A preparation method of an in-situ ceramic particle reinforced medium-entropy alloy composite coating based on controllable oxidizing atmosphere and AlTi alloying synergistic induction regulation

By adding TiAl alloy powder to CoNi-based medium-entropy alloy powder and performing laser cladding under a controllable oxidizing atmosphere, core-shell nano-oxides are formed, solving the problems of single phase composition control and high process cost of medium-entropy alloy-based coatings, and achieving high hardness, low friction coefficient and good wear resistance of the coating.

CN123132877APending Publication Date: 2026-11-20SUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611656540.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-26
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In existing technologies, the phase composition control method of medium-entropy alloy-based coatings is singular, the process cost is high, and the in-situ formation of nano-oxides is difficult to achieve, making it difficult to achieve both good plastic deformation capacity and high hardness and wear resistance in medium-entropy alloy-based coatings.

Method used

By adding TiAl alloy powder to CoNi-based entropy alloy powder, mixing them by ball milling, and then performing laser cladding under a controllable oxidizing atmosphere, a core-shell nano-oxide with an Al₂O₃ core and a Ti shell is formed. The volume fraction of carbon dioxide in the protective atmosphere is adjusted to control the content of FCC and BCC phases, thereby achieving synchronous control of the coating phase composition.

Benefits of technology

This study achieved a medium-entropy alloy composite coating that maintains high hardness while exhibiting a low steady-state coefficient of friction and less wear, thus improving wear resistance and microstructure stability and reducing process costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123132877A_ABST
    Figure CN123132877A_ABST
Patent Text Reader

Abstract

This application relates to the field of laser cladding technology, specifically to a method for preparing an in-situ ceramic particle-reinforced medium-entropy alloy composite coating based on the synergistic induction and regulation of a controllable oxidizing atmosphere and AlTi alloying. The method includes: adding TiAl alloy powder to CoNi-based medium-entropy alloy powder; laser cladding the mixed powder under a protective atmosphere of Ar and CO2, wherein the TiAl alloy powder accounts for 7%-15% of the mass fraction of the mixed metal powder; and controlling the effective oxygen content in the laser molten pool region by adjusting the CO2 content in the mixed gas, thereby selectively oxidizing elements such as Al and Ti. This application, while maintaining a constant AlTi content, achieves control over the composition of the FCC and BCC phases of the coating by adjusting the oxidizing properties of the protective atmosphere, simultaneously generating core-shell nano-oxides in situ. This allows the coating to maintain high hardness while improving tribological properties, reducing the cost of phase composition control, and increasing process flexibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of laser cladding technology, specifically relating to a method for preparing an in-situ ceramic particle-reinforced medium-entropy alloy composite coating based on the synergistic induction and regulation of controllable oxidizing atmosphere and AlTi alloying. Background Technology

[0002] With the increasing demands on the service performance of key components in aerospace, energy, and high-end equipment manufacturing, surface strengthening technology has become an important research direction for improving the strength, wear resistance, corrosion resistance, and high-temperature microstructure stability of metallic materials. Laser cladding, characterized by high energy density, small heat-affected zone, adjustable dilution rate, and metallurgical bonding between the coating and the substrate, is suitable for the preparation of medium-entropy alloys and multi-principal element alloy composite coatings. CoNi-based medium-entropy alloys, such as FeCoNi, CoCrNi, and CoNiV, typically exhibit good plasticity, toughness, and corrosion resistance. Their face-centered cubic (FCC) solid solutions provide good deformation compatibility, but the hardness and load-bearing capacity of a single FCC structure are relatively limited. Introducing body-centered cubic (BCC) phases can improve overall performance through mechanisms such as synergistic deformation of soft and hard phases and phase interface resistance to dislocation movement.

[0003] Al and Ti are important elements for controlling the phase composition of such alloys. Adding TiAl powder to CoNi-based medium-entropy alloys can promote the formation of BCC-related structures. However, excessive Al and Ti content or local segregation may lead to the formation of coarse ordered phases, brittle intermetallic compounds or other undesirable second phases. Meanwhile, existing technologies usually rely solely on changing the powder ratio to adjust the phase composition, which increases the number of powder preparation and process optimizations, as well as the cost of raw materials and processes.

[0004] On the other hand, elements such as Al, Ti, and V and Cr in some medium-entropy alloys have high oxygen affinity and can selectively react with a suitable amount of active oxygen under the high-temperature conditions of the laser cladding pool to form nano-oxides in situ. Compared with directly added oxide particles, in-situ generated nano-oxides have the characteristics of small size, stable interfacial bonding, and easy dispersion within grains, grain boundaries, or phase boundaries. They can improve the stability of the microstructure by hindering dislocation movement and pinning grain and phase boundaries. Existing laser cladding processes usually use Ar to suppress macroscopic oxidation of the molten pool, making it difficult to stably obtain nano-oxides with specific morphologies such as core-shell structures. Summary of the Invention

[0005] One objective of this invention is to provide a method for preparing an in-situ ceramic particle-reinforced medium-entropy alloy composite coating based on the synergistic induction and regulation of a controllable oxidizing atmosphere and AlTi alloying, thereby solving the technical problems of the existing medium-entropy alloy-based coating phase composition regulation method being singular, the process cost being high, and the difficulty in simultaneously controlling the coating phase composition and the in-situ formation of nano-oxides.

[0006] Another objective of this invention is to enable medium-entropy alloy-based composite coatings to achieve both good plastic deformation capacity and high hardness and wear resistance.

[0007] According to the purpose of this invention, this invention provides a method for preparing an in-situ ceramic particle-reinforced medium-entropy alloy composite coating based on the synergistic induction and regulation of controllable oxidizing atmosphere and AlTi alloying, comprising the following steps: TiAl alloy powder was added to CoNi-based medium-entropy alloy powder, and the mixture was ball-milled and then dried to obtain a mixed metal powder. The mixed metal powder is laid on the surface of a stainless steel substrate to form a pre-formed powder layer; Under a protective atmosphere, the pre-placed powder layer is laser-clad to obtain a composite coating with core-shell nano-oxides; wherein, The core-shell nano-oxide has a core-shell structure composed of an Al2O3 core and a Ti shell, and the mass fraction of the TiAl alloy powder in the mixed metal powder is 7%-15%. The protective atmosphere is formed by at least one of argon and carbon dioxide, and the volume fraction of carbon dioxide in the protective atmosphere is any value between 0% and 100%. The phase content of FCC phase and BCC phase in the composite coating is controlled by adjusting the volume fraction of carbon dioxide. Increasing the volume fraction of carbon dioxide increases the phase content of FCC phase and decreases the phase content of BCC phase.

