Method for separating iron and copper in copper sponge containing iron by synergistic copper increase in acid etching waste liquid regeneration

Through displacement, complexation, and oxidation reactions, the copper in the iron-containing sponge copper is dissolved and concentrated into the etching solution, while the iron is separated by precipitation. This solves the problems of acid etching solution regeneration and iron-copper separation, achieving efficient resource utilization and cost reduction.

CN123132885APending Publication Date: 2026-11-20CENTILLION ENVIRONMENT & RECYCLING (WUXI) CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611527473.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing acidic etching solution regeneration technology has failed to effectively solve the problem of insufficient copper content. In traditional processes, copper replenishment and regeneration are carried out independently, resulting in long process flow, high cost, and difficulty in achieving efficient iron-copper separation under mild conditions when treating iron-containing sponge copper.

Method used

Iron-containing sponge copper is mixed with acidic copper chloride etching waste liquid. Through displacement, complexation and oxidation reactions, copper is dissolved and concentrated into the etching solution. At the same time, iron oxidation precipitation separation is achieved under mild conditions. The multiple synergistic functions of sodium chlorate eliminate the need for additional copper or alkali.

Benefits of technology

This method enables the regeneration and copper enrichment of acidic etching waste liquid and the separation of iron and copper in iron-containing sponge copper. The copper concentration is increased and the iron content is reduced. The etching solution can be directly reused or used to prepare copper salts, thus realizing the value-added utilization of resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123132885A_ABST
    Figure CN123132885A_ABST
Patent Text Reader

Abstract

The application relates to a method for regenerating acid etching waste liquid, increasing copper and cooper-iron separation in iron-containing sponge copper, which comprises the following steps: firstly, mixing iron-containing sponge copper and acid copper chloride etching waste liquid to obtain first reaction liquid through first reaction; secondly, mixing hydrochloric acid and the first reaction liquid in step (1) to obtain second reaction liquid through second reaction; thirdly, mixing sodium chlorate and the second reaction liquid in step (2) to obtain acid copper chloride etching new liquid and Fe(OH)3 precipitate through third reaction and solid-liquid separation; the three functions of copper increase, regeneration and iron removal are realized; the total copper concentration in the obtained acid copper chloride etching new liquid is up to 150 g / L or more, the iron content is as low as 0.50 g / L or less, the obtained Fe(OH)3 product has high purity, the Fe2O3 dry basis content is up to 85 wt% or more, the low-grade iron-containing sponge copper is converted into high-copper etching new liquid, and the high-value Fe(OH)3 product is obtained, so that waste is treated by waste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of etching waste liquid regeneration technology, and in particular to a method for regenerating copper from acidic etching waste liquid and simultaneously separating iron and copper from iron-containing sponge copper, and more particularly to a method for regenerating copper from acidic copper chloride etching waste liquid and simultaneously separating iron and copper from iron-containing sponge copper. Background Technology

[0002] In the manufacturing process of printed circuit boards, acidic copper chloride etching solution (mainly composed of a CuCl2-HCl-NaCl system) is the most commonly used etching medium. During the etching process, Cu... 2+ Reduced to Cu + The etching ability gradually decreases, forming a mixture containing a large amount of Cu. + Etching waste liquid. Currently, acidic etching solution regeneration technologies mainly include: (1) Chemical oxidation regeneration method: adding oxidants such as sodium chlorate (NaClO3), hydrogen peroxide (H2O2) or oxygen to the etching waste liquid, and then using Cu + Oxidized to Cu 2+ (2) Electrolytic regeneration method: Cu is regenerated by electrolysis. + Oxidized to Cu 2+ However, existing regeneration technologies only restore the etching capacity of the etching solution and do not solve the problem of insufficient copper content in the etching solution. In actual production, as the etching process proceeds, the total amount of copper in the etching solution is continuously lost, requiring the addition of additional copper sources (such as copper chloride) to maintain the copper concentration, which increases production costs and raw material consumption.

[0003] For example, CN101532136A discloses an electrolytic regeneration method for acidic etching waste liquid. The method uses acidic etching waste liquid of copper chloride-hydrochloric acid system as anode liquid, adds inhibitor ammonium salt or organic amine, and uses acidic etching waste liquid with diluted copper mass concentration of 15-40 g / L as cathode liquid. The method performs DC electrolysis to obtain acidic etching regeneration liquid. However, although the method achieves the regeneration of acidic etching waste liquid to a certain extent, its copper concentration not only does not increase, but actually decreases.

[0004] Sponge copper is a common intermediate product in hydrometallurgical processes and waste liquid replacement and recycling. Its main component is elemental copper (Cu), but it usually contains a large amount of iron impurities (Fe content can reach 5%~20%). Due to the difficulty in separating iron and copper and its low grade, iron-containing sponge copper is traditionally processed by either being recycled or sold directly as a low-value product, resulting in low resource utilization and limited economic value.

[0005] In existing technologies, copper replenishment and regeneration in etching solutions are independent: in traditional processes, copper replenishment requires the separate purchase of copper sources such as copper chloride, while regeneration uses an oxidant alone, and the oxidant is only used to remove Cu. + Oxidized to Cu2+ The existing methods for treating sponge copper are limited in function and not fully utilized. The two processes are carried out in separate steps, resulting in a long and costly process flow. Current methods for treating sponge copper struggle to achieve efficient iron-copper separation under mild conditions, often requiring high-temperature smelting or multi-stage treatment with strong acids and alkalis. Traditional iron removal processes require the addition of alkali to adjust the pH, increasing reagent costs and wastewater generation.

