Process for hot deformation lubrication and oxidation prevention of copper-nickel alloys
By using a composite lubricating coating and a three-stage atmosphere treatment during the hot deformation process of copper-nickel alloys, the problem of preferential oxidation of grain boundaries caused by carbide embedding during the hot deformation process of copper-nickel alloys was solved, and the high efficiency of oxidation prevention and corrosion resistance of copper-nickel alloys was significantly improved.
Patent Information
- Application Number
- CN202611337465.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-20
AI Technical Summary
During the hot deformation of copper-nickel alloys, the decomposition products of conventional carbon-containing lubricants embed into the grain boundaries of the alloy surface, which synergistically couples with the alloy oxidation behavior, leading to preferential oxidation of the grain boundaries. This problem gradually emerges during subsequent cooling, storage, or service, affecting the long-term reliability of the product.
A composite lubricating coating composed of glass powder and nano-sized SnO₂ powder is applied to the surface of copper-nickel alloy billet. During the hot deformation process, a molten lubricating film is formed. The coating is then subjected to a three-stage atmosphere treatment: oxidation burn-off, reduction repair, and rapid cooling to eliminate residual carbides and prevent preferential oxidation of grain boundaries.
It effectively reduces the amount of residual carbon on the alloy surface, controls the depth of the grain boundary oxide layer to within 2μm, significantly improves corrosion resistance, and solves the stress cracking and grain boundary preferential oxidation hysteresis defects caused by the thermal expansion mismatch between carbides and matrix. It is suitable for hot extrusion, hot rolling and hot forging of copper-nickel alloys such as B10, B30 and C71500.
Smart Images

Figure CN123132879A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of non-ferrous metal hot working technology, specifically relating to a hot deformation lubrication and anti-oxidation process for copper-nickel alloys. Background Technology
[0002] Copper-nickel alloys (such as B10, B30, C71500, and C70600) are widely used in marine engineering fields such as marine seawater condensation systems and heat exchangers in coastal power plants due to their excellent resistance to seawater corrosion, high heat transfer coefficient, superior resistance to microbial adhesion, and good hot and cold working properties. Copper-nickel alloys can be manufactured into products such as thick plates, large-diameter pipes, and thick bars through methods such as hot rolling and hot extrusion.
[0003] In hot extrusion, hot rolling, or hot forging of copper-nickel alloys, lubrication is crucial for ensuring product quality and extending die life. Currently, for the extrusion of nickel and nickel alloys, cupronickel, and other alloy tubes and bars with high resistance to high-temperature deformation, "glass pads" or glass powder coatings are commonly used as extrusion lubricants in China. Glass lubricants melt into a liquid film at temperatures ranging from 450℃ to 2200℃, extending with metal deformation to form a high-viscosity, complete fluid lubricating film on the deformed metal surface. This film separates the metal from the deformation tool, providing lubrication and insulation. However, glass lubricants present several problems in practical applications. Extruded products lubricated with "glass pads" often have residual glass lubricant on their surface, resulting in severe peeling and "dust inclusions," causing significant problems for subsequent processing. Furthermore, conventional glass lubricants often contain carbonaceous components such as graphite and carbon black to improve lubrication performance. However, the incomplete decomposition of these carbonaceous components at high temperatures forms carbide particles that embed into the alloy surface, posing a serious threat to product quality.
[0004] Through long-term production practice, the inventors discovered a long-overlooked, hidden quality problem in the hot deformation process of copper-nickel alloys: conventional carbon-containing lubricants (such as the organic components in graphite-based, oil-based, or glass lubricants) undergo incomplete decomposition at high temperatures. The decomposition products, especially free carbon / carbide particles, are partially embedded in the grain boundaries of the alloy surface. In the solid solution state, copper-nickel alloys are a single-phase α-solid solution, with the surface oxide film mainly composed of Cu₂O and NiO. These carbide particles form micro-stress concentrations between themselves and the alloy matrix due to the difference in their coefficients of thermal expansion. The coefficient of thermal expansion of the carbides is approximately 4~6 × 10⁻⁶. -6 / ℃, while copper-nickel alloys are approximately 16~18×10 -6 The temperature drops to a certain level (°C), causing the surface oxide film to preferentially crack at the carbide-matrix interface. Oxygen then penetrates along the crack channels to the grain boundaries, forming a "grain boundary preferential oxidation zone" dominated by NiO. This oxidation zone is difficult to completely remove during subsequent cold working or pickling processes, ultimately leading to stress corrosion cracks or pitting initiation at this location in the finished product during subsequent service.
[0005] What's more challenging is that this problem doesn't manifest during the hot deformation process, but rather gradually emerges during subsequent cooling, storage, or service. It's a typical "hysteresis defect," easily overlooked yet severely impacting the long-term reliability of the product. Currently, there is no systematic solution in existing technology for this "carbide-induced preferential oxidation of grain boundaries" problem.
[0006] Therefore, in order to address the above-mentioned technical problems, it is necessary to provide a process for hot deformation lubrication and anti-oxidation of copper-nickel alloys. Summary of the Invention
[0007] The purpose of this invention is to provide a lubrication and anti-oxidation process for hot deformation of copper-nickel alloys, which can solve the hidden technical problem that the decomposition products of conventional carbon-containing lubricants embed into the grain boundaries of the alloy surface during the hot deformation of copper-nickel alloys, and have a synergistic coupling effect with the alloy oxidation behavior, inducing preferential oxidation of the grain boundaries.