[0008] Furthermore, the particle size of the metal elements in the CoNi-based medium-entropy alloy powder is 15μm-53μm.

[0009] Furthermore, during the laser cladding process, the laser power is 600W-1400W, the scanning speed is 3mm / s-20mm / s, and the spot diameter is 2mm-6mm.

[0010] Furthermore, the protective atmosphere flow rate is 20 L / min-25 L / min.

[0011] Furthermore, the thickness of the pre-placed powder layer is 0.3mm-0.8mm.

[0012] Furthermore, the argon gas and the carbon dioxide gas are introduced into a static mixer after the flow rate is adjusted by a flow controller, and mixed in the static mixer to form the protective atmosphere.

[0013] Furthermore, the process of laying the pre-set powder layer includes: adding the mixed metal powder into the powder trough of the motor-driven scraper-type powder spreading device, and driving the lead screw and scraper to move along the powder spreading direction by the motor to form the pre-set powder layer.

[0014] This application achieves simultaneous control of the phase composition and nano-oxide content of the cladding layer in a CoNi-based medium-entropy alloy powder system through a multi-step synergistic approach involving powder composition control, powder homogenization treatment, pre-laying powder, protective atmosphere adjustment, and laser cladding. Specifically, controlling the mass fraction of TiAl alloy powder to 7%-15% provides a foundation for the formation of the BCC phase and the selective oxidation of Al and Ti. Ball milling is used to uniformly disperse the TiAl alloy powder among the CoNi-based medium-entropy alloy powder. Laser cladding is then performed under a protective atmosphere of a mixed gas with a carbon dioxide volume fraction of 0%-100%. By adjusting the carbon dioxide volume fraction, the effective oxygen content in the molten pool is altered, causing different degrees of selective oxidation of oxyphilic elements in Al, Ti, and the CoNi-based medium-entropy alloy. This changes the content of effective elements participating in the formation of the metal phase, resulting in an overall increase in the FCC phase content in the cladding layer with increasing carbon dioxide volume fraction, while the BCC phase content decreases accordingly. This allows for the control of the relative content of the FCC and BCC phases without repeatedly changing the powder ratio, reducing process costs. Meanwhile, the high-temperature molten pool generated by laser cladding and its rapid solidification process promote the in-situ formation of core-shell nano-oxides with Al2O3 cores and Ti-rich oxide shells in the cladding layer, reducing the uneven dispersion and insufficient interfacial bonding that may be caused by directly added oxide particles.

[0015] In the composite coating of this application, the FCC phase provides deformation coordination capability, the BCC phase provides hardness and load-bearing capacity, and the dispersed core-shell nano-oxides can hinder dislocation movement and pin grain boundaries and phase boundaries. The three work together to enable the composite coating to maintain high hardness while having a low steady-state friction coefficient and less wear, thereby improving the wear resistance and microstructure stability of the cladding layer.

[0016] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, the preferred embodiments of the present invention are described in detail below with reference to the accompanying drawings. Attached Figure Description

[0017] The following sections will describe some specific embodiments of the invention in detail by way of example and not limitation, with reference to the accompanying drawings. The same reference numerals in the drawings denote the same or similar parts or portions. Those skilled in the art should understand that these drawings are not necessarily drawn to scale. In the drawings: Figure 1 This is a schematic flowchart illustrating the preparation of an in-situ ceramic particle-reinforced medium-entropy alloy composite coating based on the synergistic induction and regulation of a controllable oxidizing atmosphere and AlTi alloying in one embodiment of the present invention. Figure 2 These are SEM images and EDS distribution diagrams of the CoNi-based medium-entropy alloy powder in Example 1 of this invention; Figure 3 These are SEM images and EDS distribution diagrams of the mixed metal powder in Example 1 of this invention; Figure 4 These are low-magnification and high-magnification EBSD phase distribution diagrams of the composite coating prepared in Example 1 of this invention; Figure 5 These are low-magnification and high-magnification EBSD phase distribution diagrams of the composite coating prepared in Example 2 of this invention; Figure 6 These are low-magnification and high-magnification EBSD phase distribution diagrams of the composite coating prepared in Example 3 of this invention; Figure 7 These are low-magnification EBSD phase distribution diagrams of the composite coatings prepared in Examples 4-6 of this invention; Figure 8 These are the XRD patterns of the composite coatings prepared in Examples 1-3 of this invention; Figure 9 These are TEM images of the core-shell nano-oxides in the composite coating prepared in Example 2 of this invention; Figure 10 This is an elemental distribution diagram of the core-shell nano-oxides in the composite coating prepared in Example 2 of this invention; Figure 11 This is a selected area electron diffraction (SED) result of the core-shell nano-oxide in the composite coating prepared in Example 2 of this invention. Figure 12 This is a hardness comparison diagram of the composite coatings prepared in Examples 1-3 of the present invention and the CoNiV coatings prepared in Comparative Examples 1-3; Figure 13 The graph shows the friction and wear coefficients of the composite coatings prepared in Examples 1-3 of this invention and the CoNiV coating prepared in Comparative Example 1. Figure 14 These are three-dimensional morphological images of the wear marks of the composite coatings prepared in Examples 1-3 of this invention and the CoNiV coating prepared in Comparative Example 1. Figure 15These are the wear track cross-sectional depth profile curves of the composite coatings prepared in Examples 1-3 of this invention and the CoNiV coating prepared in Comparative Example 1. Detailed Implementation

[0018] The specific embodiments of the present invention will be described in further detail below with reference to the accompanying drawings and examples. The following examples are for illustrative purposes only and are not intended to limit the scope of the invention.

[0019] To make the above-mentioned objectives, features, and advantages of this application more apparent and understandable, the specific embodiments of this application will be described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustrative purposes only and are not intended to limit the scope of this application. Furthermore, it should be noted that, for ease of description, only the parts relevant to this application are shown in the accompanying drawings, not the entire structure. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without inventive effort are within the scope of protection of this application.

[0020] The terms “comprising” and “having”, and any variations thereof, used in this application are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or apparatus that includes a series of steps or units is not limited to the steps or units listed, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to such process, method, product, or apparatus.

[0021] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0022] Figure 1 This is a schematic flowchart illustrating the preparation of an in-situ ceramic particle-reinforced medium-entropy alloy composite coating based on the synergistic induction and regulation of a controllable oxidizing atmosphere and AlTi alloying, according to one embodiment of the present invention.

