A low-scratch polishing liquid for red copper parts and a preparation process thereof

By combining modified coated gradient abrasives with friction-triggered polishing slurries, the problems of global corrosion, micro-scratches, and slurry aging in copper polishing have been solved, achieving efficient dimensional control and long-life polishing slurry application.

CN123132886APending Publication Date: 2026-11-20HUZHOU JINYUAN GRINDING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611123306.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-28
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing copper polishing slurries suffer from problems such as global corrosion leading to tolerance exceeding limits, failure of dynamic corrosion inhibition, micro-scratches caused by bare abrasive grinding, and accelerated aging of the slurry by free copper ions.

Method used

A modified coated gradient abrasive system, a friction-triggered polishing and corrosion inhibition system, and a lubricating chelating dispersion system were used to construct a friction field-responsive point polishing system. The lactone precursor was hydrolyzed at the local stress point, the double-layer self-healing corrosion inhibitor repaired in situ when friction damage occurred, and the multi-toothed chelating agent captured free copper ions to form a stable suspended network structure.

Benefits of technology

It achieves zero etching in non-friction areas, eliminates micro-scratches and grain boundary tears, ensures extremely low dimensional tolerances, provides excellent dynamic corrosion protection, extends solution life, and meets the needs of long-term cyclic mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123132886A_ABST
    Figure CN123132886A_ABST
Patent Text Reader

Abstract

The application discloses a low-scratch polishing liquid for red copper parts and a preparation process thereof, and belongs to the technical field of metal surface polishing. The polishing liquid comprises, in percentage by weight, 12.0-22.0% of a modified coated abrasive system, 2.5-7.5% of a friction-triggered polishing and corrosion inhibition system, 2.0-4.5% of a lubricating chelating dispersion system, an appropriate amount of a pH regulator (adjusting the initial pH to 6.8-7.2), and the balance of deionized water. The friction-triggered polishing and corrosion inhibition system comprises lactone precursors (such as gluconolactone, caprolactone, butyrolactone, etc.), heterocyclic corrosion inhibitors and long-chain flexible corrosion inhibitors. The application realizes stress-free rolling grinding through the heterocharge coated abrasive, realizes fixed-point polishing and double-layer self-repairing corrosion inhibition by combining the friction force to trigger lactone hydrolysis, ensures the size accuracy of the red copper thin-walled part, completely eliminates microscopic scratches, and significantly prolongs the service life of the polishing liquid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal surface polishing technology, and in particular to a low-scratch polishing fluid for copper parts and its preparation process. Background Technology

[0002] Due to its excellent electrical conductivity, thermal conductivity, and ductility, copper is widely used in high-end manufacturing fields such as precision electronic components, micro-structural parts, and thin-walled tubes. In order to meet the requirements of subsequent electroplating, spraying, or assembly, the surface of copper parts must have extremely high flatness and gloss, and there must be no micro-scratches or oxidation blackening. Therefore, the performance of the grinding and polishing slurry directly determines the processing yield of the final product.

[0003] In the prior art, polishing slurries that combine chemical corrosion with mechanical friction are commonly used. For example, Chinese authorized invention patent CN103757636B discloses a chemical polishing slurry, which is mainly composed of corrosive oxidizing substances such as sulfuric acid, hydrogen peroxide, and acetic acid, combined with conventional corrosion inhibitors such as benzotriazole. Such conventional solutions attempt to achieve a bright finish on the surface of copper parts by using acidic substances to etch the entire surface of the copper parts in combination with static anti-corrosion components.

[0004] However, the aforementioned existing technologies have the following inherent defects in practical applications: First, acidic systems exhibit indiscriminate corrosion across the entire surface, which can easily lead to localized over-corrosion of thin-walled or complex grooved parts, and dimensional tolerances can easily be exceeded; second, conventional corrosion inhibitors can only adsorb and form films under static conditions, and the protective film is easily torn and peeled off under dynamic friction conditions, resulting in corrosion prevention failure during processing; third, the exposed hard abrasives in traditional systems can cause destructive ploughing cutting of soft copper, which can easily cause grain boundary tearing, surface micro-scratches, and residual stress; finally, the system cannot effectively constrain the free copper ions stripped off during processing, resulting in rapid aging and degradation of the solution, which cannot meet the requirements of long-term cyclic mass production. Summary of the Invention

[0005] (a) Technical problems to be solved

[0006] To address the shortcomings of existing copper polishing slurries, such as global corrosion leading to tolerance exceeding limits, failure of dynamic corrosion inhibition, micro-scratches caused by bare abrasive grinding, and accelerated aging of the slurry by free copper ions, this invention provides a low-scratching polishing slurry for copper parts and its preparation process.