[0006] Therefore, there is an urgent need in this field for a new method that can deeply couple the copper dissolution, iron separation and etching solution regeneration of iron-containing sponge copper to achieve integrated synergistic processing of "copper enhancement-regeneration-iron removal". Summary of the Invention

[0007] To address the aforementioned technical problems, this application provides a method for the regeneration and copper enrichment of acidic etching waste liquid, along with the separation of iron and copper in iron-containing sponge copper. This method efficiently dissolves and concentrates copper from iron-containing sponge copper into the acidic etching regeneration solution, and oxidizes and precipitates the iron in the iron-containing sponge copper in situ. No additional copper or alkali is required. Under mild conditions, this method achieves the regeneration and copper enrichment of acidic etching waste liquid and the efficient separation of iron and copper in iron-containing sponge copper.

[0008] To achieve this objective, the following technical solution is adopted in this application: This application provides a method for regenerating and adding copper from acidic etching waste liquid, and for separating iron and copper from iron-containing sponge copper. The method includes the following steps: (1) Mix iron-containing sponge copper and acidic copper chloride etching waste liquid, and obtain the first reaction solution through the first reaction; (2) Mix hydrochloric acid and the first reaction solution from step (1), and then react them to obtain the second reaction solution; (3) Mix sodium chlorate and the second reaction solution from step (2), and after a third reaction, separate the solid and liquid to obtain a new acidic copper chloride etching solution and Fe(OH)3 precipitate.

[0009] Specifically, in step (1), the first reaction includes a displacement reaction between the iron in the iron-containing sponge copper and the CuCl2 in the acidic copper chloride etching waste liquid, and a disproportionation reaction between the elemental copper in the iron-containing sponge copper and CuCl2 to generate cuprous chloride (CuCl) precipitate. The specific reaction equation is as follows: Reaction ① (displacement reaction): Fe + 2CuCl2 → FeCl2 + 2CuCl↓; Reaction ② (disproportionation reaction): Cu + CuCl₂ → 2CuCl↓; Step (2) provides sufficient Cl by hydrochloric acid - This causes the CuCl precipitate in the first reaction solution to undergo complexation and dissolution, transforming into a soluble cuprous complex [CuCl2]. - Meanwhile, the residual Fe in the sponge copper urgently needs to be dissolved by reacting with hydrochloric acid. The specific reaction equation is as follows: Reaction ③ (complex dissolution): CuCl(s) + Cl - →[CuCl2] - (Soluble); Reaction ④ (acid dissolution of residual iron): Fe + 2HCl → FeCl2 + H2↑; In step (3), sodium chlorate exhibits multiple synergistic oxidation functions. Furthermore, following the aforementioned multiple oxidation reactions, as hydrochloric acid is gradually consumed during the reaction, the pH of the system naturally increases. When the pH reaches a suitable range, the Fe in the system... 3+ A hydrolysis reaction occurs, and iron precipitates out as Fe(OH)3, thus achieving efficient removal of iron. The specific reaction equation is as follows: Reaction ⑤ (Oxidation of cuprous oxide, main reaction): 6[CuCl2] - +6HCl+NaClO3→6CuCl2+NaCl+3H2O+6Cl - ; Reaction ⑥ (Direct oxidation and dissolution of residual copper): 3Cu+6HCl+NaClO3→3CuCl2+NaCl+3H2O; Reaction ⑦ (oxidation of ferrous iron to ferric iron): 6FeCl2+6HCl+NaClO3→6FeCl3+NaCl+3H2O; Reaction ⑧ (precipitation of ferric iron): Fe 3+ +3H₂O→Fe(OH)₃↓+3H + .

[0010] The method described in this application utilizes iron-containing sponge copper to deeply couple the three independent processes of "copper enrichment, regeneration, and iron removal" into an integrated process. This synergistically achieves copper enrichment through the regeneration of acidic etching wastewater and iron-copper separation from the iron-containing sponge copper, yielding Cu. 2+ The new acidic copper chloride etching solution with increased concentration and reduced iron content can be directly reused or used to prepare copper salts. The Fe(OH)3 filter residue obtained can be used as a base material for preparing iron oxide red pigment after being washed with water until neutral.

[0011] The specific advantages of the method described in this application are as follows: (1) Multifunctional use of sodium chlorate with "one agent, three uses": Through pre-displacement neutralization and acid dissolution complexation reaction, external iron-containing sponge copper is introduced into the system, so that the function of NaClO3 can be transformed from the single "Cu" function of traditional etching solution regeneration. + →Cu 2+ The "oxidation" function has been expanded to include a triple synergistic function of "copper complex oxidation concentration, etching capability regeneration, and ferrous oxidation iron removal precursor", which greatly improves the utilization rate of oxidant. (2) Three-stage copper dissolution and concentration: "displacement-neutralization-complexation" is used to uniformly convert copper of different forms (elemental copper and copper displaced by iron) in iron-containing sponge copper into soluble cuprous complex, and then oxidize it into CuCl2 to achieve complete copper dissolution and significantly increase the copper concentration of the etching solution. (3) Zero-addition alkali removal with pH self-regulation: The pH of the system is spontaneously increased by utilizing the natural consumption of hydrochloric acid in each stage of the reaction, without the need for additional alkali solution to remove Fe. 3+ Hydrolysis produces Fe(OH)3 precipitate, which ultimately reduces the iron content in the etching solution, and also reduces reagent costs and wastewater generation; (4) Efficient separation and high-value utilization of copper and iron in iron-containing sponge copper: Based on the synergistic effect of pH self-regulation, copper is separated into Cu 2+ The iron is retained in the solution and precipitated as Fe(OH)3, realizing the transformation of low-grade iron-containing sponge copper into high-copper etching solution raw material, achieving the resource value-added utilization of "waste treatment".