[0023] like Figure 1 As shown, this invention provides a method for preparing a medium-entropy alloy-based composite coating with controllable oxidizing atmosphere and phase composition, comprising the following steps: Step S100: Add TiAl alloy powder to CoNi-based medium-entropy alloy powder, mix by ball milling, and then dry to obtain mixed metal powder; Step S200: The mixed metal powder is laid on the surface of the stainless steel substrate to form a pre-formed powder layer; Step S300: Laser cladding is performed on the pre-placed powder layer under a protective atmosphere of argon and carbon dioxide to obtain a composite coating with core-shell nano-oxides. The core-shell nano-oxides consist of an Al2O3 core and a Ti shell, and the mass fraction of TiAl alloy powder in the mixed metal powder is 7%-15%. That is, the mass fraction of TiAl alloy powder can be 7%, 9%, 11%, 13%, or 15%, or any other value within the 7%-15% range. The protective atmosphere is formed by at least one of argon and carbon dioxide, and the volume fraction of carbon dioxide in the protective atmosphere is any value within the 0%-100% range. That is, the volume fraction of carbon dioxide can be 0%, 20%, 40%, 60%, 80%, or 100%, or any other value within the 0%-100% range. The phase content of FCC and BCC phases in the composite coating is controlled by adjusting the volume fraction of carbon dioxide. Increasing the volume fraction of carbon dioxide increases the phase content of the FCC phase and decreases the phase content of the BCC phase.

[0024] In this embodiment, through the synergistic multi-step process of powder composition control, powder homogenization treatment, pre-laying powder, protective atmosphere adjustment, and laser cladding, the phase composition and nano-oxide content of the cladding layer are simultaneously regulated in a CoNi-based medium-entropy alloy powder system. Specifically, controlling the mass fraction of TiAl alloy powder to 7%-15% provides a foundation for the formation of the BCC phase and the selective oxidation of Al and Ti. Ball milling is used to uniformly disperse the TiAl alloy powder among the CoNi-based medium-entropy alloy powder. Laser cladding is then performed under a protective atmosphere of a mixed gas with a carbon dioxide volume fraction of 0%-100%. By adjusting the carbon dioxide volume fraction, the effective oxygen content in the molten pool is altered, causing different degrees of selective oxidation of the oxygen-loving elements in Al, Ti, and the CoNi-based medium-entropy alloy. This changes the content of effective elements participating in the formation of the metal phase, resulting in an overall increase in the FCC phase content in the cladding layer with increasing carbon dioxide volume fraction, while the BCC phase content decreases accordingly. Therefore, the relative content of the FCC and BCC phases can be controlled without repeatedly changing the powder ratio, reducing process costs. Meanwhile, the high-temperature molten pool generated by laser cladding and its rapid solidification process promote the in-situ formation of core-shell nano-oxides with Al2O3 cores and Ti-rich oxide shells in the cladding layer, reducing the uneven dispersion and insufficient interfacial bonding that may be caused by directly added oxide particles.

[0025] In this embodiment, the FCC phase provides deformation coordination capability, the BCC phase provides hardness and load-bearing capacity, and the dispersed core-shell nano-oxides can hinder dislocation movement and pin grain boundaries and phase boundaries. The three work together to enable the composite coating to maintain high hardness while having a low steady-state friction coefficient and less wear, thereby improving the wear resistance and microstructure stability of the cladding layer.

[0026] In this embodiment, ball milling and mixing are used to uniformly distribute TiAl alloy powder (7%-15% by mass) among CoNi-based medium-entropy alloy powder. After the mixed metal powder is placed on the surface of a stainless steel substrate, it is rapidly melted under laser irradiation to form a molten pool containing Co, Ni, Al, and Ti. The Al and Ti introduced by the TiAl alloy powder can change the phase stability relationship of the alloy system and promote the formation of BCC-related phases. When the volume fraction of carbon dioxide in the protective atmosphere is low, the oxidation degree of the molten pool is low, and more Al and Ti are retained in the molten metal, which is conducive to the formation of the BCC phase. As the volume fraction of carbon dioxide increases, the effective oxygen content in the molten pool increases, and Al, Ti, and other oxyphilic elements in the medium-entropy alloy undergo selective oxidation. Some Al and Ti are transferred from the metallic phase to the oxide phase, reducing the effective Al and Ti content participating in the formation of the BCC phase, thereby reducing the BCC phase content and retaining or increasing the FCC phase. During selective oxidation, Al preferentially combines with oxygen to form a stable Al2O3 core, and Ti subsequently accumulates around the Al2O3 core to form a Ti-rich oxide shell. After rapid solidification in a laser molten pool, the FCC phase, BCC phase, and core-shell nano-oxides are retained in the cladding layer, ultimately forming a composite coating reinforced by the FCC / BCC dual-phase structure and in-situ nano-oxides.

[0027] In other embodiments, when the TiAl alloy powder accounts for less than 7% of the mass fraction of the mixed metal powder, the content of Al and Ti elements participating in promoting the formation of the BCC phase is relatively low. Even if the effective oxygen content in the molten pool region is changed by adjusting the volume fraction of carbon dioxide in the mixed gas, the remaining Al and Ti content in the metallic phase after selective oxidation of Al and Ti elements is insufficient to form a distinguishable BCC-related structure under different atmospheric conditions, resulting in the coating phase composition being difficult to change significantly with the change of carbon dioxide volume fraction. When the TiAl alloy powder accounts for more than 15% of the mass fraction of the mixed metal powder, the content of Al and Ti elements participating in promoting the formation of the BCC phase is excessive, even if carbon dioxide... Carbon dioxide selectively oxidizes and consumes some Al and Ti elements. The remaining Al and Ti content in the metal phase is still sufficient to maintain the structure dominated by the BCC-related phase. As a result, the phase composition of the coating is also difficult to change significantly with the change of carbon dioxide volume fraction. Therefore, controlling the mass fraction of TiAl alloy powder in the mixed metal powder within the range of 7%-15% can keep the initial content of Al and Ti elements in the metal phase within a suitable range. This ensures that there are enough Al and Ti elements to participate in the formation of the BCC phase, and that this content can be effectively adjusted by the change of carbon dioxide volume fraction. This ensures that the atmosphere-controlled phase composition method of the present invention has a good control effect within this mass fraction range.