[0007] (II) Technical Solution

[0008] To achieve the above objectives, the present invention provides the following technical solution:

[0009] A low-scratch polishing slurry for copper parts comprises, by weight percentage: 12.0%-22.0% modified coated gradient abrasive system; 2.5%-7.5% friction-triggered polishing and corrosion inhibition system; 2.0%-4.5% lubricating chelating dispersion system; appropriate amount of pH adjuster to adjust the initial pH value of the system to 6.8-7.2; the balance being deionized water.

[0010] Furthermore, the modified coated gradient abrasive system comprises: 5.0%-10.0% cationic modified coarse abrasive; 5.0%-8.0% nonionic coated medium abrasive; and 2.0%-4.0% anionic modified nanospherical abrasive.

[0011] Furthermore, the cationic modified coarse abrasive is alumina particles coated with cationic polyurethane elastomer with a particle size of 3-5 μm; the nonionic coated medium abrasive is alumina or silica particles coated with nonionic polyvinyl alcohol film with a particle size of 0.5-1 μm; and the anionic modified nanospherical abrasive is spherical silica particles grafted with anionic polyacrylate with a particle size of 50-100 nm.

[0012] Furthermore, the friction-triggered polishing and corrosion inhibition system comprises: 2.0%-5.0% of a lactone precursor, which is gluconolactone; 0.1%-0.5% of a heterocyclic corrosion inhibitor, which is 2-mercaptobenzothiazole; and 0.4%-2.0% of a long-chain flexible corrosion inhibitor, which is sodium dodecylsarcosinate.

[0013] Furthermore, the lubricating chelating dispersion system comprises: 1.0%-2.0% of a multidentate chelating agent, which is phytic acid; and 1.0%-2.5% of a silicone-free block polyether interfacial lubricant, which is EO-PO block polyether. The pH adjuster is triethanolamine.

[0014] A preparation process for the aforementioned low-scratch polishing fluid for copper parts includes the following purely physical mixing steps: S1, adding the cationic modified coarse abrasive, the nonionic coated medium abrasive, and the anionic modified nanospherical abrasive to deionized water, and stirring and dispersing at 300-500 rpm for 20-30 minutes at room temperature to construct a network suspension system; S2, sequentially and slowly adding the lactone precursor, heterocyclic corrosion inhibitor, and long-chain flexible corrosion inhibitor, maintaining a stirring speed of 100-200 rpm; S3, adding the multi-toothed chelating agent and the silicone-free block polyether interface lubricant and mixing evenly; S4, adding the pH adjuster to adjust and stabilize the initial pH value of the system to 6.8-7.2.

[0015] Compared with the prior art, the beneficial effects of the present invention are:

[0016] This invention constructs a friction field-responsive point polishing system, in which lactone precursors are hydrolyzed only at the stress points of mechanical grinding, achieving zero etching in non-friction areas and completely solving the problem of dimensional deviations in thin-walled parts caused by acidic global indiscriminate corrosion.

[0017] The dual-layer self-healing corrosion inhibition coupling system constructs a hard-flexible dual-layer film in situ through heterocyclic molecules and long-chain molecules. When the film is damaged by friction, free molecules quickly penetrate and repair it, overcoming the defect of static corrosion inhibitors that are easily torn and peeled off during dynamic processing.

[0018] The modified coated gradient abrasive system utilizes an elastic coating to transform the destructive ploughing of sharp bare abrasive into stress-free rolling grinding. Combined with a mesh-like suspension structure with opposite charge self-assembly, it eradicates grain boundary tears and micro-scratches on the surface of copper at the microscopic level.

[0019] The multidentate chelating agent introduced into the system specifically captures and passivates free copper ions, breaks their catalytic reaction chain, significantly delays the degradation and deterioration of the drug solution, and meets the requirements of long-term cyclic mass production. Attached Figure Description

[0020] The present invention will be further described below with reference to the accompanying drawings and embodiments:

[0021] Figure 1 Diagram showing the modified coated gradient abrasive system and its three-dimensional suspended network structure;

[0022] Figure 2 Flowchart of the low-scratch polishing slurry preparation process;

[0023] Figure 3 The image shows a SEM image of the copper surface after polishing with the low-scratch polishing fluid of the present invention in Example 1.

[0024] Figure 4 This is a SEM image of the copper surface after polishing with ordinary bare abrasive in Comparative Example 1.

[0025] Figure 5 The image shown is a SEM image of the copper surface after polishing with the low-scratch polishing fluid of the present invention in Example 2. Detailed Implementation

[0026] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only for explaining the present invention and are not intended to limit the scope of protection of the present invention.

