Method for manufacturing tantalum capacitor anode and tantalum capacitor anode

By constructing a three-dimensional micropillar array on the surface of tantalum foil and generating nanoscale channels, the problem of insufficient effective specific surface area of ​​tantalum capacitor anodes in existing technologies is solved, thereby improving electrical performance and high-frequency stability.

CN123132876APending Publication Date: 2026-11-20HUNAN XINXIN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611630928.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing tantalum capacitor anode manufacturing technology makes it difficult to construct a three-dimensional ordered structure and finely control multi-scale channels, resulting in insufficient effective specific surface area and affecting electrical performance.

Method used

A three-dimensional micropillar array was constructed on the surface of tantalum foil using laser-directed energy deposition technology, and nanoscale channels were generated on the micropillars by electrochemical etching. A hierarchical channel structure was formed by combining high-energy pulse nucleation steps.

Benefits of technology

It significantly increases the effective specific surface area of ​​the tantalum capacitor anode, reduces the diffusion resistance of ions, improves the capacitance retention rate of the capacitor under high-frequency environment, and avoids grain growth and particle agglomeration caused by traditional high-temperature sintering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123132876A_ABST
    Figure CN123132876A_ABST
Patent Text Reader

Abstract

The application discloses a tantalum capacitor anode manufacturing method and a tantalum capacitor anode. The method comprises the following steps: cleaning a tantalum foil, and forming a micron-level pit array on the surface of the tantalum foil through dot matrix laser scanning; adopting a laser directional energy deposition process to construct a three-dimensional micro column array on the surface of the tantalum foil by taking the micron-level pit as an initial deposition position; and placing the tantalum foil with the three-dimensional micro column array in an organic electrolyte, and forming a hierarchical pore structure with different pore diameters on the three-dimensional micro column through step-by-step electrochemical etching. The three-dimensional micro column array construction is combined with hierarchical pore regulation, the available surface area of the anode is increased, and a method for preparing a tantalum capacitor anode with a large specific surface area is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrolytic capacitor technology, and in particular to a method for manufacturing a tantalum capacitor anode and the tantalum capacitor anode itself. Background Technology

[0002] Tantalum capacitors are widely used in aerospace, communication equipment, and electronic circuits due to their advantages such as small size, stable capacitance, and high reliability. As the core component of tantalum capacitors, the microstructure, effective specific surface area, and surface dielectric layer quality of the tantalum anode directly affect the capacitor's electrical performance. Currently, tantalum anodes are mainly manufactured using powder sintering technology. High-temperature sintering binds tantalum powder particles together to form a porous anode with a specific pore structure. While this technology is relatively mature, during high-temperature sintering, tantalum powder particles are prone to grain growth and agglomeration, leading to some pores shrinking or closing, reducing the effective specific surface area. Furthermore, the pore structure formed by powder sintering has a certain degree of randomness, making it difficult to precisely control the size, distribution, and connectivity of the pores, thus limiting further optimization of the tantalum anode structure.

[0003] In recent years, rapid heating technologies such as flash Joule heating (FJH) have been applied to the sintering and forming of metal powders. These technologies achieve rapid particle bonding through high energy input over short periods, which to some extent helps reduce grain growth and agglomeration caused by prolonged high-temperature processing. However, these technologies primarily focus on the rapid sintering of powder particles, and their ability to actively control the overall geometry and internal pore morphology of the anode remains limited. They struggle to simultaneously achieve the construction of a three-dimensional ordered framework and the precise control of multi-scale channels. Furthermore, while existing electrochemical etching technologies can alter the surface morphology of materials by adjusting electrolyte composition and electrochemical parameters, balancing channel formation, size control, and framework integrity in complex three-dimensional structures remains a technical challenge that needs to be addressed.