[0008] To achieve the above objectives, a specific embodiment of the present invention provides the following technical solution:
[0009] A hot deformation lubrication and anti-oxidation process for copper-nickel alloys includes the following steps:
[0010] S1. Lubricant pretreatment: Coating the surface of the copper-nickel alloy billet with a composite lubricant coating;
[0011] S2. Hot deformation: The blank coated with the composite lubricating coating is subjected to hot deformation processing at a hot deformation temperature, during which the composite lubricating coating forms a molten lubricating film;
[0012] S3. In-situ atmosphere treatment after demolding: After the heat-deformed part leaves the deformation zone and before cooling to 600℃, a three-stage atmosphere treatment is performed sequentially:
[0013] The first stage of oxidation and burn-off treatment: an oxygen-rich atmosphere is introduced to oxidize and burn off the residual carbides;
[0014] The second stage of reduction and repair treatment involves introducing a reducing protective atmosphere to reduce the surface oxide film to a metallic state.
[0015] The third stage of rapid cooling: the workpiece is forced to cool to below 500°C;
[0016] S4. Post-cooling treatment: Perform a short-time weak acid wash on the cooled product.
[0017] In one or more embodiments of the present invention, in step S1, the composite lubricating coating is composed of glass powder, nano-sized SnO2 powder and water-based binder; wherein the particle size of the nano-sized SnO2 powder is 50~200nm, the median particle size D50 of the glass powder is 10~30μm, and the mass ratio of the SnO2 powder to the glass powder is 1:(4~15).
[0018] The SnO2 powder melts and softens preferentially over the glass powder during the heat deformation heating process and adheres to the surface of the glass powder particles. This serves to pre-catalyze the cracking of the organic components in the lubricant before the glass powder melts and spreads, thus inhibiting the organic components from condensing into polycyclic aromatic hydrocarbon carbon precursors.
[0019] In one or more embodiments of the present invention, the coating thickness of the composite lubricating coating on the surface of the blank is controlled to be 80~150μm;
[0020] When the coating melts in the initial stage of hot deformation, the micron-sized CO / CO2 bubbles generated by the SnO2-catalyzed oxidative decomposition of organic components form a porous buffer structure within the molten glass layer. This porous buffer structure reduces the peak shear stress between the molten glass layer and the billet surface at the initial moment of hot deformation. At the same time, when the bubbles escape, they carry some undecomposed carbon particles away from the alloy surface, achieving bubble-assisted self-cleaning.
[0021] In one or more embodiments of the present invention, in step S2, the heating rate of the billet from room temperature to the heat distortion temperature is controlled at 15~30℃ / min;
[0022] At this heating rate, the nano-SnO2 in the composite lubricating coating reaches its catalytic activity peak in the temperature range of 400~600℃, making the oxidation reaction rate constant K of the carbonaceous component in the lubricant at 600℃ at least 3 times that under conventional non-catalytic conditions. This allows the main mass fraction of the carbonaceous component to be converted into gaseous products before the heat deformation temperature is reached, thus avoiding solid-phase carbon precipitation reaction of the carbonaceous component during the high-temperature deformation stage.
[0023] In one or more embodiments of the present invention, in step S2, the strain rate of the hot deformation process is 0.1~10s. -1 ;
[0024] During hot deformation, dynamic recrystallization occurs on the alloy surface, generating fresh grain boundaries. The diffusion coefficient of the incompletely converted trace residual carbonaceous components in the composite lubricating coating at the fresh grain boundaries is suppressed by the interface pinning effect of SnO2. SnO2 nanoparticles are oriented along the deformation direction at the subgrain boundaries, increasing the grain boundary diffusion activation energy of the residual carbonaceous components from the original 120~150kJ / mol to over 200kJ / mol, physically blocking the channels for carbonaceous components to penetrate into the grain boundary.
[0025] In one or more embodiments of the present invention, in step S3, the atmosphere of the first stage of oxidation and burn-off treatment also contains 10~20 vol% CO2 gas, and the CO2 and oxygen-enriched air together constitute an oxidation-gasification dual-function atmosphere.
[0026] The CO2 reacts with the residual solid carbides at 600-800°C in a Bourdon gasification reaction.
[0027] C + CO₂ → 2CO;
[0028] The gasification reaction proceeds in tandem with the oxygen oxidation reaction. The Bodor gasification reaction takes precedence over the oxygen oxidation reaction in acting on the hidden carbides embedded in the microcracks of the alloy surface. It utilizes the characteristic that the size of CO2 molecules is smaller than that of O2 molecules to penetrate deep into the bottom of the microcracks for gasification and removal, thus avoiding overheating of the alloy surface caused by local reaction overheating in a pure oxygen atmosphere.
[0029] In one or more embodiments of the present invention, in step S3, the dew point of the atmosphere in the second stage of reduction and repair treatment is controlled between -30°C and -40°C;
[0030] During the reduction and repair process, H2 preferentially reacts with NiO exposed at the grain boundary due to the previous oxidation and burn-off to generate metallic Ni and H2O vapor. At the same time, by controlling the dew point, the oxygen partial pressure in the atmosphere is precisely adjusted to be lower than the Cu2O / Cu equilibrium oxygen partial pressure but higher than the NiO / Ni equilibrium oxygen partial pressure. This allows the reduction reaction to selectively occur preferentially at the grain boundary NiO rather than on the surface of the alloy substrate, thus maintaining the overall metallic luster of the substrate surface while repairing the oxidation defects at the grain boundary.
[0031] In one or more embodiments of the present invention, in step S3, a transition gas curtain isolation process is provided between the first oxidation burn-off treatment and the second reduction repair treatment. The transition gas curtain is vertically blown at the junction of the two treatment zones using nitrogen or argon at a flow rate of 40~80L / min.
[0032] The air curtain is used to physically isolate the atmosphere between the oxidation section and the reduction section, preventing the risk of combustion and explosion caused by the mixing of H2 and residual O2. At the same time, the airflow of the air curtain blows the carbide dust and debris that fall off after oxidation and burning away from the alloy surface, preventing the debris from being reduced and fixed on the alloy surface in the reduction section to form secondary inclusions.