[0012] The specific uses of the acidic copper chloride etching solution obtained in this application are as follows: ①Direct reuse: Based on the required ratio of etching solution, various additives are added quantitatively without the need to add copper source, so that the etching ability can be restored and returned to the PCB etching process; ② Preparation of copper salts: Using acidic copper chloride etching solution as raw material, copper salt products such as basic copper carbonate, copper chloride or copper sulfate are prepared. Due to the increase in copper concentration, the product output per unit volume of etching solution increases significantly.

[0013] In some technical solutions of this application, the acidic copper chloride etching waste liquid in step (1) comprises 120~135g / L Cu 2+ 10~30g / L Cu + And 0.8~1.5 mol / L free HCl.

[0014] Among them, 120~135g / L Cu 2+ For example, it could be 120g / L, 122g / L, 125g / L, 128g / L, 130g / L, 132g / L, or 135g / L, etc.; 10~30g / L Cu + For example, it can be 10 g / L, 12 g / L, 15 g / L, 18 g / L, 20 g / L, 22 g / L, 25 g / L, 28 g / L or 30 g / L, etc.; 0.8~1.5 mol / L free HCl, for example, it can be 0.8 mol / L, 0.9 mol / L, 1.0 mol / L, 1.1 mol / L, 1.2 mol / L or 1.5 mol / L, etc.

[0015] In some technical solutions of this application, based on the total mass of the iron-containing sponge copper being 100wt%, the iron-containing sponge copper in step (1) includes 60~90wt% Cu and 5~20wt% Fe.

[0016] Among them, 60~90wt%Cu, for example, can be 60wt%, 65wt%, 70wt%, 75wt%, 80wt%, 85wt%, or 90wt%; 5~20wt%Fe, for example, can be 5wt%, 8wt%, 10wt%, 12wt%, 15wt%, 18wt%, or 20wt%;

[0017] In some technical solutions of this application, the amount of iron-containing sponge copper added in step (1) is 8 to 20% of the total mass of the acidic copper chloride etching waste liquid, for example, it can be 8%, 10%, 12%, 15%, 18% or 20%, etc.

[0018] The amount of iron-containing sponge copper added in step (1) of the method described in this application is within the above range, specifically added according to the acidic etching waste liquid and the copper content in the iron-containing sponge copper, so that the total amount of copper ions in the system after the reaction does not exceed the solubility of copper chloride at the corresponding system temperature.

[0019] If the amount of iron-containing sponge copper added is too small, the introduced copper source will be insufficient, resulting in a small amount of CuCl precipitate generated in the neutralization reaction. Consequently, the amount of CuCl entering the liquid phase after subsequent sodium chlorate oxidation will be insufficient. 2+ The incremental increase was limited, and the total copper concentration did not improve significantly; meanwhile, Fe in the system 2+ and Cu + The total amount is too low, resulting in less HCl consumption during the oxidation stage and insufficient natural pH increase. The final pH may be below 2, leading to Fe... 3+ Incomplete hydrolysis and precipitation resulted in poor iron removal. Furthermore, the triple synergistic function of sodium chlorate—"cuprous oxidation concentration - etching regeneration - ferrous oxidation iron removal"—could not be fully utilized.

[0020] If the amount of iron-containing sponge copper added is too high, the excess Fe will preferentially react with Cu. 2+ It reacts with HCl, consuming large amounts of hydrochloric acid and sodium chlorate, and is used to oxidize Cu. + Insufficient oxidant, resulting in Cu + Incomplete oxidation and endpoint residues can occur. Furthermore, the total copper content may exceed the solubility of copper chloride at the system temperature, leading to the crystallization and precipitation of CuCl2 or CuCl. This not only fails to concentrate the copper but also causes copper loss and makes filtration difficult. More importantly, excess Fe, after oxidation, generates a large amount of Fe(OH)3 colloid, which adsorbs and carries away Cu. 2+ This reduces copper recovery and leads to a sharp deterioration in filtration performance; in addition, excessive iron consumption of hydrochloric acid may cause the endpoint pH to deviate from the suitable range, affecting the copper-iron separation effect.

[0021] In some technical solutions of this application, the first reaction is accompanied by a first stirring.

[0022] In some technical solutions of this application, the rotation speed of the first stirring is 200~400 r / min, for example, it can be 200 r / min, 250 r / min, 300 r / min, 350 r / min or 400 r / min, etc.

[0023] In some technical solutions of this application, the time of the first reaction is 20 to 60 minutes, for example, it can be 20 minutes, 30 minutes, 40 minutes, 50 minutes or 60 minutes.

[0024] In some technical solutions of this application, the temperature of the first reaction solution is 45~50℃, for example, it can be 45℃, 46℃, 47℃, 48℃, 49℃ or 50℃, etc.

[0025] In this application, no additional heating is required during the first reaction process; the exothermic reaction causes the system to naturally heat up to 45-50°C.

[0026] In some technical solutions of this application, the form in which Cu exists in the first reaction solution includes CuCl precipitate.

[0027] In some technical solutions of this application, the concentration of hydrochloric acid in step (2) is 6~12 mol / L, for example, it can be 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L or 12 mol / L, etc.

[0028] In some technical solutions of this application, the amount of hydrochloric acid added in step (2) is such that the concentration of free HCl in the first reaction solution is 1.5~2.5 mol / L, for example, it can be 1.5 mol / L, 1.8 mol / L, 2.0 mol / L, 2.2 mol / L or 2.5 mol / L, etc.