[0004] Therefore, it is necessary to develop a method for preparing tantalum capacitor anodes that combines the construction of three-dimensional ordered structures with hierarchical pore size control, so as to increase the effective specific surface area of ​​the anode and achieve the controllable construction of the pore structure, thus providing a new technical approach to improve the electrical performance of tantalum capacitors. Summary of the Invention

[0005] The main objective of this invention is to provide a method for manufacturing a tantalum capacitor anode and a tantalum capacitor anode, thereby solving the technical problems described in the background section.

[0006] In a first aspect, the present invention provides a method for manufacturing a tantalum capacitor anode, the method comprising the following steps: A tantalum foil of a preset thickness is first cleaned, and then the surface of the tantalum foil is scanned by a dot matrix laser to form a micron-level pit array of a preset size. The tantalum foil is subjected to laser-directed energy deposition to form three-dimensional micropillars on each micron-sized pit; The tantalum foil with the three-dimensional micropillars formed thereon is immersed in an organic electrolyte. Using the tantalum foil as the working electrode, a voltage is applied to perform electrochemical etching, generating nanoscale channels on the micropillars to obtain the tantalum capacitor anode.

[0007] In one preferred embodiment, after the step of electrochemical etching using the tantalum foil as the working electrode and applying voltage to generate nanoscale channels on the three-dimensional micropillars, the method further includes: The tantalum foil electrode is subjected to a second cleaning process, and then the tantalum foil is placed in an anodic oxidation electrolyte and a voltage is applied to generate a dielectric layer on the surface of the tantalum foil.

[0008] In one preferred embodiment, the second cleaning process specifically includes: The electrochemically etched tantalum foil was immersed in deionized water for ultrasonic cleaning, and then dried using a nitrogen stream.

[0009] In one preferred embodiment, the step of performing laser-directed energy deposition on the tantalum foil to form three-dimensional micropillars on each micrometer-scale pit includes: The tantalum foil is placed into the working chamber, nitrogen is continuously introduced into the working chamber to maintain the oxygen content below the preset concentration, and then tantalum powder is continuously fed into the working chamber. A laser beam is applied to the micron-scale pit array using the first laser process parameters, and the tantalum powder is deeply fused with each of the micron-scale pits. The laser beam is applied to the micron-scale pit array using the second laser process parameters, guiding the tantalum powder to be stacked layer by layer in the vertical direction in each of the micron-scale pits to form a three-dimensional micropillar.

[0010] In one preferred embodiment, the step of applying a laser beam to the micron-scale pit array using second laser process parameters to guide the tantalum powder to be stacked layer by layer in each micron-scale pit to form a three-dimensional micropillar in a vertical direction includes: The laser beam is applied to the micron-sized pits in the micron-sized pit array using the second laser process parameters, and the tantalum foil is controlled to move synchronously downward in the vertical direction at a preset speed. When the tantalum powder is deposited layer by layer to a preset height starting from the micron-level pit to form a three-dimensional micropillar, the laser beam is turned off, and the tantalum foil is controlled to reset vertically upward and move horizontally to the next micron-level pit position. Repeat the above operation until all micron-level pits in the micron-level pit array have been processed.

[0011] In one preferred embodiment, the step of using the tantalum foil as a working electrode and applying voltage to perform electrochemical etching to generate nanoscale channels on the three-dimensional micropillars includes: Using the tantalum foil as the working electrode, electrochemical etching is performed by applying voltage with the first electrochemical process parameters to generate first channels with a diameter of 300-500 nm in the sidewalls and skeleton of each three-dimensional micropillar. Electrochemical etching is performed by applying voltage with the second electrochemical process parameters to form a second channel with a smaller diameter than the first channel on the inner wall of the first channel.

[0012] In one preferred embodiment, the diameter of the first channel is 300-500 nm, and the diameter of the second channel is 30-50 nm.

[0013] In one preferred embodiment, the step of performing a first cleaning process on the tantalum foil of a predetermined thickness includes: Tantalum foil of a predetermined thickness is placed in acetone and anhydrous ethanol for ultrasonic cleaning in sequence. Then immerse it in a 5% hydrofluoric acid solution for a preset time. Finally, the tantalum foil was cleaned with deionized water and dried with nitrogen gas.