[0028] In a further embodiment, the CoNi-based medium-entropy alloy powder includes at least one of FeCoNi, CoCrNi, and CoNiV, and the CoNi-based medium-entropy alloy powder is composed of the corresponding metal elements in equimolar ratios. In this embodiment, various Co and Ni-containing medium-entropy alloys such as FeCoNi, CoCrNi, and CoNiV can be prepared using the method of this application. Using equimolar ratios helps to ensure the uniformity and stability of the phase structure of the powder system itself.

[0029] In a further embodiment, the particle size of the metal elements in the CoNi-based medium-entropy alloy powder is 15μm-53μm, that is, the particle size of the metal elements in the CoNi-based medium-entropy alloy powder can be 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, or 53μm, or any other value within the range of 15μm-53μm. Controlling the particle size of the CoNi-based medium-entropy alloy powder within the above range is beneficial for forming a uniform powder layer during the pre-laying process, reducing problems such as agglomeration and poor flowability caused by excessively fine powder particles, or uneven powder laying and insufficient laser melting caused by excessively coarse particles. This ensures uniform melting and stable microstructure in the subsequent laser cladding process, providing a basis for the controllable formation of phase composition and nano-oxides.

[0030] In a further embodiment, the laser power during laser cladding is 600W-1400W, the scanning speed is 3mm / s-20mm / s, and the spot diameter is 2mm-6mm. That is, the laser power can be 600W, 700W, 800W, 900W, 1000W, 1100W, 1200W, 1300W, or 1400W, or any other value among 600W-1400W; the scanning speed can be 3mm / s, 6mm / s, 9mm / s, 12mm / s, 15mm / s, 18mm / s, or 20mm / s, or any other value among 3mm / s-20mm / s; and the spot diameter can be 2mm, 3mm, 4mm, 5mm, or 6mm, or any other value among 2mm-6mm. By coordinating the adjustment of laser power, scanning speed and spot diameter, the laser energy input and the formation and solidification process of the molten pool can be controlled, so that the dilution rate of the composite coating is kept at about 10%. This ensures that there is enough energy to fully melt the mixed metal powder and form a continuous cladding layer that is well bonded to the substrate metallurgy, while avoiding excessive heat input, excessive dilution rate or coarsening of the structure caused by excessive power or slow scanning speed.

[0031] In a further embodiment, the protective atmosphere flow rate is 20 L / min-25 L / min, meaning the flow rate can be 20 L / min, 21 L / min, 22 L / min, 23 L / min, 24 L / min, or 25 L / min, or any other value within the range of 20 L / min-25 L / min. By controlling the protective atmosphere flow rate, argon and carbon dioxide can be continuously delivered to the laser molten pool region, forming a relatively stable protective atmosphere and oxidizing atmosphere during the cladding process. A suitable gas flow rate helps maintain the stability of the atmosphere composition in the molten pool region, allowing carbon dioxide to continuously participate in the regulation of the oxidizing atmosphere in the molten pool region, thereby improving the stability and repeatability of the oxidizing atmosphere regulation, and facilitating the stable control of the phase composition and nano-oxide formation in the cladding layer.

[0032] In a further embodiment, the thickness of the pre-placed powder layer is 0.3mm-0.8mm, that is, the thickness of the pre-placed powder layer can be 0.3mm, 0.4mm, 0.5mm, 0.6mm, 0.7mm, or 0.8mm, or any other value among 0.3mm-0.8mm. By controlling the thickness of the pre-placed powder layer, the mixed metal powder can be distributed on the substrate surface in a more uniform and stable state, reducing insufficient powder melting caused by an excessively thick powder layer and insufficient cladding layer thickness caused by an excessively thin powder layer, thereby improving the consistency of coating formation.

[0033] In a further embodiment, argon and carbon dioxide gases are introduced into a static mixer after their flow rates are regulated by a flow controller, where they mix to form the protective atmosphere. By separately adjusting the flow rates of argon and carbon dioxide by the flow controller, precise control of the ratio of the two gases can be achieved; the static mixer ensures that the two gases are fully mixed before entering the molten pool region, thereby guaranteeing a stable and consistent composition of the mixed gas reaching the molten pool region, allowing the selective oxidation process of elements such as Al and Ti to proceed stably throughout the entire cladding area.

[0034] In a further embodiment, the pre-laid powder layer process includes: adding mixed metal powder into the powder trough of a motor-driven scraper-type powder spreading device; and using a motor to drive a lead screw and scraper to move along the powder spreading direction to form a pre-laid powder layer. Compared to manual powder spreading or other non-mechanized powder spreading methods, the motor-driven scraper-type powder spreading device can precisely control the moving speed and displacement of the scraper through lead screw transmission, thereby ensuring that the pre-laid powder layer has a uniform thickness and a smooth surface, reducing thickness deviations, local accumulation, and powder shortages caused by manual operation.

[0035] Example 1: S1: Add TiAl powder to equimolar CoNiV pre-alloyed powder, mechanically mix in a ball mill, and dry for 3 hours to obtain a mixed powder, wherein TiAl powder accounts for 10% of the total mass of the mixed powder; S2: Using 304 stainless steel with dimensions of 80×50×10mm as a substrate, the mixed powder is added to the powder trough of a motor-driven scraper-type powder spreading device. The gap between the scraper and the 304 stainless steel is adjusted to form a uniform pre-placed powder layer with a thickness of about 0.5mm on the substrate surface.

[0036] S3: A 100% Ar protective atmosphere is used, with the total flow rate controlled at 25 L / min. A 2 kW fiber laser is used to laser cladize the pre-placed powder layer, ensuring complete melting of the powder to form a laser cladding layer. The parameters during the laser cladding process are: spot diameter 4 mm, defocusing amount -10 mm, total gas flow rate 25 L / min, laser power 700 W, and scanning speed 14 mm / s.

[0037] Example 2: The only difference from Example 1 is that in step S3, the protective atmosphere is a mixture of CO2 with a volume fraction of 40% and Ar with a volume fraction of 60%, while the other reaction conditions are completely the same.

[0038] Example 3: The only difference from Example 1 is that the protective gas in step S3 is 100% CO2 gas, while the other reaction conditions are exactly the same.

[0039] Example 4: The only difference from Example 1 is that in step S1, TiAl powder accounts for 7% of the total mass of the mixed powder, while the other reaction conditions are completely the same.

[0040] Example 5: The only difference from Example 2 is that in step S1, TiAl powder accounts for 7% of the total mass of the mixed powder, while the other reaction conditions are completely the same.