[0029] In the method described in this application, the amount of hydrochloric acid added in step (2) is such that the concentration of free HCl in the first reaction solution is 1.5~2.5 mol / L; if the amount of hydrochloric acid added is too small, the concentration of free HCl in the first reaction solution will be too low, which will in turn lead to Cl - Insufficient concentration prevents the generated CuCl precipitate from being completely complexed and dissolved into soluble [CuCl2]. - Copper remains in the solid phase as CuCl precipitate and cannot enter the liquid phase to participate in subsequent oxidation and concentration. If too much hydrochloric acid is added, the concentration of free HCl in the first reaction solution will be too high, leading to a large amount of H₂ in the system.+ This hindered the natural pH rise during the NaClO3 oxidation reaction, preventing the final pH from reaching above 2.0. (Fe) 3+ It cannot be hydrolyzed and precipitated.

[0030] In some technical solutions of this application, step (2) of the second reaction process is accompanied by a second stirring.

[0031] In some technical solutions of this application, the rotation speed of the second stirring is 200~400 r / min, for example, it can be 200 r / min, 250 r / min, 300 r / min, 350 r / min or 400 r / min, etc.

[0032] In some technical solutions of this application, the temperature of the second reaction in step (2) is 30~60℃, for example, it can be 30℃, 35℃, 40℃, 45℃, 50℃, 55℃ or 60℃, for example, it can also be 40~55℃.

[0033] In some technical solutions of this application, the time for the second reaction in step (2) is 20~60min, for example, it can be 20min, 30min, 40min, 50min or 60min, for example, it can also be 30~45min.

[0034] In some technical solutions of this application, the form in which Cu exists in the second reaction solution in step (2) includes [CuCl2]. - .

[0035] In some technical solutions of this application, the amount of sodium chlorate added in step (3) is the same as the amount of [CuCl2] in the second reaction solution in step (2). - and Fe 2+ The total oxygen demand is 1.05 to 1.2 times the theoretical oxygen requirement for total oxidation, for example, it can be 1.05 times, 1.08 times, 1.1 times, 1.12 times, 1.15 times, 1.18 times or 1.2 times, etc.

[0036] In step (3) of the method described in this application, the monovalent copper (Cu) in the reaction system is sampled and detected. + ) and divalent iron (Fe) 2+ Stop adding the drug when none of the above are detected.

[0037] In the method described in this application, the amount of sodium chlorate added in step (3) is the same as the amount of [CuCl2] in the second reaction solution in step (2). - and Fe 2+ The total oxygen demand for oxidation is 1.05 to 1.2 times the theoretical oxygen requirement, ensuring [CuCl2]... - and Fe 2+Sufficient oxidation is required to reduce the Cu content in the resulting acidic copper chloride etching solution. + and Fe 2+ Residue, improve recycling capacity; if the amount of sodium chlorate added in step (3) is too small, it will lead to Cu in the system + and Fe 2+ Incomplete oxidation, low endpoint pH, Fe 3+ The precipitate cannot be fully generated and hydrolyzed, and the copper and iron levels in the new acidic copper chloride etching solution are both unqualified; if the amount of sodium chlorate added in step (3) is too high, it will cause the excess sodium chlorate to react with Cl in the system under acidic conditions. - A side reaction occurs, producing toxic chlorine gas (Cl2), while simultaneously consuming excessive amounts of hydrochloric acid and lowering the Cl2 level. - Concentration, causing an abnormal increase in the system's pH and potentially leading to Cu 2+ Hydrolysis and precipitation ultimately worsen the operating environment, reduce copper recovery rates, and compromise the quality of the new etching solution.

[0038] In some technical solutions of this application, the sodium chlorate addition method in step (3) includes batch addition, and the time interval between two adjacent batches is 10~15min, for example, it can be 10min, 11min, 12min, 13min, 14min or 15min, etc.

[0039] In some technical solutions of this application, the temperature of the third reaction in step (3) is 50~90℃, for example, it can be 50℃, 60℃, 70℃, 80℃ or 90℃, for example, it can also be 70~80℃.

[0040] In some technical solutions of this application, the time of the third reaction in step (3) is 60~180min, for example, it can be 60min, 80min, 100min, 120min, 140min, 160min or 180min, etc., and it can also be 90~120min.

[0041] In some technical solutions of this application, the final pH of the third reaction solution after the third reaction in step (3) is 2~3, for example, it can be 2, 2.2, 2.5, 2.8 or 3, etc.

[0042] The final pH of the third reaction solution after the third reaction in step (3) of the method described in this application is 2~3. This pH value is spontaneously formed by the natural consumption of hydrochloric acid during the oxidation of sodium chlorate, without the need for external alkali adjustment.

[0043] In some technical solutions of this application, the method further includes aging the third reaction solution after the third reaction in step (3).

[0044] In some technical solutions of this application, the aging treatment temperature is 70~85℃, for example, it can be 70℃, 75℃, 80℃ or 85℃, etc.

[0045] In some technical solutions of this application, the aging treatment time is 40~120min, for example, it can be 40min, 50min, 60min, 70min, 80min, 90min, 100min, 110min or 120min.

[0046] In some technical solutions of this application, the total copper concentration in the acidic copper chloride etching solution in step (3) is ≥170g / L, for example, it can be 170g / L, 180g / L, 190g / L, 200g / L or 210g / L, etc.

[0047] In some technical solutions of this application, the iron content in the acidic copper chloride etching solution in step (3) is ≤0.1g / L, for example, it can be 0.1g / L, 0.09g / L, 0.08g / L, 0.07g / L, 0.06g / L or 0.05g / L, etc.

[0048] In some technical solutions of this application, the Fe2O3 dry basis content in the Fe(OH)3 precipitate in step (3) is ≥94wt%, for example, it can be 94wt%, 94.5wt%, 95wt%, 95.5wt%, 96wt%, 96.5wt% or 97wt%, etc.