[0014] In a second aspect, the present invention provides a tantalum capacitor anode, which is manufactured by the method described in any one of the first aspects.

[0015] The above-mentioned method for fabricating the tantalum capacitor anode involves constructing a three-dimensional micropillar array on the surface of a tantalum foil substrate using laser-directed energy deposition (LDED) technology. This expands the original planar structure into a three-dimensional structure, increasing the tantalum surface area available for forming the dielectric layer per unit projected area. Through electrochemical etching, nanoscale channels are constructed on the micropillars, greatly improving the effective specific surface area. The three-dimensional framework constructed in this invention has a defined geometric periodicity, and the ordered conductive and transport network significantly reduces the diffusion impedance of ions, thereby improving the capacitance retention rate of the capacitor under high-frequency operating conditions. Attached Figure Description

[0016] Figure 1 This is a schematic flowchart of a method for manufacturing a tantalum capacitor anode in one embodiment of the present invention; Figure 2 This is a schematic flowchart of a method for manufacturing a tantalum capacitor anode in one embodiment of the present invention; Figure 3 This is a schematic flowchart of a method for manufacturing a tantalum capacitor anode in one embodiment of the present invention; Figure 4 This is a schematic flowchart of a method for manufacturing a tantalum capacitor anode in one embodiment of the present invention; Figure 5 This is a schematic diagram of the structure of the tantalum capacitor anode in one embodiment of the present invention; Figure 6 This is a schematic flowchart illustrating a method for manufacturing the anode of a tantalum capacitor in one embodiment of the present invention. Detailed Implementation

[0017] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.

[0018] Firstly, referring to Figure 1-6 This invention provides a method for manufacturing a tantalum capacitor anode, characterized in that the method for manufacturing the tantalum capacitor anode includes: S110, a first cleaning process is performed on a tantalum foil of a preset thickness, and then a dot matrix laser scan is performed on the surface of the tantalum foil to form a micron-level pit array of a preset specification; In this step, a tantalum foil with a thickness of 1 mm is preferred as the substrate, and its purity should be no less than 99.95%.

[0019] In step S110, the step of performing a first cleaning treatment on the tantalum foil of a preset thickness specifically includes: Tantalum foil of a preset thickness is placed in acetone and anhydrous ethanol for ultrasonic cleaning in sequence. The cleaning time is preferably 15 minutes for each time to remove oil stains. The tantalum foil is then immersed in a 5% hydrofluoric acid solution for a preset time of 10 seconds to remove the oxide layer on the surface of the tantalum foil.

[0020] Finally, the tantalum foil was cleaned with deionized water and dried with nitrogen gas.

[0021] For example, the tantalum foil is washed three times with deionized water and then dried with high-purity nitrogen. Furthermore, the tantalum foil after the first cleaning process needs to be stored in a vacuum desiccator to prevent re-oxidation.

[0022] In step S110, the step of performing a dot matrix laser scan on the surface of the tantalum foil to form a micron-sized pit array of preset specifications involves laser scanning parameters including wavelength, laser power, pulse frequency, scanning rate, and scanning spacing. For example, a pulsed laser with a wavelength of 1064 nm is used to perform a dot matrix scan on the cleaned tantalum foil surface. The laser power is set to 40W, the pulse frequency to 20kHz, the scanning rate to 500mm / s, and the scanning spacing to 0.11mm. Finally, a micro-pit array with a depth of approximately 15μm, a diameter of approximately 100μm, and a dot matrix spacing of 10μm is formed on the tantalum foil surface, providing nucleation sites for subsequent additive growth. It should be noted that the laser scanning method used in this step is only illustrative and does not constitute a limitation on the pit forming process. In specific implementations, other physical or chemical processing methods can also be used to achieve a micron-sized pit array with the same effect.