[0041] Example 6: The only difference from Example 3 is that in step S1, TiAl powder accounts for 7% of the total mass of the mixed powder, while the other reaction conditions are completely the same.

[0042] Comparative Example 1: The only difference from Example 1 is that TiAl powder was not added in step S1.

[0043] Comparative Example 2: The only difference from Example 2 is that TiAl powder was not added in step S1.

[0044] Comparative Example 3: The only difference from Example 3 is that TiAl powder was not added in step S1.

[0045] Figure 2 These are SEM images and EDS distribution diagrams of the CoNi-based medium-entropy alloy powder in Example 1 of this invention. Figure 2 Image (a) is a SEM image of the CoNi-based medium-entropy alloy powder in Example 1 of this invention. Figure 2 (b) is the EDS distribution diagram of Co element in CoNi-based medium-entropy alloy powder in Example 1 of the present invention. Figure 2 (c) EDS distribution diagram of Ni element in CoNi-based medium-entropy alloy powder in Example 1 of the present invention. Figure 2 (d) is the EDS distribution diagram of V element in CoNi-based medium-entropy alloy powder in Example 1 of the present invention.

[0046] like Figure 2 As shown, the CoNi-based medium-entropy alloy powder in Example 1 is generally spherical or nearly spherical (refer to...). Figure 2 In (a) of the sample, the particle size distribution ranges from 15 μm to 53 μm, and the elements Co, Ni, and V are uniformly distributed within individual particles and in the powder group (see reference). Figure 2 (b) in Figure 2 (d) in Example 1 shows that the CoNi-based medium-entropy alloy powder has good sphericity and compositional uniformity, which can provide a raw material basis for stable element supply in the subsequent uniform powder spreading and cladding process.

[0047] Figure 3 These are SEM images and EDS distribution diagrams of the mixed metal powder in Example 1 of this invention. Figure 3 Image (a) is a SEM image of the mixed metal powder in Example 1 of this invention. Figure 3 (b) is the EDS distribution diagram of Co element in the mixed metal powder in Example 1 of the present invention. Figure 3 (c) in the figure is the EDS distribution diagram of Ni element in the mixed metal powder in Example 1 of the present invention. Figure 3 (d) in the figure is the EDS distribution diagram of V element in the mixed metal powder in Example 1 of the present invention. Figure 3 (e) in the figure is the EDS distribution diagram of Al element in the mixed metal powder in Example 1 of the present invention. Figure 3 (f) is the EDS distribution diagram of Ti element in the mixed metal powder in Example 1 of the present invention.

[0048] like Figure 3 As shown in (a), the mixed metal powder as a whole also exhibits a spherical or near-spherical shape. Figure 3 In (b), the Co element is widely and relatively uniformly distributed in the mixed metal powder. Figure 3In (c), the Ni element is also relatively evenly distributed. Figure 3 In (d), the V element is also uniformly distributed in the mixed metal powder. Figure 3 As shown in (e), the overall content of Al in the mixed metal powder is relatively low, but its distribution is relatively uniform. Figure 3 In (f), the Ti element is also present in relatively small amounts and is distributed relatively evenly. Figure 3 (b) in Figure 3 (f) shows that Al and Ti elements are distributed in the form of discrete TiAl particles between the CoNiV powders, indicating that after ball milling and mixing, TiAl powder is relatively uniformly dispersed between the medium-entropy alloy powders without obvious agglomeration, which provides a basis for subsequent laser cladding.

[0049] Figure 4 These are low-magnification and high-magnification EBSD phase distribution diagrams of the laser cladding layer prepared in Example 1 of this invention. Figure 4 Image (a) is a low-magnification EBSD phase distribution diagram of the laser cladding layer prepared in Example 1. Figure 4 (b) is a high-magnification EBSD phase distribution diagram of the laser cladding layer prepared in Example 1.

[0050] like Figure 4 As shown in (a), under low-magnification EBSD and in a 100% Ar atmosphere (Example 1), the area fraction of the BCC-related phase in the composite coating is approximately 98.8%, and the FCC phase is close to 0. Figure 4 As shown in (b) in the figure, the area fraction of the BCC-related phase is approximately 98.5% under high-magnification EBSD, which is basically consistent with the results at low magnification. Figure 4 This indicates that under a 100% Ar atmosphere without the introduction of carbon dioxide, the Al and Ti elements introduced by the TiAl powder are mainly retained in the metal melt, significantly promoting the formation of BCC-related structures. The coating structure is dominated by a single BCC phase at both the macroscopic and microscopic scales, with no obvious two-phase structure characteristics.

[0051] Figure 5 These are low-magnification and high-magnification EBSD phase distribution diagrams of the composite coating prepared in Example 2 of this invention. Figure 5 (a) is a low-magnification EBSD phase distribution diagram of the composite coating prepared in Example 2. Figure 5 (b) is a high-magnification EBSD phase distribution diagram of the composite coating prepared in Example 2.

[0052] Figure 5 As can be seen in (a), the central region of the coating is still dominated by the BCC phase, with an area fraction of about 61.3% under low magnification EBSD, but the peripheral region has obvious FCC phase distribution, with an area fraction of about 37.8%; Figure 5 As can be seen in (b), the BCC phase and the FCC phase are intertwined.

[0053] Comparing Example 2 with Example 1, it can be seen that after introducing 40% carbon dioxide, the coating has obviously changed from a near-single BCC phase structure to a structure in which BCC and FCC coexist. The two phases exhibit clear dual-phase characteristics at both the low-magnification macroscopic scale and the high-magnification microscopic scale.

[0054] Figure 6 These are low-magnification and high-magnification EBSD phase distribution diagrams of the composite coating prepared in Example 3 of this invention. Figure 6 (a) is a low-magnification EBSD phase distribution diagram of the composite coating prepared in Example 3. Figure 6 Figure (b) shows the high-magnification EBSD phase distribution of the composite coating prepared in Example 3. Compared with Example 2, the area occupied by the FCC phase (the lighter-colored outer periphery and part of the inner area in the figure) is further expanded, and the low-magnification FCC phase area fraction increases to approximately 51.4%. Figure 6 In (a) of the high-density FCC phase, the area fraction increased to 33.4%. Figure 6 (b)). This figure shows that when the CO2 volume fraction is increased to 100%, the phase content of the FCC phase further increases, while the phase content of the BCC phase further decreases.

[0055] Table 1 shows the above. Figures 4-6 The statistical results of the phase content of FCC and BCC phases in the composite coatings prepared in Examples 1-3 are shown in low and high magnification EBSD phases.