[0049] Compared with the prior art, this application has at least the following beneficial effects: The method provided in this application for the regeneration and copper enrichment of acidic etching waste liquid in conjunction with the separation of iron and copper in iron-containing sponge copper utilizes iron-containing sponge copper to regenerate and enrich the copper in acidic copper chloride etching waste liquid, which can be directly reused without additional copper replenishment. At the same time, it achieves efficient separation of iron and copper in iron-containing sponge copper without the need for additional alkali addition. The resulting acidic copper chloride etching solution has a total copper concentration of over 150 g / L and an iron content as low as below 0.50 g / L. The resulting ferric hydroxide precipitate has high purity, and after washing with water to neutrality, the Fe2O3 dry basis content is over 85 wt%. This method realizes the transformation of low-grade iron-containing sponge copper into high-copper etching solution, achieving the added value utilization effect of treating waste with waste. Attached Figure Description

[0050] Figure 1 This is a process flow diagram of the method for treating acidic copper chloride etching waste liquid using iron-containing sponge copper provided in Embodiment 1 of this application. Detailed Implementation

[0051] The technical solution of this application will be further described below with reference to the accompanying drawings and specific embodiments. However, the examples below are merely simplified examples of this application and do not represent or limit the scope of protection of this application. The scope of protection of this application shall be determined by the claims.

[0052] In some implementations, step (1) of the first reaction includes: Reaction ① (displacement reaction): Fe + 2CuCl2 → FeCl2 + 2CuCl↓; Reaction ② (disproportionation reaction): Cu + CuCl₂ → 2CuCl↓; Step (2) The second reaction includes: Reaction ③ (complex dissolution): CuCl(s) + Cl - →[CuCl2] - (Soluble); Reaction ④ (acid dissolution of residual iron): Fe + 2HCl → FeCl2 + H2↑; The third reaction described in step (3): Reaction ⑤ (Oxidation of cuprous oxide, main reaction): 6[CuCl2] - +6HCl+NaClO3→6CuCl2+NaCl+3H2O+6Cl - ; Reaction ⑥ (Direct oxidation and dissolution of residual copper): 3Cu+6HCl+NaClO3→3CuCl2+NaCl+3H2O; Reaction ⑦ (oxidation of ferrous iron to ferric iron): 6FeCl2+6HCl+NaClO3→6FeCl3+NaCl+3H2O; Reaction ⑧ (precipitation of ferric iron): Fe 3+ +3H₂O→Fe(OH)₃↓+3H + .

[0053] I. Implementation Examples Example 1 This embodiment provides a method for regenerating and increasing copper content in acidic copper chloride etching waste liquid, along with the separation of iron and copper from iron-containing sponge copper. According to... Figure 1 The process flow shown is as follows, and the acidic copper chloride etching waste liquid includes 130 g / L Cu 2+ 20g / L Cu + 1.2 mol / L free HCl; the iron-containing sponge copper comprises 78 wt% Cu, 17 wt% Fe and 5 wt% H2O; The method includes the following steps: (1) The amount of iron-containing sponge copper added is 10% of the total mass of the acidic copper chloride etching waste liquid. The iron-containing sponge copper and the acidic copper chloride etching waste liquid are mixed and reacted for 40 min under stirring conditions of 200 r / min to obtain a first reaction solution containing CuCl precipitate. (2) Mix hydrochloric acid (6 mol / L) and the first reaction solution from step (1) until the concentration of free HCl in the first reaction solution is 1.8 mol / L, and then carry out a second reaction for 35 min at 45℃ and 200 r / min to obtain [CuCl2]. - and Fe 2+ The second reaction solution; (3) The [CuCl2] in the second reaction solution from step (2) - and Fe 2+ Sodium chlorate was added in batches (6 batches) to the second reaction solution in step (2) at 1.1 times the theoretical oxygen requirement for total oxidation. The amount added in each batch was the same, and the time interval between two adjacent batches was 12 min. The third reaction was carried out at 75°C for 120 min. The pH at the end of the reaction was 2.2. The reaction system was then aged at 70°C for 45 min. After filtration, acidic copper chloride etching solution and filter mud were obtained. The filter mud was washed with water to obtain Fe(OH)3 precipitate. The wash water was returned to the acidic copper chloride etching solution.

[0054] Example 2 This embodiment provides a method for regenerating and increasing copper content in acidic copper chloride etching waste liquid, along with the separation of iron and copper from iron-containing sponge copper. The acidic copper chloride etching waste liquid contains 120 g / L Cu 2+ 30g / L Cu + 0.8 mol / L free HCl; the iron-containing sponge copper comprises 79 wt% Cu, 18 wt% Fe and 3 wt% H2O; The method includes the following steps: (1) The iron-containing sponge copper is added at a ratio of 13% of the total mass of the acidic copper chloride etching waste liquid. The iron-containing sponge copper and the acidic copper chloride etching waste liquid are mixed and reacted for 30 min under stirring conditions of 300 r / min to obtain a first reaction solution containing CuCl precipitate. (2) Mix hydrochloric acid (12 mol / L) and the first reaction solution from step (1) until the concentration of free HCl in the first reaction solution is 2.2 mol / L, and then carry out a second reaction for 20 min at 60℃ and 300 r / min to obtain [CuCl2]. - and Fe 2+ The second reaction solution; (3) The [CuCl2] in the second reaction solution from step (2)- and Fe 2+ Sodium chlorate was added in batches (4 batches) to the second reaction solution in step (2) at 1.05 times the theoretical oxygen requirement for total oxidation. The amount added in each batch was the same, and the time interval between two adjacent batches was 15 min. The third reaction was carried out at 90℃ for 60 min. The pH at the end of the reaction was 2.4. The reaction system was then aged at 80℃ for 40 min. After that, the acidic copper chloride etching solution and filter mud were obtained by filtration. The filter mud was washed with water to obtain Fe(OH)3 precipitate. The wash water was returned to the acidic copper chloride etching solution.

