor does it necessarily have to be performed in the order described. For example, some operations / steps can be broken down, combined, or partially merged, so the actual execution order may change depending on the actual situation.

[0010] It should be understood that the terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to limit the scope of the application. As used in this specification and the appended claims, the singular forms “a,” “an,” and “the” are intended to include the plural forms unless the context clearly indicates otherwise.

[0011] It should also be understood that the term “and / or” as used in this application specification and the appended claims means any combination of one or more of the associated listed items and all possible combinations, and includes such combinations.

[0012] Laser cladding requires stringent environmental conditions, resulting in high equipment investment and operating costs. Furthermore, the large size of the equipment makes in-situ repair of the first wall within a fusion reactor difficult. In addition, improper matching of laser cladding parameters can directly disrupt the stability of the molten pool, interfering with the solidification process and gas expulsion, leading to defects such as deformation, cracks, and porosity. Most importantly, laser heating inherently possesses high heating and rapid cooling rates; even with highly matched parameters, it is still impossible to overcome the secondary cracking problems caused by the inherent characteristics of high-energy beams.

[0013] To address the aforementioned issues, this application provides a method for repairing microcracks on the surface of tungsten in the first wall of the blanket of a nuclear fusion device. This method utilizes the moderate energy density and strong penetration capability of a plasma arc, combined with precise heat input control under inert gas protection and synergistic optimization of a preset scanning path, to induce local remelting, spreading, and solidification in the microcrack area. This ensures sufficient fusion of the microcracks while effectively suppressing the generation of secondary cracks. Furthermore, this repair method employs a powder-free remelting approach, avoiding the dust pollution and subsequent equipment cleaning difficulties easily introduced by conventional powder additive repair processes. In addition, compared to laser cladding equipment, this repair method has lower requirements for the working environment, uses smaller equipment, and can achieve in-situ repair without disassembling the tungsten in the first wall of the nuclear fusion device blanket.

[0014] The following detailed description of some embodiments of this application is provided in conjunction with the accompanying drawings. Unless otherwise specified, the following embodiments and features can be combined with each other.

[0015] Please see Figure 1 , Figure 1 This is a flowchart illustrating the steps of a method for repairing microcracks on the tungsten surface of the first wall of a nuclear fusion device blanket, as provided in an embodiment of this application.

[0016] like Figure 1 As shown, the method for repairing microcracks on the tungsten surface of the first wall of the blanket of a nuclear fusion device includes steps S101 to S103.

[0017] Step S101: Provide a first tungsten cladding layer, the surface of which includes a microcrack region.

[0018] The first tungsten blanket refers to the plasma-facing structure in the blanket of a nuclear fusion device. It is made of tungsten and is used to withstand the plasma's thermal load and neutron irradiation.

[0019] In some embodiments, the width of the microcrack region is 1 μm to 5 μm, and the depth of the microcrack region is 10 μm to 50 μm.

[0020] Since conventional powder additive repair processes are prone to dust pollution and subsequent cleaning is difficult, this application adopts a powder-free remelting method for in-situ repair. By controlling the width of the microcrack region to be 0.10μm~10.00μm and the depth of the microcrack region to be 5μm~100μm, the plasma arc can achieve complete remelting and surface reconstruction of the microcrack region. If the width or depth of the microcrack region is too large, it is difficult to achieve complete remelting and surface reconstruction of the microcrack region by powder-free remelting alone. If the width or depth of the microcrack region is too small, the positioning accuracy requirement is high, the repair operation is difficult and the economy is poor. For example, the width of the microcrack region can be 0.10 μm, 1.15 μm, 2.15 μm, 2.31 μm, 2.55 μm, 3.00 μm, 4.50 μm, 4.85 μm, 5.55 μm, 7.60 μm, 9.50 μm, 10.00 μm, etc.; the depth of the microcrack region can be 5 μm, 8 μm, 10 μm, 15 μm, 20 μm, 30 μm, 50 μm, 60 μm, 80 μm, 100 μm, etc. Preferably, based on the influence of the size of the microcrack region on the remelting effect, the width of the crack region is 1 μm to 5 μm, and the depth of the microcrack region is 10 μm to 50 μm.