[0056] Table 1. FCC / BCC phase content of composite coatings in Examples 1-3

[0057] Combination Figures 4-6 As shown in Table 1, with the TiAl addition amount remaining constant, by increasing the volume fraction of carbon dioxide in the mixed gas from 0% to 40% and then to 100% (corresponding to Examples 1-3), the area fraction of the BCC-related phase in the coating decreased from approximately 98.8% (Example 1, low magnification) to approximately 61.3% (Example 2) and approximately 47.2% (Example 3), while the area fraction of the FCC phase correspondingly increased from nearly 0% (Example 1) to approximately 37.8% (Example 2) and approximately 51.4% (Example 3). The same trend was observed in the high-magnification local areas. The numerical differences between the low-magnification and high-magnification results stemmed from the different EBSD observation field sizes and the non-uniformity of the local coating structure, but the trends were consistent. These results demonstrate that, without changing the powder ratio, simply adjusting the volume fraction of carbon dioxide in the protective atmosphere can achieve a transformation in the coating structure from a single BCC phase to a BCC / FCC dual-phase coexistence with continuously adjustable phase ratios at both the macroscopic and microscopic scales.

[0058] Figure 7 These are low-magnification EBSD phase distribution diagrams of the composite coatings prepared in Examples 4-6 of this invention. Figure 7 Image (a) is a low-magnification EBSD phase distribution diagram of the composite coating prepared in Example 4 (100% Ar). Figure 7 Image (b) is a low-magnification EBSD phase distribution diagram of the composite coating prepared in Example 5 (40% CO2 + 60% Ar). Figure 7 (c) is a low-magnification EBSD phase distribution diagram of the composite coating prepared in Example 6 (100% CO2). The light-colored area in the diagram represents the FCC phase, and the dark-colored area represents the BCC phase.

[0059] like Figure 7 As shown, when the TiAl alloy powder accounts for 7% of the mixed metal powder, under a 100% Ar atmosphere, the composite coating is dominated by the BCC phase, with only a small amount of light-colored FCC phase present at the coating edge contour. Figure 7 As shown in (a)), under a 40% CO2 + 60% Ar atmosphere, the coating microstructure transforms into a microstructure dominated by the FCC phase, with fine, discretely distributed BCC phase particles scattered within it. Figure 7 As shown in (b) of the figure, under a 100% CO2 atmosphere, the composite coating is still dominated by the FCC phase, while the BCC phase is further reduced, with only a small amount of BCC phase distributed at the bottom of the coating. Figure 7 (as shown in (c)).

[0060] Will Figure 7 (a) Figure 7 (b) and Figure 7 As can be seen from the comparison in (c), under the condition of TiAl mass fraction of 7%, as the volume fraction of CO2 in the protective atmosphere increases from 0% to 40% and 100%, the coating phase composition changes from BCC phase to FCC phase. This shows that when the TiAl mass fraction is 7%, the coating phase composition can also be effectively controlled by adjusting the volume fraction of carbon dioxide in the protective atmosphere. This further verifies that the atmosphere-controlled phase composition method described in this invention has good applicability in the range of TiAl mass fraction of 7%-15%.

[0061] Figure 8 These are XRD patterns of the composite coatings prepared in Examples 1-3 of this invention.

[0062] like Figure 8As shown, the composite coating prepared under a 100% Ar atmosphere (Example 1) mainly exhibits BCC-related diffraction characteristics (where L21 in the spectrum is the BCC ordered phase), and no FCC-related diffraction peaks are observed. After the atmosphere is adjusted to 40% CO2 + 60% Ar, FCC-related diffraction peaks are clearly observed in the spectrum, while BCC-related diffraction peaks are still present. Under a 100% CO2 atmosphere, the FCC-related diffraction characteristics are further enhanced. Figure 8 It can also be demonstrated that as the volume fraction of CO2 in the mixed atmosphere increases, the coating gradually changes from being dominated by the BCC phase to being coexisting with the FCC phase and the BCC phase.

[0063] Figure 9 This is a TEM image of the core-shell nano-oxide in the composite coating prepared in Example 2 of this invention. Figure 9 As shown, nanoscale oxide particles can be observed in the composite coating prepared in Example 2. The particles exhibit two distinct layers, namely the core region and the shell region, which are clearly distinguishable in morphology. This indicates that nanoscale oxide particles with core-shell structure characteristics were generated in situ in the composite coating under an oxidizing atmosphere containing CO2.

[0064] Figure 10 This is an elemental distribution diagram of the core-shell nano-oxides in the composite coating prepared in Example 2 of this invention. Figure 10 (a) in the figure is the elemental distribution diagram of Co in the core-shell nano-oxide in the composite coating prepared in Example 2 of the present invention. Figure 10 (b) in the figure is the elemental distribution diagram of V in the core-shell nano-oxide in the composite coating prepared in Example 2 of the present invention. Figure 10 (c) in the figure is the elemental distribution diagram of Ti element in the core-shell nano-oxide in the composite coating prepared in Example 2 of the present invention. Figure 10 (d) in the figure is the elemental distribution diagram of Al in the core-shell nano-oxide in the composite coating prepared in Example 2 of the present invention. Figure 10 (e) in the figure is the elemental distribution diagram of O element in the core-shell nano-oxide in the composite coating prepared in Example 2 of the present invention. Figure 10 (f) is the elemental distribution diagram of Ni in the core-shell nano-oxide in the composite coating prepared in Example 2 of the present invention.

[0065] from Figure 10 As can be seen in (a), the region where the nano-oxide is located ( Figure 10 In (a), the irregular polyhedral outline region appears dark, while the region surrounding the nano-oxide appears bright. The Co element signal is strong, indicating that the Co element is mainly distributed on the outside of the nano-oxide and does not participate in the formation of the nano-oxide.

[0066] from Figure 10As can be seen in (b), the region where the nano-oxide is located ( Figure 10 In (b), the irregular polyhedral outline region is generally dark and the V element signal is weak. However, a transition region with slightly enhanced local brightness can be observed near the edge outline of the nano oxide, indicating that there are a small amount of V element enrichment at the edge of the particle shell. This suggests that V element may be involved in the local oxidation of the nano oxide shell region.

[0067] from Figure 10 As can be seen in (c), the edges of the nano-oxides show obvious bright ring-shaped areas, while the central area of ​​the nano-oxides is relatively dark, indicating that Ti elements are mainly enriched in the outer shell area of ​​the particles, and the Ti element signal in the central area is weak, forming a Ti-rich shell.