[0055] Example 3 This embodiment provides a method for regenerating and increasing copper content in acidic copper chloride etching waste liquid, along with the separation of iron and copper from iron-containing sponge copper. The acidic copper chloride etching waste liquid contains 135 g / L Cu. 2+ 10g / L Cu + 1.5 mol / L free HCl; the iron-containing sponge copper comprises 85 wt% Cu, 9 wt% Fe and 6 wt% H2O; The method includes the following steps: (1) The iron-containing sponge copper was added at a ratio of 8% of the total mass of the acidic copper chloride etching waste liquid. The iron-containing sponge copper and the acidic copper chloride etching waste liquid were mixed and reacted for 20 minutes under stirring at 400 r / min to obtain a first reaction solution containing CuCl precipitate. (2) Mix hydrochloric acid (10 mol / L) and the first reaction solution from step (1) until the concentration of free HCl in the first reaction solution is 2.0 mol / L, and then carry out a second reaction for 35 min at 55℃ and 380 r / min to obtain [CuCl2]. - and Fe 2+ The second reaction solution; (3) The [CuCl2] in the second reaction solution from step (2) - and Fe 2+ Sodium chlorate was added in batches (4 batches) to the second reaction solution in step (2) at 1.2 times the theoretical oxygen requirement for total oxidation. The amount added in each batch was the same, and the time interval between two adjacent batches was 10 min. The third reaction was carried out at 50°C for 180 min. The pH at the end of the reaction was 2.2. The reaction system was then aged at 75°C for 50 min. After filtration, acidic copper chloride etching solution filter mud was obtained. The filter mud was washed with water to obtain Fe(OH)3 precipitate. The wash water was returned to the acidic copper chloride etching solution.

[0056] Example 4 This embodiment provides a method for regenerating copper from acidic copper chloride etching waste liquid and separating iron and copper from iron-containing sponge copper. Except for step (1), in which the amount of iron-containing sponge copper added is 6% of the total mass of the acidic copper chloride etching waste liquid, the method is the same as in embodiment 1.

[0057] Example 5 This embodiment provides a method for regenerating copper from acidic copper chloride etching waste liquid and separating iron and copper from iron-containing sponge copper. Except for step (1), in which the amount of iron-containing sponge copper added is 22% of the total mass of the acidic copper chloride etching waste liquid, the method is the same as in embodiment 1.

[0058] Example 6 This embodiment provides a method for regenerating copper from acidic copper chloride etching waste liquid and separating iron and copper from iron-containing sponge copper. Except for step (2), in which the amount of hydrochloric acid added is such that the concentration of free HCl in the first reaction solution is 1.3 mol / L, the method is the same as in Example 1.

[0059] Example 7 This embodiment provides a method for regenerating copper from acidic copper chloride etching waste liquid and separating iron and copper from iron-containing sponge copper. Except for step (2), in which the amount of hydrochloric acid added is such that the concentration of free HCl in the first reaction solution is 3.0 mol / L, the method is the same as in Example 1.

[0060] Example 8 This embodiment provides a method for regenerating and increasing copper content in acidic copper chloride etching waste liquid, along with the separation of iron and copper from iron-containing sponge copper. The method, except that the amount of sodium chlorate added in step (3) is the same as the amount of [CuCl2] in the second reaction solution in step (2), is... - and Fe 2+ Except for the requirement of 0.9 times the theoretical oxygen demand for total oxidation, everything else is the same as in Example 1.

[0061] Example 9 This embodiment provides a method for regenerating and increasing copper content in acidic copper chloride etching waste liquid, along with the separation of iron and copper from iron-containing sponge copper. The method, except that the amount of sodium chlorate added in step (3) is the same as the amount of [CuCl2] in the second reaction solution in step (2), is... - and Fe 2+ Except for the requirement of 1.3 times the theoretical oxygen demand for total oxidation, everything else is the same as in Example 1.

[0062] II. Comparative Example Comparative Example 1 This comparative example provides a method for treating acidic copper chloride etching waste liquid. The method is the same as in Example 1, except that the iron-containing sponge copper in step (1) is replaced with reduced iron powder.

[0063] Comparative Example 2 This comparative example provides a method for treating acidic copper chloride etching waste liquid. The method employs a conventional iron powder replacement method to treat the same batch of acidic copper chloride etching waste liquid (130 g / L Cu) as in Example 1. 2+ 20g / L Cu + 1.2 mol / L free HCl), and reduced iron powder was directly added to the etching waste liquid at a stoichiometric ratio of 1.1. The iron powder will cause Cu 2+ All of the copper was replaced by sponge copper precipitate, and after filtration, sponge copper and a high Fe content were obtained. 2+ The reaction was carried out with a 24 g / L ferrous chloride solution at a temperature of 50°C for 60 min.

[0064] The method described in this comparative example has the following drawbacks: It consumes a large amount of iron powder, requiring 2.45 kg of iron powder to treat 100 kg of acidic etching waste liquid (the amount of iron consumed when the original copper concentration is 130 g / L); the copper in the acidic copper chloride etching waste liquid is completely extracted, rendering the etching solution unusable and unable to achieve concentration recycling; and it generates a large amount of Fe-containing waste liquid. 2+ The solution requires additional oxidation and alkali precipitation before it can be discharged, making the process lengthy; when there is an excess of iron powder, the purity of the sponge copper decreases, affecting its subsequent use.