[0033] In one or more embodiments of the present invention, in step S3, the cooling rate of the third rapid cooling process is ≥80℃ / s, and the cooling medium is a water mist mixture containing 3~8wt% ethanol.
[0034] When the ethanol component comes into contact with the high-temperature alloy surface, it evaporates and absorbs heat, generating a micro-explosion effect. This disrupts the gaseous boundary layer between the alloy surface and the residual atmosphere during the cooling process. At the same time, the rapid cooling rate is used to suppress the non-equilibrium segregation of Ni elements at the grain boundaries due to the vacancies left after the carbides on the alloy surface are burned off. This restores the Ni / Cu ratio at the grain boundaries to be consistent with the matrix, thereby shutting down the chemical driving force for preferential oxidation at the grain boundaries from the root.
[0035] In one or more embodiments of the present invention, the copper-nickel alloy is a B30 or C71500 series alloy with a nickel content of ≥30wt%, and the hot deformation processing is hot extrusion forming of tubes or bars.
[0036] The process is designed for alloys with a nickel content of ≥30wt% that have lower NiO formation free energy and a more significant tendency for grain boundary oxidation. After the three-stage atmosphere treatment in step S3, the depth of the grain boundary oxide layer on the alloy surface is ≤2μm, and after pickling in step S4, the pitting potential of the product in 3.5wt% NaCl solution is shifted at least 150mV in a positive direction compared to the control product that has not undergone the three-stage atmosphere treatment.
[0037] Compared with existing technologies, the copper-nickel alloy hot deformation lubrication and anti-oxidation process of the present invention, through the catalytic cracking effect of SnO2 in the composite lubricating coating and the synergistic effect of three-stage in-situ atmosphere treatment after hot deformation, fundamentally eliminates the problem of preferential grain boundary oxidation induced by the embedding of carbide particles from lubricant decomposition into the alloy surface grain boundaries. This reduces the residual carbon content on the alloy surface from 0.2~0.5 mg / cm³ in conventional processes. 2 Reduced to 0.05 mg / cm 2 The following method controls the depth of the grain boundary oxide layer to within 2 μm. Simultaneously, after short-term weak acid pickling, the pitting potential of the product in 3.5 wt% NaCl solution shifts at least 150 mV positively compared to the control product without three-stage atmosphere treatment. This significantly improves the corrosion resistance of the alloy surface, effectively solving the hidden hysteresis defects caused by stress cracking due to the thermal expansion mismatch between carbides and the matrix, as well as preferential oxidation of grain boundaries. Furthermore, this process is simple to operate, safe, and controllable, and is suitable for hot extrusion, hot rolling, and hot forging of copper-nickel alloys such as B10, B30, C71500, and C70600, showing broad industrial application prospects. Attached Figure Description
[0038] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0039] Figure 1 This is a flowchart illustrating the overall process of a copper-nickel alloy hot deformation lubrication and anti-oxidation process in one embodiment of the present invention.
[0040] Figure 2 This is a schematic diagram of a three-stage atmosphere treatment zone structure in a copper-nickel alloy hot deformation lubrication and anti-oxidation process according to an embodiment of the present invention.
[0041] Figure 3 This is a bar chart comparing the grain boundary oxide layer depth in a copper-nickel alloy hot deformation lubrication and anti-oxidation process according to an embodiment of the present invention.
[0042] Figure 4 This is a bar chart comparing the pitting potentials of a copper-nickel alloy hot deformation lubrication and anti-oxidation process in one embodiment of the present invention. Detailed Implementation
[0043] To enable those skilled in the art to better understand the technical solutions in this disclosure, the technical solutions in the embodiments of this disclosure will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this disclosure, and not all embodiments. Based on the embodiments in this disclosure, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this disclosure.
[0044] Example 1
[0045] like Figure 1 As shown, a hot deformation lubrication and anti-oxidation process for copper-nickel alloys includes the following steps:
[0046] S1. Lubricant pretreatment:
[0047] Preparation of the composite lubricating coating: Take 68 wt% glass powder with a softening point of 780℃ and a median particle size D50 of 20 μm; 10 wt% nano-sized SnO2 powder with a particle size of 80~150 nm; the balance is a water-based binder—sodium polyacrylate aqueous solution with a solid content of 15 wt%; place in a high-speed disperser and stir at 1200 r / min for 40 min until homogeneous. The mass ratio of SnO2 powder to glass powder is 1:6.8.
[0048] The B30 copper-nickel alloy billet was sequentially ultrasonically cleaned with acetone for 5 minutes, rinsed with deionized water, and dried with hot air. Then, the composite lubricating coating was uniformly applied to the billet surface using an air spraying method. The spraying pressure was 0.4 MPa, the spraying distance was 200 mm, and the coating thickness was controlled between 100 and 120 μm. After coating, the billet was dried in an oven at 80°C for 30 minutes.
[0049] S2. Thermal distortion:
[0050] The billet coated with the composite lubricating coating was placed in a medium-frequency induction heating furnace and heated from room temperature to the heat distortion temperature of 920℃ at a heating rate of 20℃ / min, and held at that temperature for 10 minutes to ensure uniform temperature inside and outside the billet. During this heating process, the nano-SnO2 in the composite lubricating coating reached its catalytic activity peak in the temperature range of 400~600℃, catalyzing the oxidative decomposition of trace organic binders in the lubricant.
[0051] The uniformly heated billet is transferred to the extrusion cylinder of a horizontal copper extruder and extruded at 920°C for 2 seconds. -1 Hot extrusion molding was performed at a strain rate of λ=12. During the hot deformation process, the glass component in the composite lubricating coating melted to form a continuous lubricating film. Under the action of extrusion shear stress, SnO2 nanoparticles were oriented along the deformation direction at the subgrain boundaries formed by dynamic recrystallization, increasing the grain boundary diffusion activation energy of the residual carbonaceous component to approximately 210 kJ / mol.