[0068] from Figure 10 (d) in Figure 10 As can be seen in (e), the internal region of the nano-oxide is enriched with Al and O elements. Figure 10 (d) in Figure 10 The bright circular region in (e) corresponds to the Al2O3 phase.

[0069] Figure 10 The Ni element in (f) and Figure 10 The distribution characteristics of Co in (a) are similar, while Ni is mainly distributed on the outside of the nano oxide.

[0070] Figure 11 This is a selected area electron diffraction (SED) pattern of the core-shell nano-oxide in the composite coating prepared in Example 2 of this invention. Figure 11 Image (a) shows the selected area electron diffraction pattern of the core-shell nano-oxide shell region along the 110 zone axis, labeled as Ti-VO phase. Figure 11 (b) is a selected area electron diffraction pattern of the core-shell nano-oxide shell region along the 01-1 zone axis and labeled as Ti-O phase.

[0071] like Figure 11 As shown, Figure 11 In (a), the diffraction spots are labeled as (1-11), (002), (1-1-1), (00-2), (-111), and (-11-1), and the spots are arranged in a regular hexagonal pattern. The labeling result is Ti-VO phase. Figure 11 In (b), the diffraction spots are labeled as (111), (200), (-111), (-200), (1-1-1), (-1-1-1), which are also arranged in a hexagonal pattern. The labeling result is Ti-O phase. Figure 11 (a) Figure 11(b) in the above examples together show that the outer shell region of the core-shell nano-oxide is mainly rich in Ti oxide. In some of the particles, the outer shell is accompanied by the enrichment of V element, forming Ti-VO composite oxide. In other particles, no obvious enrichment of V element is detected in the outer shell, forming simple Ti-O oxide. This further illustrates that the core-shell nano-oxide of the present invention has a core-shell structure with an Al2O3 core and a Ti oxide-rich outer shell.

[0072] Figure 12 This is a hardness comparison chart between the composite coatings prepared in Examples 1-3 of this invention and the CoNiV coatings prepared in Comparative Examples 1-3. From... Figure 12 As can be seen, the hardness of Comparative Examples 1-3 in atmospheres of 100% Ar, 40% CO2 + 60% Ar, and 100% CO2 is approximately 284.7 N / mm. 2 324.6 N / mm 2 369.4 N / mm 2 When TiAl was added at 10% of the total mass of the mixed powder (Examples 1-3), the hardness under the corresponding atmosphere increased to approximately 596.4 N / mm. 2 591.3 N / mm 2 582.4 N / mm 2 The concentrations were significantly higher than those of the control group without TiAl in all three atmospheres. Figure 12 The results show that the addition of TiAl can significantly improve the hardness of the coating, and this hardness improvement effect can be maintained under different CO2 volume fraction atmospheres. The hardness of the composite coating fluctuates only slightly with the increase of CO2 volume fraction, indicating that the phase composition control method of the present invention does not significantly sacrifice the hardness performance of the coating while changing the phase composition of the composite coating.

[0073] Figure 13 This is a graph showing the friction and wear coefficients of the composite coatings prepared in Examples 1-3 of this invention and the CoNiV coating prepared in Comparative Example 1. From... Figure 13 It is evident that the friction coefficients of each sample fluctuated during the initial break-in period, gradually stabilizing thereafter. The steady-state friction coefficients of the composite coatings in Examples 1-3 were generally lower than those of the composite coating prepared in Comparative Example 1, indicating that the coatings prepared in this invention exhibit superior frictional response and lower wear. Furthermore, as the volume fraction of CO2 in the mixed gas atmosphere increased, the friction coefficients of the composite coatings prepared in Examples 2 and 3 after reaching steady state were lower than those in Examples 1 and Comparative Example 1, demonstrating the beneficial effects of the synergistic effect of the FCC and BCC phases, as well as the dispersion reinforcement of core-shell nano-oxides, on improving the stability of the coating's tribological properties.

[0074] Figure 14 These are three-dimensional morphological images of the wear tracks of the composite coatings prepared in Examples 1-3 of this invention and the CoNiV coating prepared in Comparative Example 1. Figure 14 Image (a) shows the three-dimensional morphology of the wear marks on the coating of Comparative Example 1 (CoNiV, 100% Ar atmosphere). Figure 14 Image (b) is a three-dimensional morphology image of the wear marks on the coating of Example 1 (100% Ar atmosphere). Figure 14 Image (c) in the image is a three-dimensional morphology diagram of the wear marks on the coating of Example 2 (40% CO2 + 60% Ar atmosphere). Figure 14 (d) in the figure is a three-dimensional morphology diagram of the wear marks of the coating in Example 3 (100% CO2 atmosphere). The color bars on the left side of each figure represent the height distribution of the wear mark surface in pseudo-color, with the color from blue to red / orange indicating the height from low to high.

[0075] like Figure 14 As shown, Figure 14 In Comparative Example 1 (a), the maximum height of the color mark in the wear area of ​​the coating is approximately 78.01 μm. The wear groove area (blue area) is relatively wide and the color difference transition is relatively smooth. Figure 14 In Example (b), the maximum height of the color mark in the wear area of ​​the coating in Example 1 was reduced to about 34.62 μm, and the width and depth of the wear grooves were significantly reduced compared with Comparative Example 1. Figure 14 In Example 2 of Example (c), the maximum height of the color mark in the coating wear area is approximately 33.62 μm, the wear groove area is further narrowed, and the raised edges (red / orange areas) on both sides of the groove are clearer; Figure 14 In Example 3 (d), the maximum height of the color mark in the coating wear area is about 39.08 μm. The morphology of the wear groove is similar to that of Example 1 and Example 2, and the groove area is the smallest among the four groups of samples.

[0076] Will Figure 14 (a) to Figure 14 As can be seen from the comparison in (d), the three-dimensional morphology of the wear marks of the coatings in Examples 1-3 is significantly improved compared with that in Comparative Example 1. The width of the wear marks grooves and the range of surface height variation reflected by the color mark are reduced overall. At the same time, as the proportion of carbon dioxide in the mixed gas increases, the wear mark groove area of ​​the composite coating is further reduced, indicating that the addition of TiAl and the method of atmosphere control phase composition can effectively improve the wear resistance of the composite coating.

[0077] Figure 15 These are the wear track cross-sectional depth profile curves of the composite coatings prepared in Examples 1-3 of this invention and the CoNiV coating prepared in Comparative Example 1.