[0027] This invention aims to solve the problems of scratches, corrosion, and short lifespan in the copper grinding process by combining pure physical components with specific chemical substances, without relying on any complex electromechanical monitoring equipment, and by relying on the spontaneous regulation of interfacial chemical reactions by mechanical and physical working conditions.

[0028] In friction-triggered polishing systems, organic lactone compounds (such as gluconate-δ-lactone, ε-caprolactone, γ-butyrolactone, etc.) are structurally stable in neutral water-soluble systems and exist in an inert, non-acidic state. However, at the microscopic contact surface of the grinding process, under the influence of local high shear force and frictional heat (friction field) between the medium and the workpiece, the lactone ring is induced to undergo site-specific ring-opening hydrolysis, releasing organic acid groups, thus achieving micro-site-specific dissolution only at the microscopic high-protrusion points.

[0029] To achieve the above technical solutions, the commercially available sources of some of the specific core chemical raw materials mentioned in this invention specification are listed below:

[0030] EO-PO block polyether (silicone-free interface lubricant): purchased from Zhejiang Huangma Technology Co., Ltd.;

[0031] Sodium dodecyl sarcosinate (long-chain flexible corrosion inhibitor): purchased from Zanyu Technology Group Co., Ltd. (Zhejiang);

[0032] Anion-modified nanosphere abrasive (spherical silica with anion-grafted polyacrylate on the surface, particle size 50-100nm): purchased from Zhejiang Micro-Nano New Materials Technology Co., Ltd.

[0033] Lactone precursors (such as gluconate-δ-lactone, ε-caprolactone, etc.): purchased from Zhejiang Xinhua Chemical Co., Ltd.

[0034] (Note: Other conventional components of this invention, such as deionized water, triethanolamine, and 2-mercaptobenzothiazole, can be obtained from commercially available conventional chemical sources without any special restrictions.)

[0035] I. Examples and Comparative Examples

[0036] Example 1: A low-scratch polishing fluid for copper parts, the formulation components by weight percentage are as follows:

[0037] Modified coated gradient abrasive system: cationic modified coarse abrasive (alumina surface coated with cationic polyurethane elastomer, 3-5 μm) 8.0%; nonionic coated medium abrasive (silica surface coated with nonionic polyvinyl alcohol, 0.5-1 μm) 6.0%; anionic modified nanospherical abrasive (spherical silica surface grafted with anionic polyacrylate, 50-100 nm) 3.0%.

[0038] Friction-triggered polishing and corrosion inhibition system: gluconate-δ-lactone 3.5%; 2-mercaptobenzothiazole (MBT) 0.3%; sodium dodecyl sarcosinate 1.0%.

[0039] Lubricating chelating dispersion system: 1.5% phytic acid; 1.5% EO-PO block polyether (silicone-free interface lubricant).

[0040] Solvent and pH adjuster: 75.2% deionized water; add an appropriate amount of triethanolamine to precisely adjust the pH of the system to 7.0.

[0041] Combination Figure 2 As shown, its preparation process includes the following mixing steps:

[0042] S1. Add the above three abrasives to deionized water and disperse them at 400 rpm for 25 minutes at room temperature. Relying on the adsorption of opposite charges, they spontaneously construct [a process] in the liquid phase. Figure 1 The three-dimensional mesh suspension system shown;

[0043] S2. Slowly add gluconate-δ-lactone, 2-mercaptobenzothiazole and sodium dodecyl sarcosinate in sequence, and reduce the speed to 150 rpm while maintaining stirring.

[0044] S3. Add phytic acid and EO-PO block polyether and continue to mix evenly;

[0045] S4. Slowly add triethanolamine, monitoring the process throughout, and adjust and stabilize the initial pH of the system to 7.0 to obtain the finished grinding slurry.

[0046] Example 2: Following the same preparation process as Example 1, the following components were prepared by weight percentage: 5.0% cationic modified coarse abrasive, 5.0% nonionic coated medium abrasive, and 2.0% anionic modified nanosphere abrasive; the lactone precursor was replaced with 2.0% ε-caprolactone, 0.1% 2-mercaptobenzothiazole, and 0.4% sodium dodecyl sarcosinate; 1.0% phytic acid and 1.0% EO-PO block polyether; 83.5% deionized water; and the pH was adjusted to 6.8 with triethanolamine.