[0052] S3. Post-demolding atmosphere treatment:
[0053] like Figure 2 As shown, after the hot-extruded pipe exits the extrusion die, it enters a three-stage atmosphere treatment zone within 3 seconds. The total length of the treatment zone is 2.5m, and the pipe travels at a speed of approximately 0.5m / s.
[0054] The first stage, oxidation and ablation treatment (0.6m in length): Oxygen-enriched air containing 22 vol% oxygen (a mixture of compressed air and pure oxygen in a specific ratio) and 15 vol% CO2 gas is introduced at a total flow rate of 120 L / min. The pipe passes through this stage for 6 seconds. CO2 reacts with residual solid carbides via a Bourdon gasification reaction (C + CO2 → 2CO), synergistically removing residual carbides through oxidation with the oxygen. The temperature at the end of this stage is monitored at 720℃.
[0055] Transitional air curtain isolation (width 0.2m): High-purity nitrogen gas with a purity of 99.999% is used to vertically blow from top to bottom at a flow rate of 60L / min at the junction of the oxidation section and the reduction section. The air curtain is 150mm wide, which physically isolates the two atmospheres to prevent H2 from mixing with residual O2, and at the same time blows away the carbide dust that falls off after oxidation and burning off from the alloy surface.
[0056] The second stage, reduction and repair treatment (0.8m in length): A nitrogen-hydrogen mixed protective gas containing 8 vol% H2, composed of high-purity nitrogen and high-purity hydrogen in a specific ratio, is introduced. The atmosphere dew point is controlled at -35℃, the total gas flow rate is 100 L / min, and the pipe passage time in this stage is 10 seconds. H2 preferentially reacts with NiO exposed at the grain boundaries: NiO + H2 → Ni + H2O (g). The temperature at the end of this stage is monitored at 650℃.
[0057] The third stage, rapid cooling (0.9m in length): forced jet cooling is performed using a water mist mixture containing 5wt% ethanol at a pressure of 0.6MPa. The nozzles are arranged in a ring, and the cooling rate is 90℃ / s. The temperature of the pipe has dropped to 480℃ when it exits the cooling section. When the ethanol component comes into contact with the high-temperature alloy surface, it evaporates and absorbs heat, producing a micro-explosion effect. This breaks down the gas boundary layer between the alloy surface and the residual atmosphere during the cooling process, improving the uniformity of cooling.
[0058] S4. Post-cooling treatment:
[0059] The cooled pipe is placed in an acid pickling tank and pickled with a 6wt% dilute sulfuric acid solution at room temperature for 45 seconds. After being removed, it is washed with running water for 2 minutes, washed with deionized water for 1 minute, and dried with hot air to obtain the finished product.
[0060] Example 2
[0061] Except for the following parameters, everything else is the same as in Example 1:
[0062] Alloy grade: C71500 copper-nickel alloy, Ni content 30.5 wt%;
[0063] Composite lubricating coating: 72wt% glass powder, softening point 820℃, D50=25μm, 8wt% SnO2, particle size 50~120nm, mass ratio 1:9, water-based binder balance;
[0064] Coating method: Roller coating, coating thickness 90~110μm;
[0065] Heating rate: 25℃ / min; Heat distortion temperature: 950℃;
[0066] Strain rate: 5s -1 ;
[0067] First stage atmosphere: O2 20 vol% + CO2 12 vol%, total flow rate 150 L / min, processing time 8 seconds;
[0068] Air curtain: Argon gas, flow rate 50L / min;
[0069] Second stage: H2 6vol%, dew point -38℃, flow rate 120L / min, treatment time 12 seconds;
[0070] Third section: 6 wt% ethanol, cooling rate 100℃ / s;
[0071] Pickling: 5wt% H2SO4, 50 seconds.
[0072] Example 3
[0073] Except for the following parameters, everything else is the same as in Example 1:
[0074] Alloy grade: C70600 copper-nickel alloy, B10, Ni content 10.5wt%;
[0075] Hot deformation method: hot rolling of sheet metal, billet size 200×150×30mm;
[0076] Composite lubricating coating: 65wt% glass powder, softening point 760℃, D50=15μm, 12wt% SnO2 with particle size 100~200nm, mass ratio 1:5.4, balance water-based binder;
[0077] Coating method: brush coating, coating thickness 80~100μm;
[0078] Heating rate: 18℃ / min; Heat distortion temperature: 880℃;
[0079] Strain rate: 0.5s -1 ;
[0080] First stage atmosphere: O2 24 vol% + CO2 18 vol%, total flow rate 80 L / min, processing time 5 seconds;
[0081] Air curtain: Nitrogen, flow rate 70L / min;
[0082] Second stage: H2 9vol%, dew point -32℃, flow rate 90L / min, treatment time 8 seconds;
[0083] Third section: 4 wt% ethanol, cooling rate 85℃ / s;
[0084] Pickling: 7wt% H2SO4, 35 seconds.
[0085] Comparative Example 1
[0086] A commercially available glass lubricant for hot extrusion of copper alloys was applied to the surface of the B30 billet, with the same coating thickness as in Example 1. The commercially available glass lubricant for hot extrusion of copper alloys consisted of 75 wt% glass powder, 5 wt% graphite powder, and 20 wt% sodium silicate aqueous solution. The heat deformation parameters were consistent with those in Example 1. After heat deformation, the billet was directly cooled to room temperature with water at a rate of approximately 30°C / s, and then pickled with 6 wt% dilute sulfuric acid at room temperature for 60 seconds.
[0087] Comparative Example 2
[0088] The composite lubricating coating formulation and heat deformation parameters were exactly the same as in Example 1. After heat deformation and demolding, the coating was not placed in the three-stage atmosphere treatment zone, but directly cooled to room temperature by water at a rate of about 30°C / s. The pickling parameters were the same as in Example 1.