[0078] in Figure 15 In the figure, (a) is the cross-sectional depth profile curve of the wear track of the coating in Comparative Example 1 (CoNiV, 100% Ar atmosphere), A1 is the peak point of the left edge of the wear track groove, A2 is the lowest point of the bottom of the wear track groove, and A3 is the peak point of the right edge of the wear track groove. Figure 15 In (b), the cross-sectional depth profile curve of the wear mark of the coating in Example 1 (100% Ar atmosphere) is shown. B1 is the peak point of the left edge of the wear mark groove, B2 is the lowest point of the bottom of the wear mark groove, and B3 is the peak point of the right edge of the wear mark groove. Figure 15 In Example 2 (40% CO2 + 60% Ar atmosphere), (c) is the cross-sectional depth profile curve of the wear mark of the coating. C1 is the peak point of the left edge of the wear mark groove, C2 is the lowest point of the bottom of the wear mark groove, and C3 is the peak point of the right edge of the wear mark groove. Figure 15 In the figure, (d) is the cross-sectional depth profile curve of the wear mark of the coating in Example 3 (100% CO2 atmosphere), D1 is the peak point of the left edge of the wear mark groove, D2 is the lowest point of the bottom of the wear mark groove, and D3 is the peak point of the right edge of the wear mark groove.

[0079] like Figure 15 As shown, Figure 15 In Comparative Example 1 (a), the lowest point depth of the wear groove in the coating is approximately 7.54 μm, and the calculated wear volume is 1.17 mm. 3 ; Figure 15 In Example 1 (b), the lowest point depth of the wear groove in the coating is approximately 4.92 μm, and the wear volume is reduced to 0.38 mm. 3 ; Figure 15 In Example 2 (c), the lowest point depth of the coating wear groove is approximately 13.84 μm, and the wear volume is further reduced to 0.24 mm. 3 ; Figure 15 In Example 3 (d), the lowest point depth of the wear groove in the coating is approximately 5.71 μm, and the wear volume is 0.21 mm. 3 It is the smallest among the four groups of samples.

[0080] Comparing Examples 1-3, it can be seen that the wear volume decreases with the increase of carbon dioxide volume fraction in the protective atmosphere, indicating that adjusting the ratio of FCC phase to BCC phase in the composite coating is beneficial to reduce the wear amount of the coating and improve the wear resistance of the coating.

[0081] In summary, under the premise that the TiAl alloy powder accounts for 7%-15% of the mixed metal powder, as the volume fraction of CO2 in the protective atmosphere increases from 0% to 40% and then to 100%, the BCC phase content in the coating gradually decreases while the FCC phase content gradually increases. Furthermore, the low-magnification and high-magnification EBSD and XRD results show consistent changes, indicating that the BCC / FCC phase composition of the coating can be continuously controlled by adjusting the CO2 volume fraction. Simultaneously, core-shell nano-oxides composed of an Al2O3 core and a Ti-rich oxide shell can be formed in situ under a CO2 atmosphere, demonstrating that atmosphere control can simultaneously regulate the coating phase composition and nano-oxide structure. In terms of performance, the coating hardness increases from 284.7 N / mm² after the addition of TiAl. 2 -369.4 N / mm 2 Increased to 582.4 N / mm 2 -596.4 N / mm 2 This significantly improved the coating hardness, and the hardness of the composite coating fluctuated only slightly with the increase of CO2 volume fraction. While changing the phase composition of the composite coating, it did not significantly sacrifice the coating's hardness performance. Simultaneously, the overall steady-state friction coefficient of the composite coating decreased, and the wear volume decreased from 1.17 mm in the comparative example. 3 The thickness was reduced to 0.38 mm. 3 0.24mm 3 and 0.21mm 3 Meanwhile, as the volume fraction of CO2 increases, the wear volume of the composite coating further decreases, indicating that this application improves the wear resistance of the composite coating without sacrificing its hardness by controlling the volume fraction of carbon dioxide and thus controlling the BCC / FCC phase composition in the coating.

[0082] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0083] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A method for preparing an in-situ ceramic particle-reinforced medium-entropy alloy composite coating based on the synergistic induction and regulation of controllable oxidizing atmosphere and AlTi alloying, characterized in that, Includes the following steps: TiAl alloy powder was added to CoNi-based medium-entropy alloy powder, and the mixture was ball-milled and then dried to obtain a mixed metal powder. The mixed metal powder is laid on the surface of a stainless steel substrate to form a pre-formed powder layer; Under a protective atmosphere, the pre-placed powder layer is laser-clad to obtain a composite coating with core-shell nano-oxides; wherein, The core-shell nano-oxide has a core-shell structure composed of an Al2O3 core and a Ti shell, and the mass fraction of the TiAl alloy powder in the mixed metal powder is 7%-15%. The protective atmosphere is formed by at least one of argon and carbon dioxide, and the volume fraction of carbon dioxide in the protective atmosphere is any value between 0% and 100%. The phase content of FCC phase and BCC phase in the composite coating is controlled by adjusting the volume fraction of carbon dioxide. Increasing the volume fraction of carbon dioxide increases the phase content of FCC phase and decreases the phase content of BCC phase.

2. The preparation method according to claim 1, characterized in that, The CoNi-based medium-entropy alloy powder includes at least one of FeCoNi, CoCrNi, and CoNiV, and the CoNi-based medium-entropy alloy powder is composed of the corresponding metal elements in an equimolar ratio.

3. The preparation method according to claim 2, characterized in that, The particle size of the metal elements in the CoNi-based medium-entropy alloy powder is 15μm-53μm.

4. The preparation method according to claim 1, characterized in that, During the laser cladding process, the laser power is 600W-1400W, the scanning speed is 3mm / s-20mm / s, and the spot diameter is 2mm-6mm.

5. The preparation method according to claim 1, characterized in that, The protective atmosphere flow rate is 20L / min-25L / min.

6. The preparation method according to claim 1, characterized in that, The thickness of the pre-placed powder layer is 0.3mm-0.8mm.

7. The preparation method according to claim 1, characterized in that, The argon gas and the carbon dioxide gas are introduced into a static mixer after the flow rate is adjusted by a flow controller, and they are mixed in the static mixer to form the protective atmosphere.

8. The preparation method according to claim 6, characterized in that, The process of laying the pre-set powder layer includes: adding the mixed metal powder into the powder trough of the motor-driven scraper-type powder spreading device, and using the motor to drive the lead screw and scraper to move along the powder spreading direction to form the pre-set powder layer.