[0065] Comparative Example 3 This comparative example provides a method for treating acidic copper chloride etching waste liquid. The method employs a two-step process of iron powder replacement followed by electrolytic regeneration to treat the same batch of acidic copper chloride etching waste liquid (130 g / L Cu) as in Example 1. 2+ 20g / L Cu + (1.2 mol / L free HCl); the specific steps are as follows: (1) Iron powder replacement: Following the method described in Comparative Example 2, reduced iron powder was directly added to the etching waste liquid at a stoichiometric ratio of 1.1. The reaction was carried out at 50°C with stirring for 60 minutes. The iron powder replaced Cu. 2+ All of the precipitate was replaced by sponge copper; after the reaction was complete, the mixture was filtered to obtain sponge copper and ferrous chloride solution. The ferrous chloride solution contained Fe... 2+ The concentration is 24 g / L, Cu 2+ Concentration <0.05 g / L, free HCl is 0.2 mol / L; (2) Electrolytic oxidation: The above ferrous chloride solution is pumped into the anode chamber of a two-chamber electrolytic cell. The anode is a titanium-based lead dioxide (Ti / PbO2) electrode, and the cathode is a stainless steel plate. The anode chamber and the cathode chamber are separated by a cation exchange membrane. 0.5 mol / L dilute hydrochloric acid is added to the cathode chamber as the catholyte. The anode current density is controlled at 250 A / m. 2The cell voltage was 3.2V, the electrolysis temperature was 50℃, and the electrolysis time was 4 hours, during which the solution in the anode chamber circulated. During electrolysis, the anode will convert Fe... 2+ Oxidized to Fe 3 + A small amount of copper is deposited at the cathode, producing hydrogen gas. Samples are taken and analyzed using potassium dichromate titration. When Fe in the anolyte... 2+ Electrolysis is stopped when the oxidation rate is ≥95%. The anolyte is a ferric chloride solution, which can be used directly as a water treatment agent, or precipitated with alkali to prepare ferric hydroxide; the small amount of copper deposited at the cathode is recovered separately.

[0066] The method described in this comparative example has the following drawbacks: the process requires three steps (replacement, filtration, and electrolysis or oxidation), the equipment investment is large, requiring a replacement reactor, a filter press, and an electrolytic cell or oxidation tower; the electrolysis energy consumption is high, about 3 kWh / kg Cu, and the total copper yield is 95% (there are losses during the electrolysis process); the etching solution cannot be reused.

[0067] III. Tests and Results The total copper concentration and iron content in the acidic copper chloride etching solution obtained in the above examples or Comparative Example 1 were measured, and the Fe2O3 dry basis content in the Fe(OH)3 precipitate was tested. The results are shown in Table 1. Table 1 Where "-" indicates that there is no relevant data; The test results show that: (1) As can be seen from Examples 1 to 3, the method of regenerating copper in acidic etching waste liquid and separating iron from copper in iron-containing sponge copper provided in this application simultaneously achieves the effects of increasing copper, regeneration and iron separation. The total copper concentration in the new acidic copper chloride etching solution is as high as 170 g / L or more, and the iron content is as low as 0.08 g / L or less. Moreover, the Fe(OH)3 precipitate has high purity and the Fe2O3 dry basis content is as high as 94 wt% or more. That is, this application utilizes the efficient dissolution and concentration of copper in iron-containing sponge copper into the etching solution, and the iron is simultaneously oxidized and precipitated to separate, thus achieving the triple synergistic effect of "increasing copper-regeneration-removing iron".

[0068] (2) As can be seen from Examples 1 and 4 to 9, in the method described in this application, the amount of iron-containing sponge copper added in step (1) is 8-20% of the total mass of the acidic copper chloride etching waste liquid; the amount of hydrochloric acid added in step (2) is such that the concentration of free HCl in the first reaction solution is 1.5-2.5 mol / L; and the amount of sodium chlorate added in step (3) is such that the concentration of [CuCl2] in the second reaction solution in step (2) is... - and Fe 2+The total oxygen demand for oxidation is 1.05 to 1.2 times the theoretical oxygen requirement. The combined effect of these three factors improves the separation of copper and iron. Specifically: In Example 4, the dosage of iron-containing sponge copper (6%) was too low, resulting in only 155 g / L of total copper and 0.15 g / L of iron, leading to insufficient copper addition and incomplete iron removal; In Example 5, the dosage of iron-containing sponge copper (22%) was too high, resulting in 185 g / L of total copper, but the iron content increased to 0.20 g / L, and the Fe2O3 purity decreased to 92 wt%, indicating that excessive iron consumed the oxidant and caused copper loss; In Example 6, the amount of hydrochloric acid added was too low, resulting in a low level of free HCl (1.3 mol / L), leading to only 150 g / L of total copper and 0.50 g / L of iron, due to the low concentration of Cl... - Insufficient amounts of hydrochloric acid resulted in incomplete dissolution of the CuCl complex; the amount of hydrochloric acid added in Example 7 was too low, leading to a high level of free HCl (3.0 mol / L). Although the total copper content reached 190 g / L, the iron content was as high as 0.50 g / L, and the Fe2O3 purity was only 85 wt%. The excessively high acidity inhibited the natural pH rise, resulting in Fe... 3+ Unable to hydrolyze and precipitate; the amount of sodium chlorate added in Example 8 was too low (0.9 times the theoretical oxygen demand), resulting in a total copper concentration of 170 g / L, but Cu... + There were residual iron residues, with an iron content reaching 0.30 g / L, indicating incomplete oxidation. In Example 9, the amount of sodium chlorate added was too high (1.3 times the theoretical oxygen requirement), resulting in a decrease in total copper to 175 g / L, an increase in iron content to 0.10 g / L, and a decrease in Fe2O3 purity to 91 wt%. This was due to a side reaction between excess sodium chlorate and hydrochloric acid, leading to partial hydrolysis loss of copper and a decrease in the purity of the iron slag. The above examples fully demonstrate the critical significance and synergistic necessity of each parameter range.