[0089] Comparative Example 3
[0090] The composite lubricating coating formulation and heat distortion parameters were exactly the same as in Example 1. After demolding, a three-stage atmosphere treatment was performed, but no CO2 gas was added to the first stage atmosphere; only oxygen-enriched air containing 22 vol% oxygen was introduced, with a total flow rate of 120 L / min and a treatment time of 6 seconds. The parameters of the second and third stages and the air curtain were the same as in Example 1.
[0091] Comparative Example 4
[0092] The composite lubricating coating formulation and heat distortion parameters are exactly the same as those in Example 1. After demolding, a three-stage atmosphere treatment is performed, but the second stage of reduction and repair treatment is omitted, i.e.: first stage (same as Example 1) → air curtain (same as Example 1) → third stage (same as Example 1), with no water mist or ethanol content.
[0093] Comparative Example 5
[0094] The composite lubricating coating formulation and heat distortion parameters are exactly the same as those in Example 1. After demolding, a complete three-stage atmosphere treatment is performed, with parameters for each stage being the same as in Example 1. However, the dew point of the atmosphere in the second stage of the reduction and repair treatment is controlled at -15°C, while the other parameters remain unchanged.
[0095] Experimental Example
[0096] To fully verify the feasibility and technical effectiveness of the present invention, the following experimental and control groups were designed:
[0097] Experimental materials: B30 copper-nickel alloy (Ni 30.2wt%, balance Cu and unavoidable impurities) tube blanks were used, with an outer diameter of Φ120mm, a wall thickness of 12mm, and a length of 200mm. The alloy chemical composition met the requirements of GB / T 5231-2022 standard.
[0098] Experimental Groups:
[0099]
[0100] The parts of each comparative example that are the same as those in Example 1 will not be repeated, and only the differences will be marked.
[0101] Detection method:
[0102] Surface carbon residue: measured using a LECO CS-230 carbon-sulfur analyzer according to ASTM E1019 standard.
[0103] Grain boundary oxide layer depth: After the sample was mounted and polished, it was measured at 200x magnification using a LEICA DMi8 optical microscope and Image-Pro Plus image analysis software. Ten fields of view were taken for each sample to calculate the average value.
[0104] Pitting potential: The potentiodynamic polarization curve was tested in a 3.5 wt% NaCl solution according to ASTM G61 standard, with a scan rate of 0.1667 mV / s and a current density of 10 μA / cm. 2 The potential at which the pitting corrosion occurred was taken as the pitting potential, and the average value of 3 parallel samples in each group was taken.
[0105] Ni / Cu atomic ratio at grain boundaries: The average Ni / Cu atomic ratio was measured at 5 points at the grain boundaries using a Thermo Scientific Apreo 2S field emission scanning electron microscope equipped with an EDS spectrometer, with an accelerating voltage of 15 kV.
[0106] Surface hardness: HVS-1000A Vickers hardness tester, load 200g, hold for 10s, average value of 5 points.
[0107] The experimental results are statistically analyzed, as shown in Table 1:
[0108] Table 1 Summary of process parameters and test results for each embodiment and comparative example
[0109]
[0110] Note: The matrix Ni / Cu atomic ratio of the solid solution-treated master alloy is 0.43, and the surface hardness is 148HV0.2; SCE is a saturated calomel electrode.
[0111] Data Analysis:
[0112] (a) Analysis of surface carbon residue
[0113] As shown in Table 1, the carbon residue in all embodiments (1-3) and most comparative examples (2-5) using the composite lubricating coating of the present invention is ≤0.04 mg / cm³. 2 This is far superior to the 0.35 mg / cm³ of Comparative Example 1, which uses a conventional graphite glass lubricant. 2 This indicates that the catalytic cracking effect of nano-SnO2 is the decisive factor in reducing carbon residue. Regardless of whether subsequent atmosphere treatment is performed, as long as the lubricating coating contains SnO2, the carbon residue on the surface after heat deformation can be reduced by about an order of magnitude.
[0114] In Comparative Example 1, a large amount of free carbon generated by the incomplete decomposition of graphite lubricant at high temperature remained on the surface, providing a sufficient "stress concentration source" for subsequent grain boundary oxidation.
[0115] (II) Analysis of Grain Boundary Oxide Layer Depth
[0116] The depth of the grain boundary oxide layer is a core indicator for measuring whether the technical problem to be solved by this invention—"carbide-induced preferential oxidation of grain boundaries"—has been effectively suppressed.
[0117] like Figure 3 As shown, the grain boundary oxide layer depth data of each group are compared:
[0118] Average value of Examples 1-3: 1.5 μm.
[0119] Among them, the original grain size of B30 alloy is about 65 μm, and the depth of the grain boundary oxide layer accounts for only 2.3% of the grain size, indicating that preferential oxidation at the grain boundaries is significantly suppressed.
[0120] Comparative Example 1 (conventional lubrication, no water cooling): 8.5 μm.
[0121] The large amount of carbon residue provides abundant crack sources, and oxygen penetrates deep into the grain boundaries along the carbide-matrix interface, with the grain boundary oxide layer depth being 5.7 times the average of the examples.
[0122] Comparative Example 2 (with SnO2, no atmosphere treatment): 6.2 μm. Although the carbon residue was reduced to 0.04 mg / cm³. 2 However, trace amounts of residual carbides still cause the oxide film to crack during cooling due to thermal expansion mismatch, and oxygen penetrates along the grain boundaries to form a deeper oxide zone. This indicates that simply reducing the amount of residual carbon with SnO2 is not enough to completely solve the problem; it must be combined with subsequent "oxidation burn-off + reduction repair" atmosphere treatment.
[0123] Comparative Example 3 (without CO2): 3.8 μm.