[0021] Step S102: Pre-treat the surface of the first tungsten cladding wall and place the pre-treated first tungsten cladding wall on a plasma cladding equipment.

[0022] The surface of the first tungsten cladding wall is pretreated to remove the surface oxide layer, oil, and attached impurities.

[0023] In some embodiments, pretreatment of the surface of the cladding first wall tungsten includes: polishing the surface of the cladding first wall tungsten and cleaning the polished surface.

[0024] For example, the surface of the first tungsten cladding layer is sanded with sandpaper until it is smooth, and then the sanded surface is cleaned with an ultrasonic cleaner.

[0025] Step S103: Introduce ion gas and protective gas into the plasma cladding equipment. The ion gas and protective gas are each independently selected from inert gases. This causes the plasma cladding equipment to generate a plasma arc. The plasma arc is controlled to scan the microcrack area using a preset scanning path, forming a melt channel that covers the microcrack area. This causes the microcrack area to remelt, spread, and solidify, thus completing the repair.

[0026] It should be noted that the ionized gas forms a plasma arc after ionization, which serves as the heat source for remelting and repair; the protective gas is distributed around the plasma arc and the melting channel, forming an inert atmosphere barrier to isolate the air and prevent tungsten from oxidizing.

[0027] In some embodiments, the inert gas includes one or more of argon, helium, neon, krypton, and xenon.

[0028] Argon is chemically stable and inexpensive, with a low ionization potential, making it easy to initiate and maintain a stable plasma arc. Helium has a higher ionization potential and thermal conductivity, allowing for higher plasma arc temperatures and energy densities. Neon has a moderate ionization potential and a high arc column temperature, while its small molecular radius provides good physical cleaning properties, and its price falls between argon and helium. Krypton and xenon have high atomic weights and gas densities, forming a thick protective gas shield with excellent resistance to airflow disturbances, good arc initiation characteristics, and are easy to ignite the plasma arc. Preferably, considering cost and plasma arc stability, both the ionizing gas and the protective gas are selected from argon.

[0029] In some embodiments, the ionizing gas flow rate (PFR) is 3.0 L / min to 3.5 L / min, and the protective gas flow rate (SFR) is 8.0 L / min to 10.0 L / min.

[0030] Controlling the ion gas flow rate to 3.0 L / min to 3.5 L / min is beneficial for ionization to form a plasma arc and maintain stable combustion of the plasma arc. If the ion gas flow rate is too low, it can easily lead to plasma arc divergence and fluctuations in the heat input of the molten pool. If the ion gas flow rate is too high, the arc column will be over-compressed, resulting in excessively high energy density. For example, the ion gas flow rate can be 3.0 L / min, 3.1 L / min, 3.2 L / min, 3.3 L / min, 3.4 L / min, 3.5 L / min, etc.

[0031] By controlling the protective gas flow rate to 8.0 L / min to 10.0 L / min, an inert atmosphere barrier can be formed in the melt channel to isolate air, prevent tungsten oxidation, and continuously protect the repair zone during the solidification stage. If the protective gas flow rate is too low, the protection will be insufficient and oxide inclusions will easily occur. If the protective gas flow rate is too high, the airflow will disturb the melt pool, leading to poor forming. For example, the protective gas flow rate can be 8.0 L / min, 8.2 L / min, 8.5 L / min, 8.8 L / min, 9.0 L / min, 9.5 L / min, 9.8 L / min, 10.0 L / min, etc.

