A composition with gas phase corrosion inhibition and lubrication functions, a preparation method and application thereof

By integrating corrosion inhibitors and lubricants into the same powdered composition and using a porous adsorbent carrier to load volatile lubricants to form a composite film, the problem of single function of vapor phase corrosion inhibitors is solved. This achieves corrosion protection and lubrication protection for moving parts in a closed cavity, improves corrosion inhibition efficiency, and reduces the coefficient of friction.

CN123132887APending Publication Date: 2026-11-20CHINA SHIPBUILDING INDUSTRY CORPORATION NO725 RESEARCH INSTITUTE
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611310789.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing vapor phase corrosion inhibitors have limited functionality and cannot adequately provide lubrication. Furthermore, there is a contradiction between vapor phase volatilization and interfacial lubrication at the molecular design level, making it difficult to achieve both long-term corrosion inhibition and continuous lubrication in the same system.

Method used

By integrating corrosion inhibitors and lubricants into the same powdered composition, and by rationally controlling the ratio and loading volatile lubricants onto porous adsorbent carriers, a composite film is formed to achieve non-contact protection.

Benefits of technology

It achieves both corrosion protection and lubrication protection for moving parts in closed or semi-closed cavities, improves corrosion inhibition efficiency, reduces the coefficient of friction, and uses environmentally friendly raw materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123132887A_ABST
    Figure CN123132887A_ABST
Patent Text Reader

Abstract

The application provides a composition with gas-phase corrosion inhibition and lubrication functions, a preparation method and application, and the composition comprises a corrosion inhibition component and a lubrication component; the corrosion inhibition component comprises a gas-phase corrosion inhibitor; the lubrication component comprises a volatile lubricant and a porous adsorption carrier, and the volatile lubricant is loaded on the porous adsorption carrier. The corrosion inhibition component is volatilized in a gas phase to form adsorption on a metal surface, and the porous adsorption carrier is used to load and slowly release the volatile lubricant, so that the corrosion inhibition component and the lubrication component are orderly co-adsorbed on the metal surface to form a composite film interface layer; the slow release of the lubricant by the porous carrier can keep the lubrication film stable for a long time, avoid short-term failure, and thus realize the synergistic long-term protection of corrosion protection and lubrication and friction reduction of moving parts in a closed or semi-closed cavity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal protection technology, and more specifically, to a composition that combines vapor phase corrosion inhibition and lubrication functions, its preparation method, and its application. Background Technology

[0002] Metal corrosion is a common problem in industrial production and daily life, especially in marine atmospheric environments. High salt spray, high humidity, and chloride ion corrosion significantly accelerate metal corrosion failure, leading to shortened equipment lifespan, increased safety hazards, and substantial economic losses. Volatile corrosion inhibitors (VCIs) are functional materials that release corrosion-inhibiting gases at room temperature. These gases diffuse and adsorb onto the metal surface, forming a protective film that inhibits atmospheric corrosion. Compared to traditional protective measures such as coatings and electroplating, VCIs can reach complex structures like crevices and blind holes without direct contact with the metal surface. The resulting protective film is extremely thin and does not affect component precision. Therefore, they are particularly suitable for atmospheric corrosion protection of precision instruments, enclosed cavities, and components with complex internal structures, and have become one of the most widely used methods in the field of corrosion protection.

[0003] To overcome the drawbacks of traditional synthetic vapor phase corrosion inhibitors, such as high toxicity and poor degradation, various green and environmentally friendly vapor phase corrosion inhibitors have been developed in this field. For example, patent application number 201510710217.6 discloses a plant-based vapor phase copper corrosion inhibitor, which is composed of garlic extract and bay leaf extract in a weight ratio of 3:1. It utilizes the sulfur-containing volatile organic compounds in the garlic extract to form an adsorption film on the copper surface, achieving a corrosion inhibition efficiency of up to 73.2%. Furthermore, the raw materials are natural, non-toxic, and simple to prepare. However, this type of plant-based vapor phase corrosion inhibitor, and most existing vapor phase corrosion inhibitor products, only possess the single function of corrosion protection and completely lack lubrication and friction reduction capabilities. During storage and transportation, metal products may experience relative movement or friction, especially moving parts inside devices, leading to surface scratches and accelerated wear. Single-function vapor phase corrosion inhibitors are ineffective in addressing these issues.