[0023] S120, the tantalum foil is subjected to laser-directed energy deposition to form three-dimensional micropillars on each micron-level pit; Reference Figure 3 The S120 step specifically includes: S121, the tantalum foil is placed into the working chamber, nitrogen is continuously introduced into the working chamber to maintain the oxygen content below the preset concentration, and then tantalum powder is continuously fed into the working chamber. The nitrogen gas used is high-purity nitrogen gas, with a preset concentration of 100 ppm, and the powder feeding rate should be controlled at 5.0 g / min.

[0024] S122, the laser beam is applied to the micron-scale pit array using the first laser process parameters, and the tantalum powder is deeply fused with each of the micron-scale pits; The first laser process parameters include wavelength, peak power, pulse width, and frequency. For example, the wavelength is set to 1060nm, the peak power to 30W, the modulation pulse width to 10ms, and the frequency to 15Hz. In addition, the first laser process parameters also include static irradiation time, preferably 0.5 seconds. In this step, the initial tantalum powder and the tantalum foil (with its micron-scale pit array) are deeply fused through a high-energy pulse, forming a high-strength metallurgical bonding interface.

[0025] S123, the laser beam is applied to the micron-scale pit array using the second laser process parameters, guiding the tantalum powder to be stacked layer by layer in the vertical direction in each of the micron-scale pits to form a three-dimensional micropillar.

[0026] The second laser process parameters include wavelength, peak power, pulse width, and frequency. For example, the wavelength and frequency are the same as the first laser process parameters, but the laser power is adjusted to 15W and the pulse width is 4ms. Figure 5The tantalum powder is guided to stack layer by layer in the vertical direction in each of the micron-sized pits to form a three-dimensional micropillar; For step S123, refer to... Figure 6 It also includes: S1231, the laser beam is applied to the micron-sized pits to be processed in the micron-sized pit array using the second laser process parameters, and the tantalum foil is controlled to move synchronously downward in the vertical direction at a preset speed; S1232, after the tantalum powder in the micron-level pit stacks to a preset height to form a three-dimensional micro-pillar, the laser beam is turned off, the tantalum foil is controlled to reset vertically upwards and move horizontally to the position of the next micron-level pit to be processed; S1233, repeat the above operation until all micron-level pits have been processed.

[0027] The preset speed is preferably 0.05 mm / s. When the laser beam is working, the synchronous control console moves downward in the vertical direction at the preset speed to compensate for the focal plane shift caused by the elongation of the column. Continuous local molten pool cooling and solidification are used to guide the tantalum powder to be stacked layer by layer in the vertical direction. Then the above two steps are repeated to finally obtain an ordered three-dimensional micro-pillar array with a height of 100 μm and a diameter of 100 μm.

[0028] S130, the tantalum foil with the three-dimensional micropillars formed thereon is immersed in an organic electrolyte, and the tantalum foil is used as the working electrode to perform electrochemical etching by applying voltage to generate nanoscale channels on the micropillars, thereby obtaining the tantalum capacitor anode.

[0029] The organic electrolyte needs to be prepared in advance. The organic electrolyte uses ethanol as the main solvent, and then 1 wt% HF and 1 M H2SO4 are added to it to construct a fluorine-containing organic electrolyte system. Then, a standard three-electrode electrochemical experimental system is built.

[0030] Reference Figure 4 Step S130, using the tantalum foil as the working electrode, applies voltage to perform electrochemical etching to generate nanoscale channels on the micropillars, specifically includes: S131, using the tantalum foil as the working electrode, an electrochemical etching is performed by applying voltage with the first electrochemical process parameters to generate first channels in the sidewalls and skeleton of each three-dimensional micropillar; Specifically, the laser-printed sample can be used as the working electrode, a platinum sheet or high-purity graphite as the counter electrode (CE), and a saturated calomel electrode or Ag / AgCl electrode as the reference electrode (RE). The first electrochemical process parameters include voltage, duration, frequency, and duty cycle. In this step, the etching reaction preferentially occurs at the active defect sites induced by the laser and grows vertically inward along the electric field line direction, forming a through-hole main channel with a diameter of about 300-500 nm on the sidewall of the micropillar and inside the framework. Through preliminary pore enlargement, a low-resistance channel is provided for the deep penetration of the electrolyte, and the secondary framework of the electrode is constructed. For example, the diameter of the first channel is 300-500 nm.