[0124] Although there was some improvement, local overheating in a pure oxygen atmosphere led to surface overburning, uneven oxide layer depth, and the appearance of "overburned" structural defects. This indicates that the addition of CO2 buffered the local reaction temperature rise through the endothermic effect of the Bourdon gasification reaction, thus having the dual functions of "carbon removal" and "temperature control".
[0125] Comparative Example 4 (without reduction segment): 5.1 μm.
[0126] This indicates that without the reduction and repair step, the exposed grain boundary NiO after the initial oxidation and burn-off cannot be selectively reduced, and the formed grain boundary oxide zone will still exist.
[0127] Comparative Example 5 (dew point -15℃, which is relatively high): 3.2μm.
[0128] A high dew point means that the water vapor content in the atmosphere is high, the oxygen partial pressure is too high, the reducing power of H2 is weakened, and some NiO at the grain boundaries is not completely reduced. This verifies the key importance of "controlling the dew point at -30~-40℃" for achieving selective reduction.
[0129] (III) Pitting Potential Analysis
[0130] Pitting potential is a key electrochemical indicator for evaluating the resistance of alloys to localized corrosion. A higher potential indicates a more stable passivation film on the alloy surface and stronger resistance to Cl-. - The stronger the erosion ability.
[0131] like Figure 4 As shown, the pitting potential range of Examples 1-3 is +172~+192mV (vs. SCE), with an average value of +183mV.
[0132] Comparative Example 1 (conventional process): -8mV, a negative shift of 191mV compared to the average value of the examples, indicating that the preferential oxidation zone at grain boundaries is located in Cl... - It becomes a preferred site for pitting corrosion initiation in the medium.
[0133] Comparative Example 2 (no atmosphere treatment): +18mV, a negative shift of 165mV compared to the average value of the examples. Even though the carbon residue has been reduced, the existing NiO oxide bands at the grain boundaries still significantly degrade the pitting corrosion resistance.
[0134] Comparative Example 3 (no CO2): +98mV, a negative shift of 85mV compared to the average of the examples. Localized overheating resulted in poor oxide film uniformity, limiting the increase in pitting potential.
[0135] Comparative Example 4 (without reduction segment): +52mV, a negative shift of 131mV compared to the average value of the examples, further verifying the necessity of the reduction and repair steps.
[0136] Comparative Example 5 (higher dew point): +125mV, a negative shift of 58mV compared to the average value of the examples, indicating incomplete reduction leading to some NiO residue at the grain boundaries.
[0137] The above data fully demonstrates that only by fully adopting the four-in-one technical solution of "SnO2 catalytic carbon reduction + CO2 oxidation and burn-off + dew point controllable selective reduction + rapid cooling" can the pitting potential be positively increased to a level of +150mV or higher, thus achieving a significant improvement in corrosion resistance.
[0138] (iv) Analysis of the relationship between the Ni / Cu atomic ratio at grain boundaries and the cooling rate
[0139] The Ni / Cu atomic ratio at grain boundaries reflects the degree of Ni segregation at grain boundaries. The Ni / Cu atomic ratio of the parent alloy matrix is 0.43.
[0140] The Ni / Cu atomic ratio at the grain boundaries in Examples 1-3 was 0.39-0.45, which was basically consistent with the matrix. This indicates that the rapid cooling at ≥80℃ / s, combined with the ethanol water mist micro-explosion effect to destroy the gas phase boundary layer, effectively suppressed the non-equilibrium segregation of Ni elements to the grain boundaries during the cooling process.
[0141] Comparative Example 1 (water cooling, cooling rate approximately 30℃ / s): The Ni / Cu atomic ratio at the grain boundaries reaches 0.78, which is much higher than that in the matrix. Ni is severely segregated at the grain boundaries, providing a chemical driving force for the preferential formation of NiO in the future.
[0142] Comparative Example 2 (no atmosphere treatment, water cooling): The Ni / Cu atomic ratio at the grain boundary was 0.72, and segregation was equally severe, indicating that the vacancies left after the carbide burn-off became a "trap" for the non-equilibrium segregation of Ni under slow cooling conditions.
[0143] The relationship between the Ni / Cu atomic ratio at grain boundaries and the cooling rate further illustrates that even if the carbides are burned off, if the cooling rate is insufficient, vacancies will still induce non-equilibrium segregation of Ni, causing the chemical state of the grain boundaries to deviate from the matrix, and the chemical driving force for the preferential oxidation of grain boundaries will be impossible to shut down.
[0144] (v) Surface hardness analysis
[0145] The surface hardness of Examples 1-3 is 152-160HV0.2, which is basically equivalent to the hardness of the master alloy matrix, indicating that the process of the present invention does not cause excessive hardening or softening damage to the alloy surface.
[0146] Comparative Example 1 showed a hardness of 184HV0.2, which was significantly higher. This was due to the "oxidative hardening" effect caused by the formation of a large amount of NiO oxide at the grain boundaries, which increased brittleness.
[0147] Comparative Example 2 has a hardness of 175HV0.2, which is still too high. Residual oxide layer caused surface hardening.
[0148] Comparative Example 3 has a hardness of 168HV0.2. In the local overheated areas, grain coarsening and oxidation hardening coexist, and the hardness distribution is uneven.
[0149] The hardness data, from a mechanical property perspective, corroborates that the process of this invention maintains a good mechanical state of the alloy surface while eliminating preferential oxidation zones at grain boundaries.
[0150] Supplementary verification experiment
[0151] Effect of heating rate on carbon residue: To verify the rationality of the heating rate range of 15~30℃ / min, based on Example 1, other parameters were kept unchanged, and only the heating rate was changed to investigate its effect on the carbon residue on the surface. The results are shown in Table 2.