[0004] Therefore, there is an urgent need for a green, safe, and volatile stable vapor phase corrosion inhibitor lubricant composition that can simultaneously provide long-lasting corrosion protection and continuous lubrication in enclosed or semi-enclosed spaces. Summary of the Invention

[0005] The purpose of this invention is to provide a composition, preparation method and application that have both vapor phase corrosion inhibition and lubrication functions, in order to solve the technical problems of existing vapor phase corrosion inhibitors having single function and difficulty in taking into account lubrication function, as well as the contradiction between vapor phase volatilization and interfacial lubrication at the molecular design level, making it difficult to achieve long-term corrosion inhibition and continuous lubrication in the same system.

[0006] To achieve the above objectives, the present invention provides a composition that combines vapor phase corrosion inhibition and lubrication functions, the composition comprising a corrosion inhibitor and a lubricating component;

[0007] The corrosion inhibitor component includes a vapor phase corrosion inhibitor;

[0008] The lubricating component includes a volatile lubricant and a porous adsorbent carrier, wherein the volatile lubricant is loaded on the porous adsorbent carrier.

[0009] In this invention, the composition is in powder form. The volatile lubricant does not exist in a free liquid state, but is adsorbed by the carrier and appears in powder form. When used, it enters the gas phase through volatilization.

[0010] This invention integrates corrosion inhibitors and lubricants (volatile lubricants loaded on a porous adsorbent carrier) into a single powder composition, achieving for the first time a single product simultaneously possessing both vapor-phase corrosion inhibition and vapor-phase lubrication functions. This overcomes the limitations of traditional vapor-phase corrosion inhibitors with their single-function approach and solves the technical challenge of simultaneously providing corrosion protection and lubrication / friction reduction to moving parts in closed / semi-closed cavities. Furthermore, the powder form allows for free placement within the cavity without direct contact with the protected surface, achieving non-contact protection.

[0011] Furthermore, the mass ratio of the corrosion inhibitor to the lubricant is 1-4:1-2.

[0012] In this invention, the mass ratio of the corrosion inhibitor to the lubricant is preferably 1 to 1.5: 1 to 1.5.

[0013] This invention achieves a synergistic effect of corrosion inhibition and lubrication by rationally controlling the ratio of corrosion inhibitor and lubricant components, ensuring that their concentrations in the gas phase are matched—the corrosion inhibitor concentration is sufficient to form a complete protective film, and the lubricant concentration is sufficient to reduce the coefficient of friction without interfering with the preferential adsorption of the corrosion inhibitor.

[0014] Furthermore, based on the mass of the lubricating component as 100%, the mass percentage of the volatile lubricant is 20wt% to 40wt%, and the mass percentage of the porous adsorbent carrier is 60wt% to 80wt%.

[0015] In this invention, based on the mass of the lubricating component as 100%, the mass percentage of the volatile lubricant is preferably 30wt% to 40wt%, and the mass percentage of the porous adsorbent carrier is preferably 60wt% to 70wt%.

[0016] In this invention, the volatile lubricant is loaded onto the porous adsorption carrier by atomization spraying.

[0017] Furthermore, the corrosion inhibitor component comprises a long-acting vapor phase corrosion inhibitor and a short-acting vapor phase corrosion inhibitor; based on the mass of the corrosion inhibitor component as 100%, the mass percentage of the long-acting vapor phase corrosion inhibitor is 30wt% to 50wt%, and the mass percentage of the short-acting vapor phase corrosion inhibitor is 50wt% to 70wt%.

[0018] The short-acting formulation rapidly evaporates to form an initial protective film, with quick onset of action; the long-acting formulation releases slowly to maintain long-term protection, with a long protection period. The synergy of the two allows the composition to continuously exert its corrosion-inhibiting effect throughout the entire protection cycle, avoiding the problems of no film to rely on in the initial stage of protection and film failure in the later stage of protection.