[0032] In some embodiments, the process parameters for generating a plasma arc in the plasma cladding equipment are as follows: arc initiation current (ASC) of 40A~50A, rise time (RT) of 0.5s~1.0s, pre-gas time (PreT) of 0.3s~0.5s, plasma arc current (WC) of 120A~125A, plasma arc voltage (AV) of 30V~35V, arc termination current (CAC) of 20A~25A, and post-gas time (PostT) of 2.0s~3.0s.

[0033] It should be noted that the above process parameters are preferred parameters. These parameters work synergistically to control the stability and energy density of the plasma arc, causing local remelting, propagation, and solidification in the microcrack region, thereby achieving crack closure and surface reconstruction. Specifically, the arc initiation stage ensures smooth arc ignition through arc initiation current, rise time, and pre-gas time; the constant current stage maintains appropriate heat input by matching the arc current and arc voltage; and the arc termination stage reduces the current and extends gas protection by controlling the arc termination current and gas extension time to prevent crater cracking and oxidation.

[0034] In some embodiments, the energy density of the plasma arc is 450 J / mm². 2 ~500J / mm 2 The temperature of the plasma arc is 5000K~15000K.

[0035] It should be noted that during the repair process, the plasma arc is controlled to scan the microcrack area using a preset scanning path, forming multiple melt channels. Adjacent melt channels are spaced apart, and the channels do not form simultaneously but sequentially undergo remelting, spreading, and solidification. Due to significant temperature differences between the solidified melt channels, the melting pool, and the unheated area, temperature gradients are generated at adjacent melt channels and their overlaps. For tungsten, due to its high melting point, poor low-temperature plasticity, and sensitivity to thermal stress, excessive temperature gradients can lead to uneven shrinkage during solidification, causing tensile stress concentration at the channel boundaries and potentially inducing secondary cracks. Therefore, this embodiment controls the plasma arc energy density to 450 J / mm². 2 ~500J / mm 2 This method ensures sufficient remelting of the molten channel while limiting the liquid phase duration and heat-affected zone, reducing the temperature gradient between adjacent channels and at their overlap. This suppresses residual thermal stress during cooling and reduces secondary cracking. It avoids both insufficient energy leading to incomplete fusion, weak bonding, or residual cracks between channels, and excessive energy causing an overly wide molten pool, expanded heat-affected zone, and increased cooling shrinkage stress. For example, the energy density of the plasma arc can be 450 J / mm². 2 458J / mm 2 460J / mm 2 465J / mm 2 467J / mm 2 470J / mm 2 477J / mm 2 480J / mm 2 490J / mm 2 500J / mm 2 wait.

[0036] Furthermore, to achieve effective remelting of the microcracked areas on the tungsten surface, this embodiment controls the plasma arc temperature to 5000K~15000K. This temperature range is higher than the melting point of tungsten and provides moderate overheating, enabling localized remelting of the microcracked areas. Simultaneously, through coordinated energy density control, excessive expansion of the heat-affected zone is prevented. For example, the plasma arc temperature can be 5000K, 5500K, 6000K, 7000K, 8000K, 10000K, 11000K, 12000K, 14000K, 15000K, etc. Preferably, based on considerations of heat input stability, the plasma arc temperature is 6000K~12000K.

[0037] In some embodiments, the preset scanning path is a serpentine reciprocating scanning path.

[0038] Specifically, the plasma arc is controlled to scan along a first direction to form a first melt channel, then the scanning interval is offset along a second direction, and a third direction is scanned to form a second melt channel. This process is repeated until the entire microcrack region is covered, ensuring that the microcrack region is completely remelted. The first direction is the length extension direction of the first melt channel, the second direction is the direction perpendicular to the first direction, and the third direction is the direction opposite to the first direction.

[0039] For example, a computer system can control a plasma arc to scan the microcrack area using a serpentine reciprocating scanning path, forming a melt channel that covers the microcrack area, causing the microcrack area to remelt, spread, and solidify, thus completing the repair.

[0040] In some embodiments, the scanning speed (WS) of the plasma arc is 5.0 mm / s to 7.0 mm / s, and the scanning interval is 4 mm.