[0031] S132, apply voltage with the second electrochemical process parameters to perform electrochemical etching, and form a second channel with a smaller diameter than the first channel on the inner wall of the first channel.

[0032] For example, the diameter of the second channel is 30-50 nm.

[0033] The second electrochemical process parameters include voltage, duration, frequency, and duty cycle, and the voltage in the second chemical process parameters is lower than the voltage in the first chemical process parameters. In this step, by reducing the voltage, under the synergistic effect of the electric field and fluoride ions, extremely high-density secondary nanopore cores are induced in situ on the inner wall of the already formed first channel. These nanopores grow finely in the radial and longitudinal directions to form second-order micropores with a diameter between 30-50 nm. This fractal pore structure significantly improves the specific surface area of ​​the tantalum capacitor anode.

[0034] For example, the first electrochemical process parameters include a pulse peak voltage of 10 V, a pulse frequency of 50 Hz, a duty cycle of 50%, and an etching time of 20 min; the second electrochemical process parameters include a pulse peak voltage of 3 V, a pulse frequency of 20 Hz, a duty cycle of 20%, and an etching time of 5 min.

[0035] In one embodiment, reference Figure 2 After the step of using the tantalum foil as the working electrode and applying voltage to perform electrochemical etching to generate nanoscale channels on the three-dimensional micropillars, the method further includes: S140, the tantalum foil is subjected to a second cleaning process, and then the tantalum foil is placed in an anodic oxidation electrolyte and a voltage is applied to generate a dielectric layer on the surface of the tantalum foil.

[0036] The step of performing the second cleaning process on the tantalum foil includes: The electrochemically etched tantalum foil was immersed in deionized water for ultrasonic cleaning, and then dried using a nitrogen stream.

[0037] Specifically, the tantalum foil is removed from the electrolyte and quickly immersed in a large amount of deionized water to terminate the corrosion reaction of fluoride ions, followed by multiple ultrasonic cleanings to thoroughly remove residual chemical components deep within the micropores. The cleaned sample is then slowly dried using a high-purity nitrogen stream. This second cleaning process ensures that the physical morphology of the hierarchical porous structure does not undergo secondary deformation due to residual droplets, laying a pure interfacial foundation for the subsequent anodizing process.

[0038] The anodic oxidation electrolyte was a 0.1 wt% aqueous solution of phosphoric acid (H3PO4), the voltage was set to 80 V, the oxidation time was 10 min, and the counter electrode was a platinum sheet electrode. Finally, a uniform tantalum pentoxide (Ta2O5) dielectric layer was grown in situ on the tantalum foil surface.

[0039] In addition, the tantalum capacitor anode after film formation requires a systematic structural and performance evaluation: First, the microstructure of the electrodes was observed at different magnifications using field emission scanning electron microscopy (SEM) to verify whether the laser-printed three-dimensional micron column array remained intact and whether a hierarchical porous system was successfully constructed on the surface; at the same time, the continuity and coating quality of the Ta2O5 dielectric layer in the depths of complex channels were observed.

[0040] Then, to verify the feasibility and superiority of the strategy, the specific capacitance of the tantalum foil was tested in 1 M H2SO4 solution using a digital bridge, with a platinum sheet electrode as the counter electrode.

[0041] In addition, the specific capacitance of the control group electrodes was also tested: the original tantalum foil without any treatment, the tantalum capacitor with only a three-dimensional ordered micropillar array constructed, and the tantalum capacitor with only electrochemical etching.