[0069] (3) As can be seen from Example 1 and Comparative Examples 1 to 3, since the reduction iron powder replacement was directly used in Comparative Example 1, the total copper concentration in the resulting acidic etching solution was only 120 g / L, the iron content was as high as 5 g / L, and the Fe2O3 dry basis content was only 80 wt%, which could not achieve copper enrichment or iron separation. Since the iron powder replacement method or the two-step method of iron powder replacement plus electrolytic regeneration was used in Comparative Examples 2 and 3, the copper in the etching solution was completely extracted, the etching solution lost its ability to be reused, and it could not achieve enrichment and recycling. In addition, there were defects such as large iron powder consumption, high electrolytic energy consumption, and large equipment investment.

[0070] In summary, the method for regenerating copper from acidic etching waste liquid and separating iron and copper in iron-containing sponge copper provided in this application utilizes a dual reduction pathway of Fe and Cu in iron-containing sponge copper to achieve Cu... 2+ Converted to Cu + At the same time, it does not destroy the recycling potential of the etching solution, and the Fe is subsequently precipitated through NaClO3 oxidation-spontaneous hydrolysis. 3+In-situ removal, a three-step coupling process that completes copper regeneration and concentration and iron separation in one step, with highly integrated processes; moreover, this application sequentially completes displacement / neutralization, complexation dissolution, oxidation, and hydrolysis precipitation within the same reaction system, requiring only a single reactor and filter press, with no electrolytic energy consumption, and copper is converted into Cu... 2+ The copper is retained in the liquid phase for direct enrichment and reuse, with a total copper yield of over 99%. This application has significant advantages in four dimensions: process steps, equipment investment, energy consumption, and etching solution reuse capability.

[0071] The applicant declares that the above description is only a specific implementation of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. A method for regenerating and increasing copper content in acidic etching waste liquid, combined with the separation of iron and copper from iron-containing sponge copper, characterized in that, The method includes the following steps: (1) Mix iron-containing sponge copper and acidic copper chloride etching waste liquid, and obtain the first reaction solution through the first reaction; (2) Mix hydrochloric acid and the first reaction solution from step (1), and then react them to obtain the second reaction solution; (3) Mix sodium chlorate and the second reaction solution from step (2), and after a third reaction, separate the solid and liquid to obtain a new acidic copper chloride etching solution and Fe(OH)3 precipitate.

2. The method according to claim 1, characterized in that, The acidic copper chloride etching waste liquid in step (1) includes 120~135g / L Cu 2+ 10~30g / L Cu + And 0.8~1.5 mol / L free HCl.

3. The method according to claim 1 or 2, characterized in that, Based on a total mass of 100wt% of the iron-containing sponge copper, the iron-containing sponge copper in step (1) includes 60-90wt% Cu and 5-20wt% Fe; And / or, the amount of iron-containing sponge copper added in step (1) is 8 to 20% of the total mass of the acidic copper chloride etching waste liquid.

4. The method according to any one of claims 1 to 3, characterized in that, The first reaction is accompanied by the first stirring. And / or, the time for the first reaction is 20 to 60 minutes; And / or, the temperature of the first reaction solution is 45~50℃; And / or, the presence of Cu in the first reaction solution may include CuCl precipitate.

5. The method according to any one of claims 1 to 4, characterized in that, The concentration of hydrochloric acid in step (2) is 6~12 mol / L; And / or, the amount of hydrochloric acid added in step (2) is such that the concentration of free HCl in the first reaction solution is 1.5~2.5 mol / L.

6. The method according to any one of claims 1 to 5, characterized in that, Step (2) The second reaction process is accompanied by a second stirring; And / or, in step (2), the temperature of the second reaction is 30~60℃; And / or, the reaction time in step (2) is 20~60 min; And / or, in step (2), the form in which Cu exists in the second reaction solution includes [CuCl2]. - .

7. The method according to any one of claims 1 to 6, characterized in that, The amount of sodium chlorate added in step (3) is the same as the amount of [CuCl2] in the second reaction solution in step (2). - and Fe 2+ The total oxygen demand for oxidation is 1.05 to 1.2 times the theoretical oxygen requirement. And / or, the sodium chlorate addition method in step (3) includes batch addition, and the time interval between two adjacent batches is 10~15min; And / or, the temperature of the third reaction in step (3) is 50~90℃; And / or, the time for the third reaction in step (3) is 60~180 min.

8. The method according to any one of claims 1 to 7, characterized in that, The final pH of the third reaction solution after the third reaction in step (3) is 2~3; And / or, the method further includes aging the third reaction solution after the third reaction in step (3).

9. The method according to claim 8, characterized in that, The aging process is carried out at a temperature of 70~85℃; And / or, the aging process takes 40 to 120 minutes.

10. The method according to any one of claims 1 to 9, characterized in that, The total copper concentration in the acidic copper chloride etching solution in step (3) is ≥170 g / L; And / or, the iron content in the acidic copper chloride etching solution in step (3) is ≤0.1g / L; And / or, the Fe2O3 dry basis content in the Fe(OH)3 precipitate in step (3) is ≥94wt%.

Citation Information

Patent Citations

  • Electrolytic regeneration method of acidic etching waste solution

    CN101532136A