[0041] By controlling the scanning speed of the plasma arc to 5.0 mm / s to 7.0 mm / s, the contact time between the plasma arc and the microcrack region can be ensured to be appropriate, guaranteeing sufficient heat input to the molten pool for complete remelting. If the scanning speed is too low, severe heat accumulation will occur, easily inducing deformation and secondary cracks; if the scanning speed is too high, the energy density of the plasma arc will be insufficient, easily leading to incomplete fusion or crystallization cracks. Simultaneously, setting the scanning interval to 4 mm is an optimized choice based on the coordinated matching of the plasma arc energy density and scanning speed. This ensures effective overlap fusion between adjacent molten channels while minimizing repeated heating of the overlap area, thereby reducing the temperature gradient and the risk of thermal stress concentration. For example, the scanning speed can be 5.0 mm / s, 5.2 mm / s, 5.5 mm / s, 6.0 mm / s, 6.5 mm / s, 6.8 mm / s, 7.0 mm / s, etc.

[0042] In some embodiments, solidification is achieved through natural cooling.

[0043] It should be noted that after remelting, the repaired area remains at a high temperature, and its solidification process directly affects the formation of residual stress and secondary cracks. Therefore, in this embodiment, the repaired area is allowed to cool naturally to room temperature while maintaining a constant protective gas atmosphere, avoiding direct liquid cooling or forced rapid cooling methods. This reduces the temperature gradient and residual thermal stress in the microcrack area, thereby reducing the generation of secondary cracks.

[0044] To enable those skilled in the art to clearly understand the above-described implementation details and operations of the present invention, and to demonstrate the significant improvement in the performance of the method for repairing microcracks on the tungsten surface of the first wall of the blanket of a nuclear fusion device, the following specific embodiment is used to illustrate the above technical solution.

[0045] Example 1 Please see Figure 1 The method for repairing microcracks on the tungsten surface of the first wall of the blanket of a nuclear fusion device, as described in this embodiment, includes the following steps: Step S101: Provide a first tungsten cladding layer, the surface of which includes a microcrack region with a width of 2.15 μm and a depth of 30 μm. Step S102: Use sandpaper to polish the surface of the first tungsten cladding layer until the surface is smooth, and then use an ultrasonic cleaner to clean the polished surface. Step S103: Introduce ionizing gas and protective gas, both selected from argon, into the plasma cladding equipment to generate a plasma arc. The process parameters for generating the plasma arc are as follows: ASC 40A, RT 0.5s, PreT 0.3s, WC 125A, AV 30V, CAC 20A, PostT 2.0s, PFR 3.5L / min, SFR 8L / min, WS 5mm / s, scanning interval 4mm, and plasma arc energy density 477J / mm². 2 The temperature of the plasma arc is 6000K. The plasma arc is controlled to scan the microcrack area in a serpentine reciprocating scanning path, forming a melt channel that covers the microcrack area, causing the microcrack area to remelt, spread and solidify, thus completing the repair.

[0046] The test results before and after the repair in Example 1 are as follows: Figure 2 The images show a comparison of the morphology of the microcracked area on the tungsten surface of the first cladding wall before and after repair. Figure 2 Image a shows the morphology of the microcracked area before repair. Figure 2 b is a topographic image of the cracked area after repair in Example 1. Figure 2 It can be seen that before repair, there were obvious network cracks in the microcrack area, with wide crack openings and interconnected cracks. After repair by Example 1, the number and width of microcracks were significantly reduced, and the repaired area showed a molten filling state, indicating that Example 1 can effectively repair the microcrack damage on the tungsten surface of the first wall.

[0047] Figure 3 These are XRD results of the tungsten surface of the first cladding wall before and after repair. Figure 3 As can be seen, the main diffraction peaks before (marked Before remelting) and after (marked After remelting) correspond to the W standard card (W PDF#04-001-2998), indicating that the main phase on the tungsten surface of the first wall of the cladding is still metallic tungsten, and no obvious new phase was introduced after remelting.