[0152] Table 2 Surface carbon residue at different heating rates
[0153]
[0154] The results show that when the heating rate is too low (8℃ / min), the catalytic effect of SnO2 lasts too long in the low-temperature region (300~400℃), but the organic components are not fully vaporized at this temperature, and the SnO2 surface is covered by reaction products and partially deactivated. When the heating rate is too high (40℃ / min), the billet passes through the catalytic activity window of 400~600℃ too quickly, and the catalytic effect of SnO2 is not fully utilized. Therefore, a heating rate range of 15~30℃ / min can achieve a time match between the catalytic activity of SnO2 and the vaporization and decomposition of organic components, which is the optimal process window.
[0155] The effect of dew point in the reduction stage on selective reduction effect: To verify the technical effect of controlling the dew point in the range of -30~-40℃, based on Example 1, only the dew point of the second stage reduction atmosphere was changed to investigate its effect on the reduction selectivity of grain boundary NiO and the surface state of the substrate. The results are shown in Table 3.
[0156] Table 3. Grain boundary Ni / Cu atomic ratio and matrix surface state at different dew points
[0157]
[0158] The results show that when the dew point is below -40℃, the atmosphere is too dry. Although the reducing power of H2 is strong, its selectivity is poor. Cu2O on the substrate surface is also over-reduced, resulting in surface roughness and darkening of color. In the dew point range of -30~-40℃, the ideal selective reduction effect of "preferential reduction of grain boundary NiO and intact substrate surface" can be achieved. When the dew point is above -30℃, the water vapor content in the atmosphere increases, the oxygen partial pressure increases, the reducing power of H2 is weakened, and the Ni / Cu atomic ratio at the grain boundary increases significantly, approaching 0.50~0.51, indicating that the grain boundary NiO is not fully reduced, which is consistent with the data of Comparative Example 5 in Table 1.
[0159] Based on the data analysis of all the above embodiments and comparative examples, the following conclusions can be drawn:
[0160] First, the core innovation chain of this invention consists of four indispensable steps: "SnO2 catalytic carbon reduction → CO2 oxidation and burn-off → dew point-controlled selective reduction → rapid cooling". The absence of any step or deviation of parameters will prevent the "grain boundary preferential oxidation" problem from being completely solved.
[0161] Second, only when the technical solution of this invention is fully adopted can the following four indicators be met simultaneously: surface carbon residue ≤ 0.05 mg / cm³ 2 The grain boundary oxide layer depth is ≤2μm, the pitting potential is ≥+150mV (vs. SCE), and the Ni / Cu atomic ratio at the grain boundary is consistent with that of the matrix. These combined techniques have achieved the technical effect of completely eradicating this hysteresis defect from the mechanism of "carbide-induced preferential oxidation of grain boundaries".
[0162] Third, the process of this invention is well applicable to copper-nickel alloys with different nickel contents, such as B30, C71500, and C70600. The effect is more significant on B30 and C71500 alloys with a nickel content of ≥30wt%. This is consistent with the metallurgical characteristics of high-nickel alloys, which have lower NiO formation free energy and stronger tendency for grain boundary oxidation. This further verifies that this invention is a precise solution to this specific technical problem.
[0163] The process of this invention can be implemented by modifying existing copper alloy hot extrusion / hot rolling production lines. The main equipment added is a three-stage atmosphere treatment zone after the deformation zone, which occupies a length of about 3 to 5 meters. It has low investment costs, strong operational controllability, and is suitable for hot deformation processing of copper-nickel alloy tubes, bars, and plates such as B10, B30, C71500, and C70600. It has broad prospects for industrial promotion and application.
[0164] It will be apparent to those skilled in the art that this disclosure is not limited to the details of the exemplary embodiments described above, and that this disclosure can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of this disclosure is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within this disclosure. No reference numerals in the claims should be construed as limiting the scope of the claims.
[0165] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A hot deformation lubrication and anti-oxidation process for copper-nickel alloys, characterized in that, Includes the following steps: S1. Lubricant pretreatment: Coating the surface of the copper-nickel alloy billet with a composite lubricant coating; S2. Hot deformation: The blank coated with the composite lubricating coating is subjected to hot deformation processing at a hot deformation temperature, during which the composite lubricating coating forms a molten lubricating film; S3. In-situ atmosphere treatment after demolding: After the heat-deformed part leaves the deformation zone and before cooling to 600℃, a three-stage atmosphere treatment is performed sequentially: The first stage of oxidation and burn-off treatment: an oxygen-rich atmosphere is introduced to oxidize and burn off the residual carbides; The second stage of reduction and repair treatment involves introducing a reducing protective atmosphere to reduce the surface oxide film to a metallic state. The third stage of rapid cooling: the workpiece is forced to cool to below 500°C; S4. Cooling post-treatment: Perform a short-time weak acid wash on the cooled product.
2. The copper-nickel alloy hot deformation lubrication and anti-oxidation process according to claim 1, characterized in that, In step S1, the composite lubricating coating is composed of glass powder, nano-sized SnO2 powder and water-based binder; wherein the particle size of the nano-sized SnO2 powder is 50~200nm, the median particle size D50 of the glass powder is 10~30μm, and the mass ratio of the SnO2 powder to the glass powder is 1:(4~15). The SnO2 powder melts and softens preferentially over the glass powder during the heat deformation heating process and adheres to the surface of the glass powder particles. This serves to pre-catalyze the cracking of the organic components in the lubricant before the glass powder melts and spreads, thus inhibiting the organic components from condensing into polycyclic aromatic hydrocarbon carbon precursors.
3. The copper-nickel alloy hot deformation lubrication and anti-oxidation process according to claim 2, characterized in that, The thickness of the composite lubricating coating on the surface of the blank is controlled to be 80~150μm; When the coating melts in the initial stage of hot deformation, the micron-sized CO / CO2 bubbles generated by the SnO2-catalyzed oxidative decomposition of organic components form a porous buffer structure within the molten glass layer. This porous buffer structure reduces the peak shear stress between the molten glass layer and the billet surface at the initial moment of hot deformation. At the same time, when the bubbles escape, they carry some undecomposed carbon particles away from the alloy surface, achieving bubble-assisted self-cleaning.