[0042] This invention utilizes LDED technology to construct a micrometer-scale ordered array in physical space, extending the electrode geometry from a two-dimensional plane to a three-dimensional columnar framework, thus increasing the loading of active material from a macroscopic perspective. Through a stepped etching strategy of high-voltage pore expansion and low-voltage capacitance enhancement, a hierarchical porous system consisting of 100-nanometer (300-500 nm) through-channels and nanometer-scale (30-50 nm) secondary micropores is constructed on the sidewalls and interior of the micropillars. By constructing hierarchical channels of different scales on the surface of the three-dimensional micropillars, the usable surface area of ​​the anode is increased, providing a structural basis for improving the specific capacitance of the tantalum capacitor anode.

[0043] Furthermore, unlike the random and disordered pores formed by traditional processes, the three-dimensional framework constructed in this invention possesses a defined geometric periodicity. Its large-diameter through-channels effectively reduce the wetting resistance of the electrolyte and shorten the migration path of ions deep within the micropores. This ordered conductive and transport network significantly reduces the diffusion impedance of ions, improving the capacitance retention of the capacitor under high-frequency operating conditions.

[0044] During fabrication, the high-energy pulse nucleation process creates a deep metallurgical bond between the three-dimensional micropillars and the tantalum foil substrate, fundamentally eliminating the risk of active layer peeling common in traditional coating processes and significantly reducing contact resistance and equivalent series resistance. Due to the highly ordered structure and uniform pore size distribution, the Ta2O5 dielectric layer generated during subsequent anodizing has uniform thickness and good density, significantly suppressing leakage current and improving breakdown voltage.

[0045] This invention employs laser-based instantaneous additive manufacturing to replace traditional high-temperature vacuum sintering, which takes several hours. Laser processing features highly concentrated energy density and a minimal heat-affected zone, shortening the production cycle while avoiding grain coarsening or softening of the substrate foil caused by prolonged heat accumulation. This effectively maintains the mechanical flexibility and structural integrity of the electrode substrate. In a second aspect, the present invention provides a tantalum capacitor anode, which is manufactured by the method described in any one of the first aspects, comprising a tantalum foil substrate and a three-dimensional micropillar array formed on the surface of the tantalum foil substrate, wherein the micropillars in the three-dimensional micropillar array are connected to the tantalum foil substrate, and the micropillars have a hierarchical channel structure, wherein the hierarchical channel structure includes a first channel and a second channel formed on the inner wall of the first channel, wherein the pore diameter of the second channel is smaller than the pore diameter of the first channel, and the effects thereof are as described in any one of the first aspects, and will not be repeated here.

[0046] It should be understood that although the steps in the flowcharts of the embodiments described above are shown sequentially according to the arrows, these steps are not necessarily executed in the order indicated by the arrows. Unless explicitly stated herein, there is no strict order restriction on the execution of these steps, and they can be executed in other orders. Moreover, at least some steps in the flowcharts of the embodiments described above may include multiple steps or multiple stages. These steps or stages are not necessarily completed at the same time, but can be executed at different times. The execution order of these steps or stages is not necessarily sequential, but can be performed alternately or in turn with other steps or at least some of the steps or stages of other steps.

[0047] It should be noted that, in this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or system that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or system. Unless otherwise specified, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or system that includes that element.

[0048] The sequence numbers of the above embodiments of the present invention are for descriptive purposes only and do not represent the superiority or inferiority of the embodiments.

[0049] The above are merely preferred embodiments of the present invention and do not limit the scope of the patent. Any equivalent structural or procedural transformations made based on the description and drawings of the present invention, or direct or indirect applications in other related technical fields, are similarly included within the scope of patent protection of the present invention.

Claims

1. A method for manufacturing the anode of a tantalum capacitor, characterized in that, The method for manufacturing the anode of the tantalum capacitor includes: A tantalum foil of a preset thickness is first cleaned, and then the surface of the tantalum foil is scanned by a dot matrix laser to form a micron-level pit array of a preset size. The tantalum foil is subjected to laser-directed energy deposition to form three-dimensional micropillars on each micron-sized pit; The tantalum foil with the three-dimensional micropillars formed thereon is immersed in an organic electrolyte. Using the tantalum foil as the working electrode, a voltage is applied to perform electrochemical etching, generating nanoscale channels on the three-dimensional micropillars to obtain the tantalum capacitor anode.