[0048] Figure 4This image shows a comparison of the width of the microcracked area on the tungsten surface of the first cladding wall before and after repair. Figure 4 As can be seen, the peak value of the crack width distribution before repair (marked Before repair in the figure) is mainly located around 2.15 μm, while the peak value of the crack width distribution after repair (marked After repair in the figure) moves to around 1.13 μm. This indicates that after the repair treatment in Example 1, the crack width shifts to a smaller size range as a whole, and the degree of crack opening is significantly reduced.

[0049] In summary, the repair method for microcracks on the tungsten surface of the first wall of the fusion device blanket proposed in this application utilizes the moderate energy density and strong penetration capability of the plasma arc, combined with precise heat input control under inert gas protection and synergistic optimization of the preset scanning path, to cause local remelting, spreading, and solidification in the microcrack area. This ensures sufficient fusion of the microcrack area while effectively suppressing the generation of secondary cracks. Furthermore, this repair method employs a powder-free remelting approach, avoiding the dust pollution and subsequent equipment cleaning difficulties easily introduced by conventional powder additive repair processes. In addition, compared with laser cladding equipment, this repair method has lower requirements for the working environment, uses smaller equipment, and can achieve in-situ repair without disassembling the tungsten of the first wall of the fusion device blanket.

[0050] The above description is merely a specific embodiment of this application, but the scope of protection of this application is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in this application, and these modifications or substitutions should all be covered within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.

Claims

1. A method for repairing microcracks on the tungsten surface of the first wall of the blanket of a nuclear fusion device, characterized in that, Includes the following steps: A first wall tungsten cladding is provided, the surface of which includes a microcrack region; The surface of the first tungsten cladding wall is pretreated, and the pretreated first tungsten cladding wall is placed on a plasma cladding equipment; Ionizing gas and protective gas are introduced into the plasma cladding equipment. The ionizing gas and the protective gas are each independently selected from inert gases. The plasma cladding equipment generates a plasma arc. The plasma arc is controlled to scan the microcrack area using a preset scanning path, forming a melt channel that covers the microcrack area. This causes the microcrack area to remelt, spread, and solidify, thus completing the repair.

2. The repair method according to claim 1, characterized in that, The width of the microcrack region is 0.10μm to 10.00μm, and the depth of the microcrack region is 5μm to 100μm.

3. The repair method according to claim 1, characterized in that, The process parameters for generating a plasma arc in the plasma cladding equipment are as follows: arc initiation current is 40A~50A, slow rise time is 0.5s~1.0s, pre-gas time is 0.3s~0.5s, plasma arc current is 120A~125A, plasma arc voltage is 30V~35V, arc termination current is 20A~25A, and gas extension time is 2.0s~3.0s.

4. The repair method according to claim 1, characterized in that, The energy density of the plasma arc is 450 J / mm². 2 ~500J / mm 2 The temperature of the plasma arc is 5000K~15000K.

5. The repair method according to claim 1, characterized in that, The inert gas includes one or more of argon, helium, neon, krypton, and xenon.

6. The repair method according to claim 1, characterized in that, The ion gas flow rate is 3.0 L / min to 3.5 L / min, and the protective gas flow rate is 8.0 L / min to 10.0 L / min.

7. The repair method according to claim 1, characterized in that, The preset scanning path is a serpentine reciprocating scanning path.

8. The repair method according to claim 1, characterized in that, The scanning speed of the plasma arc is 5.0 mm / s to 7.0 mm / s, and the scanning interval is 4 mm.

9. The repair method according to claim 1, characterized in that, The solidification method is natural cooling.

10. The repair method according to claim 1, characterized in that, The pretreatment of the surface of the first wall tungsten cladding includes: The surface of the first wall tungsten of the cladding is polished and then cleaned.