[0047] Example 3: Following the same preparation process as Example 1, the following components were prepared by weight percentage: 10.0% cationic modified coarse abrasive, 8.0% nonionic coated medium abrasive, and 4.0% anionic modified nanosphere abrasive; the lactone precursor was replaced with 5.0% γ-butyrolactone, 0.5% 2-mercaptobenzothiazole, and 2.0% sodium dodecyl sarcosinate; 2.0% phytic acid, 2.5% EO-PO block polyether; 66.0% deionized water; and the pH was adjusted to 7.2 with triethanolamine.

[0048] Comparative Example 1: The abrasive system was replaced with ordinary bare abrasive (i.e., ordinary alumina and silicon dioxide) without any coating or charge modification, with the same mass percentage and particle size; the remaining components and preparation process were exactly the same as in Example 1.

[0049] Comparative Example 2: The lactone precursor was replaced with citric acid (3.5%) of equivalent acidity; 2-mercaptobenzothiazole and sodium dodecyl sarcosinate were replaced with the conventional monolayer corrosion inhibitor benzotriazole (BTA) (1.3%); the pH was adjusted to 4.5 (within the range of conventional acidic polishing solutions) with triethanolamine. The remaining components and preparation process were exactly the same as in Example 1.

[0050] Comparative Example 3: Phytic acid and EO-PO block polyether were removed. Equal amounts of conventional lubricant (polyethylene glycol) and conventional silicone defoamer were added; the remaining components and preparation process were exactly the same as in Example 1.

[0051] II. Performance Testing and Effect Comparison

[0052] 1. Test conditions

[0053] The polishing slurries of Examples 1-3 and Comparative Examples 1-3 were respectively put into a high-frequency vibration polishing machine, and the same number of pure copper precision machining parts with a 0.2mm thin wall structure and matching polishing media were placed in them; the vibration frequency was set to 35Hz, and continuous polishing was performed for 45 minutes.

[0054] 2. Test Results Table

[0055]

[0056] 3. Mechanism and Data Comparison Analysis

[0057] First, combined Figure 1 and Figure 2 The microscopic mechanism was observed and compared with the SEM electron microscope images of the actual processed material. Figures 3 to 5 As can be seen, the heterogeneous charge three-dimensional suspension network and modified coating technology of the present invention play a decisive buffering role.

[0058] like Figure 3 and Figure 5 As shown, after processing with the polishing fluids of Examples 1 and 2 of this invention, the surface of the copper is extremely smooth, exhibiting a typical stress-free rolling microstructure, and no grain boundary tearing or scratches were observed. This is because the examples used coated modified abrasives, and the elastic coating effectively avoided direct rigid cutting by the hard abrasives. In contrast, in Comparative Example 1, because uncoated ordinary bare hard abrasives were used, the abrasive sharp edges directly penetrated the copper substrate. Figure 4The SEM images clearly show that the surface is covered with dense ploughing grooves, fine micro-scratches, and obvious grain boundary tearing damage. In addition, under macroscopic conditions, the bare abrasive of Comparative Example 1, due to the lack of charge network constraint, underwent severe layering and precipitation after standing for 48 hours, resulting in a polarization of the gloss of the polished copper parts in the same batch (GU value was only 60). In contrast, Examples 1-3, relying on a stable network suspension system, ensured the uniformity of polishing intensity, and the surface gloss (GU value) was stable at 85-88.

[0059] Secondly, regarding the dimensional control of precision thin-walled parts, Examples 1-3 can strictly control the thin-wall loss to an extremely low level of 0.3-0.5 μm. This is mainly due to the use of organic lactone precursors such as gluconolactone in a neutral environment (pH 6.8-7.2). These lactone molecules normally remain in an inert closed-ring state, and only when the polishing slurry and the protrusions on the copper surface are squeezed and collided (friction field) will they rely on shear stress to locally release polar acidic groups to dissolve oxides at specific points. For frictionless surfaces... The thin-walled edges of the sample were largely uncorroded by the solution. In contrast, Comparative Example 2 used conventional citric acid, which caused indiscriminate chemical corrosion throughout the entire area, resulting in severe edge corrosion of the thin-walled corners, with a loss of up to 5.8 μm, causing the parts to exceed tolerances and be scrapped. Meanwhile, the example utilized a double-layer protective film constructed from heterocyclic and long-chain flexible molecules, which allowed free molecules to penetrate and repair in situ when local damage occurred. Its dynamic anti-corrosion effect was far superior to the single-layer static BTA film in Comparative Example 2, which was easily torn and peeled off during grinding.