[0019] Furthermore, the long-acting vapor phase corrosion inhibitor is selected from one or two of acetaminophen and L-glutamine; the short-acting vapor phase corrosion inhibitor is selected from one or two of gallnut extract and garlic extract.

[0020] Acetaminophen and L-glutamine molecules contain N, O heteroatoms and amide groups, which can form coordination bonds with the metal surface through lone pairs of electrons, resulting in chemisorption with high adsorption strength and strong binding. Gallnut extract (rich in tannins and gallic acid) and garlic extract (rich in sulfur-containing compounds) have rapid volatilization rates, enabling the formation of an initial protective layer in a short time. The combination of these two ingredients achieves a complementary relationship between rapid film formation and long-lasting protection. Furthermore, since the raw materials are all natural products and drug molecules, the toxicity problems of traditional corrosion inhibitors are avoided.

[0021] In this invention, the short-acting vapor phase corrosion inhibitor is preferably a mixture of gallnut extract and garlic extract, and the mass ratio of gallnut extract to garlic extract is 1:1; the long-acting vapor phase corrosion inhibitor is preferably a mixture of acetaminophen and L-glutamine, and the mass ratio of acetaminophen to L-glutamine is 1-1.5:1-1.5.

[0022] Furthermore, the volatile lubricant is selected from one or more of polyethylene glycol monomethyl ether, ethyl oleate, ethyl lactate, and ethyl acetate.

[0023] It should be noted that the present invention does not strictly limit the specific type of the volatile lubricant, as long as it can slowly volatilize into the gas phase under normal temperature or mild heating conditions and form a gaseous lubricating film on the metal surface; the specific type of the porous adsorbent carrier is also not strictly limited, as long as it has a porous structure and can adsorb and slowly release the volatile lubricant.

[0024] Furthermore, the porous adsorbent is selected from one or more of diatomaceous earth and fumed silica.

[0025] This invention uses a porous adsorption carrier to adsorb and load liquid volatile lubricant, and slows down its release rate through capillary action, thereby achieving a long-term and continuous supply of lubricant.

[0026] In this invention, the porous adsorbent carrier is preferably a mixture of diatomaceous earth and fumed silica. The two complement each other at the pore size scale—the macropores of diatomaceous earth provide ample oil storage space, while the nanopores of fumed silica control the release rate through strong capillary action, achieving a graded slow release with macropore oil storage and mesopore controlled release. At the particle size scale, nano-sized fumed silica fills the spaces between micron-sized diatomaceous earth particles, extending the diffusion path of lubricant molecules and further slowing down release. In terms of surface properties, both contain silanol groups, but their adsorption affinity for lubricant molecules of different polarities differs. The composite carrier achieves good loading and compatible release for different types of lubricants. The synergistic effect of these three effects makes the composite carrier superior to a single carrier in terms of loading capacity, release rate, and compatibility.

[0027] The present invention also provides a method for preparing the composition described in the above technical solution, comprising the following steps:

[0028] (1) Preparation of corrosion inhibitor: The long-acting vapor phase corrosion inhibitor and the short-acting vapor phase corrosion inhibitor are mixed in proportion, ground and sieved to obtain corrosion inhibitor powder;

[0029] (2) Preparation of lubricating components: After the volatile lubricant is mixed evenly, it is added to the porous adsorption carrier by atomization spraying. The adsorption is carried out at room temperature for 20 to 30 minutes, then taken out, ground and sieved to obtain porous adsorption carrier powder loaded with volatile lubricant.

[0030] (3) Compounding: The corrosion inhibitor powder obtained in step (1) and the lubricating powder obtained in step (2) are mixed according to the ratio, ground and sieved to obtain the composition with both gas phase corrosion inhibition and lubrication functions.

[0031] The present invention also provides the application of the composition described above in the corrosion protection and lubrication of copper alloys or copper metals in marine atmospheric environments.