4. The hot deformation lubrication and anti-oxidation process for copper-nickel alloys according to claim 1, characterized in that, In step S2, the heating rate of the billet from room temperature to the heat distortion temperature is controlled at 15~30℃ / min; At this heating rate, the nano-SnO2 in the composite lubricating coating reaches its catalytic activity peak in the temperature range of 400~600℃, making the oxidation reaction rate constant K of the carbonaceous component in the lubricant at 600℃ at least 3 times that under conventional non-catalytic conditions. This allows the main mass fraction of the carbonaceous component to be converted into gaseous products before the heat deformation temperature is reached, thus avoiding solid-phase carbon precipitation reaction of the carbonaceous component during the high-temperature deformation stage.
5. The copper-nickel alloy hot deformation lubrication and anti-oxidation process according to claim 1, characterized in that, In step S2, the strain rate of the hot deformation process is 0.1~10s. -1 ; During hot deformation, dynamic recrystallization occurs on the alloy surface, generating fresh grain boundaries. The diffusion coefficient of the incompletely converted trace residual carbonaceous components in the composite lubricating coating at the fresh grain boundaries is suppressed by the interface pinning effect of SnO2. SnO2 nanoparticles are oriented along the deformation direction at the subgrain boundaries, increasing the grain boundary diffusion activation energy of the residual carbonaceous components from the original 120~150kJ / mol to over 200kJ / mol, physically blocking the channels for carbonaceous components to penetrate into the grain boundary.
6. The hot deformation lubrication and anti-oxidation process for copper-nickel alloys according to claim 1, characterized in that, In step S3, the atmosphere of the first stage of oxidation and burn-off treatment also contains 10~20 vol% CO2 gas, and the CO2 and oxygen-enriched air together constitute an oxidation-gasification dual-function atmosphere. The CO2 reacts with the residual solid carbides at 600-800°C in a Bourdon gasification reaction. C + CO₂ → 2CO; The gasification reaction proceeds in tandem with the oxygen oxidation reaction. The Bodor gasification reaction takes precedence over the oxygen oxidation reaction in acting on the hidden carbides embedded in the microcracks of the alloy surface. It utilizes the characteristic that the size of CO2 molecules is smaller than that of O2 molecules to penetrate deep into the bottom of the microcracks for gasification and removal, thus avoiding overheating of the alloy surface caused by local reaction overheating in a pure oxygen atmosphere.
7. The hot deformation lubrication and anti-oxidation process for copper-nickel alloys according to claim 1, characterized in that, In step S3, the dew point of the atmosphere in the second stage of reduction and repair treatment is controlled between -30℃ and -40℃; During the reduction and repair process, H2 preferentially reacts with NiO exposed at the grain boundary due to the previous oxidation and burn-off to generate metallic Ni and H2O vapor. At the same time, by controlling the dew point, the oxygen partial pressure in the atmosphere is precisely adjusted to be lower than the Cu2O / Cu equilibrium oxygen partial pressure but higher than the NiO / Ni equilibrium oxygen partial pressure. This allows the reduction reaction to selectively occur preferentially at the grain boundary NiO rather than on the surface of the alloy substrate, thus maintaining the overall metallic luster of the substrate surface while repairing the oxidation defects at the grain boundary.
8. The hot deformation lubrication and anti-oxidation process for copper-nickel alloys according to claim 1, characterized in that, In step S3, a transition gas curtain isolation process is provided between the first oxidation and burn-off treatment and the second reduction and repair treatment. The transition gas curtain is vertically purged at the junction of the two treatment zones using nitrogen or argon at a flow rate of 40-80 L / min. The air curtain is used to physically isolate the atmosphere between the oxidation section and the reduction section, preventing the risk of combustion and explosion caused by the mixing of H2 and residual O2. At the same time, the airflow of the air curtain blows the carbide dust and debris that fall off after oxidation and burning away from the alloy surface, preventing the debris from being reduced and fixed on the alloy surface in the reduction section to form secondary inclusions.
9. The copper-nickel alloy hot deformation lubrication and anti-oxidation process according to claim 1, characterized in that, In step S3, the cooling rate of the third rapid cooling process is ≥80℃ / s, and the cooling medium is a water mist mixture containing 3~8wt% ethanol. When the ethanol component comes into contact with the high-temperature alloy surface, it evaporates and absorbs heat, generating a micro-explosion effect. This disrupts the gaseous boundary layer between the alloy surface and the residual atmosphere during the cooling process. At the same time, the rapid cooling rate is used to suppress the non-equilibrium segregation of Ni elements at the grain boundaries due to the vacancies left after the carbides on the alloy surface are burned off. This restores the Ni / Cu ratio at the grain boundaries to be consistent with the matrix, thereby shutting down the chemical driving force for preferential oxidation at the grain boundaries from the root.
10. The hot deformation lubrication and anti-oxidation process for copper-nickel alloys according to any one of claims 1 to 9, characterized in that, The copper-nickel alloy is a B30 or C71500 series alloy with a nickel content of ≥30wt%, and the hot deformation processing is hot extrusion forming of tubes or bars. The process is designed for alloys with a nickel content of ≥30wt% that have lower NiO formation free energy and a more significant tendency for grain boundary oxidation. After the three-stage atmosphere treatment in step S3, the depth of the grain boundary oxide layer on the alloy surface is ≤2μm, and after pickling in step S4, the pitting potential of the product in 3.5wt% NaCl solution is shifted at least 150mV in a positive direction compared to the control product that has not undergone the three-stage atmosphere treatment.