[0060] Finally, the introduction of multi-toothed chelating agents is crucial for extending the cycle life of the grinding solution. Comparative Example 3 eliminated the phytic acid chelating agent, and the free copper ions that were detached during the grinding process quickly accumulated in large quantities in the grinding solution, and reversed the degradation of the solution. Combined with the damage to the protective film on the copper surface caused by conventional silicone defoamers, the grinding solution deteriorated and turned black after three cycles. Examples 1-3, on the other hand, utilized the strong multi-toothed chelating effect of phytic acid to firmly lock and passivate the free copper ions in the system, cutting off their catalytic reaction chain. This significantly increased the stable cycle life of the grinding solution under continuous mass production conditions to more than 12-15 batches. Combined with the spontaneous defoaming characteristics of silicone-free block polyether, it effectively eliminated the processing blind zone and greatly improved the actual processing yield and the continuity of equipment operation.

Claims

1. A low-scratch polishing fluid for copper parts, characterized in that, By weight percentage, it includes the following components: Modified coated gradient abrasive system: 12.0%-22.0%; Friction-triggered polishing and corrosion inhibition system: 2.5%-7.5%; Lubricating chelating dispersion system: 2.0%-4.5%; pH adjuster: Appropriate amount, used to adjust the initial pH value of the system to 6.8-7.2; The remainder is deionized water; The modified coated gradient abrasive system includes cationic modified coarse abrasive, nonionic coated medium abrasive, and anionic modified nanospherical abrasive; the friction-triggered polishing and corrosion inhibition system includes lactone precursors, heterocyclic corrosion inhibitors, and long-chain flexible corrosion inhibitors; and the lubricating chelating dispersion system includes multi-toothed chelating agents and silicone-free block polyether interface lubricants.

2. The low-scratch polishing fluid for copper parts according to claim 1, characterized in that, The modified coated gradient abrasive system comprises, by weight percentage: Cationic modified coarse abrasive: 5.0%-10.0%; Non-ionic coated medium abrasive: 5.0%-8.0%; Anion-modified nanosphere abrasive: 2.0%-4.0%.

3. The low-scratch polishing fluid for copper parts according to claim 2, characterized in that, The cationic modified coarse abrasive is alumina particles coated with cationic polyurethane elastomer, with a particle size of 3-5 μm; The abrasive in the non-ionic coating is an alumina or silica particle with a non-ionic polyvinyl alcohol film coated on its surface, and the particle size is 0.5-1μm. The anion-modified nanosphere abrasive is a spherical silica particle with anion-modified polyacrylate grafted onto its surface, and has a particle size of 50-100 nm.

4. The low-scratch polishing fluid for copper parts according to claim 1, characterized in that, The friction-triggered polishing and corrosion inhibition system comprises, by weight percentage: Lactone precursor: 2.0%-5.0%, wherein the lactone precursor is gluconolactone; Heterocyclic corrosion inhibitor: 0.1%-0.5%, wherein the heterocyclic corrosion inhibitor is 2-mercaptobenzothiazole; Long-chain flexible corrosion inhibitor: 0.4%-2.0%, wherein the long-chain flexible corrosion inhibitor is sodium dodecyl sarcosinate.

5. The low-scratch polishing fluid for copper parts according to claim 1, characterized in that, The lubricating chelating dispersion system comprises, by weight percentage: Multidentate chelating agent: 1.0%-2.0%, wherein the multidentate chelating agent is phytic acid; Silicone-free block polyether interface lubricant: 1.0%-2.5%, wherein the silicone-free block polyether interface lubricant is EO-PO block polyether.

6. The low-scratch polishing fluid for copper parts according to claim 1, characterized in that, The pH adjuster is triethanolamine.

7. A preparation process for a low-scratch polishing slurry for copper parts as described in any one of claims 1-6, characterized in that, Includes the following steps: S1. Mixing and dispersing: The cationic modified coarse abrasive, the nonionic coated medium abrasive and the anionic modified nanosphere abrasive are added to the deionized water and stirred and dispersed at room temperature, and a network suspension system is constructed by adsorption of opposite charges. S2. Addition of slow-release components: Slowly add the lactone precursor, heterocyclic corrosion inhibitor and long-chain flexible corrosion inhibitor in sequence, while maintaining stirring. S3, Chelating Lubricant Addition: Add the multi-toothed chelating agent and the silicone-free block polyether interface lubricant, and mix evenly; S4. Neutralization and steady-state adjustment: Add the pH adjuster to adjust and stabilize the initial pH value of the system to 6.8-7.2, thus obtaining the grinding slurry.

8. The preparation process according to claim 7, characterized in that, In step S1, the stirring speed is 300-500 rpm and the dispersion time is 20-30 minutes; in step S2, the stirring speed is 100-200 rpm.

Citation Information

Patent Citations

  • A chemical polishing solution and an alloy surface polishing treatment method

    CN103757636B