2. The method for manufacturing the anode of a tantalum capacitor as described in claim 1, characterized in that, After the step of using the tantalum foil as the working electrode and applying voltage to perform electrochemical etching to generate nanoscale channels on the three-dimensional micropillars, the method further includes: The tantalum foil is subjected to a second cleaning process, and then the tantalum foil is placed in an anodic oxidation electrolyte and a voltage is applied to generate a dielectric layer on the surface of the tantalum foil.

3. The method for manufacturing the anode of a tantalum capacitor as described in claim 1, characterized in that, The step of performing laser-directed energy deposition on the tantalum foil to form three-dimensional micropillars on each micrometer-level pit includes: The tantalum foil is placed into the working chamber, nitrogen is continuously introduced into the working chamber to maintain the oxygen content below the preset concentration, and then tantalum powder is continuously fed into the working chamber. A laser beam is applied to the micron-scale pit array using the first laser process parameters, and the tantalum powder is deeply fused with each of the micron-scale pits. The laser beam is applied to the micron-scale pit array using the second laser process parameters, guiding the tantalum powder to be stacked layer by layer in the vertical direction in each of the micron-scale pits to form a three-dimensional micropillar.

4. The method for manufacturing the anode of a tantalum capacitor as described in claim 3, characterized in that, The step of applying a laser beam to the micron-scale pit array using the second laser process parameters, and guiding the tantalum powder to be stacked layer by layer in each of the micron-scale pits to form a three-dimensional micropillar along the vertical direction, includes: The laser beam is applied to the micron-sized pits in the micron-sized pit array using the second laser process parameters, and the tantalum foil is controlled to move synchronously downward in the vertical direction at a preset speed. When the tantalum powder is deposited layer by layer to a preset height starting from the micron-level pit to form a three-dimensional micropillar, the laser beam is turned off, and the tantalum foil is controlled to reset vertically upward and move horizontally to the next micron-level pit position. Repeat the above operation until all micron-level pits in the micron-level pit array have been processed.

5. The method for manufacturing the anode of a tantalum capacitor as described in claim 1, characterized in that, The step of using the tantalum foil as the working electrode to perform electrochemical etching by applying voltage to generate nanoscale channels on the three-dimensional micropillars includes: Using the tantalum foil as the working electrode, an electrochemical etching process is performed by applying voltage with the first electrochemical process parameters to generate first channels in the sidewalls and skeleton of each three-dimensional micropillar. Electrochemical etching is performed by applying voltage with the second electrochemical process parameters to form a second channel with a smaller diameter than the first channel on the inner wall of the first channel.

6. The method for manufacturing the anode of a tantalum capacitor as described in claim 5, characterized in that, The diameter of the first channel is 300-500 nm, and the diameter of the second channel is 30-50 nm.

7. The method for manufacturing the anode of a tantalum capacitor as described in claim 1, characterized in that, The step of performing the first cleaning treatment on the tantalum foil of the preset thickness includes: Tantalum foil of a predetermined thickness is placed in acetone and anhydrous ethanol for ultrasonic cleaning in sequence. Then immerse it in a 5% hydrofluoric acid solution for a preset time. Finally, the tantalum foil was cleaned with deionized water and dried with nitrogen gas.

8. The method for manufacturing the anode of a tantalum capacitor as described in claim 2, characterized in that, The step of performing a second cleaning treatment on the anode of the tantalum capacitor includes: The electrochemically etched tantalum foil was immersed in deionized water for ultrasonic cleaning, and then dried using a nitrogen stream.

9. A tantalum capacitor anode, characterized in that, The tantalum capacitor anode is manufactured by the manufacturing method described in any one of claims 1-8.