[0032] Furthermore, the composition is placed directly in a closed or semi-closed cavity in powder form. After the vapor-phase corrosion inhibitor in the corrosion inhibitor component volatilizes, it is adsorbed together with the volatile lubricant in the lubricating component that volatilizes after being released by the porous adsorption carrier and forms a composite film layer, which provides non-contact corrosion protection and lubrication friction reduction for the moving parts in the cavity.

[0033] This invention eliminates the need to directly coat the composition onto the metal surface. Instead, it automatically delivers the composition to the protected surface through vapor evaporation, making it suitable for moving parts inside enclosed cavities that cannot be directly coated.

[0034] This invention places the composition in powder form directly into a closed or semi-closed cavity, eliminating the need for coating contact or any pretreatment of the protected object. It achieves automatic full-space coverage—including areas inaccessible by traditional coating methods such as gaps and dead corners—through the vapor-phase evaporation of corrosion inhibitors and lubricants. The in-situ composite of the corrosion inhibitor and lubricant films provides moving parts with dual protection against corrosion and lubrication, fundamentally solving the long-standing technical problem of not being able to apply oil or prevent rust on moving parts in closed cavities, and filling a technological gap in this application field.

[0035] Compared with existing technologies, the composition, preparation method, and application of the present invention, which combine vapor phase corrosion inhibition and lubrication functions, have the following advantages:

[0036] (1) This invention integrates corrosion inhibitors and volatile lubricants loaded on porous adsorption carriers into the same powder composition, and for the first time realizes that a single product has both gas phase corrosion inhibition and gas phase lubrication functions, solving the technical problem that moving parts in a closed cavity cannot obtain corrosion protection and lubrication protection at the same time.

[0037] (2) This invention scientifically combines short-acting and long-acting vapor phase corrosion inhibitors. The short-acting component rapidly volatilizes to form an initial protective film, achieving immediate effectiveness, while the long-acting component continuously releases to maintain long-term protection. The two work together to achieve balanced protection throughout the entire lifecycle. At the same time, the capillary action of the porous carrier is used to stably release the lubricant, ensuring a continuous and stable supply of lubricant during the 30-day protection period, thus maintaining a long-term stable friction coefficient. Based on this, by controlling the lubricant release rate through the carrier, the corrosion inhibitor component can be slowly migrated to the metal interface along with the lubricating component to continuously replenish the film. Through molecular compounding, interface regulation, and porous slow-release process design, the corrosion inhibitor component and the lubricating component are co-adsorbed on the metal surface, constructing a composite interface film that combines lubrication and friction reduction with long-term corrosion inhibition protection. This overcomes the long-standing technical prejudice in the industry that "lubricating oil will destroy the corrosion inhibitor film," achieving synergistic effect between the two. Experiments show that after adding the lubricating component, the corrosion inhibition efficiency does not decrease but increases (from 85.43% to 86.19%), and the friction coefficient decreases by more than 30%, verifying the comprehensive advantages of this invention in long-term protection and stable lubrication.

[0038] (3) In addition, the raw materials of the present invention are selected from natural plant extracts and drug molecules, which are green and environmentally friendly; the powder form can be placed directly in a closed cavity, and the gas phase volatilization automatically covers the hard-to-reach areas, realizing convenient non-contact protection. Attached Figure Description

[0039] Figure 1 The polarization curve of copper in natural seawater solution;

[0040] Figure 2 Polarization curves of copper in natural seawater solution with 1 g / L corrosion inhibitor added;

[0041] Figure 3 Photographs showing the appearance of copper sheets without any protective composition after a 30-day corrosion weight loss test;

[0042] Figure 4 The image shows the appearance of a copper sheet after a 30-day corrosion weight loss test, which was used to test the vapor phase corrosion inhibition performance of the composition of Example 2. Detailed Implementation

[0043] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the described embodiments are only some, not all, of the embodiments of this invention. The specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention. It should be noted that, unless otherwise specified, the embodiments and features described in these embodiments can be combined with each other.

[0044] For vapor-phase corrosion inhibitors, their molecules typically need to possess high vapor pressure to achieve effective transport in the gas phase; while for lubrication, molecules are required to form a stable, dense adsorption film on the metal surface to bear frictional loads. These two requirements are fundamentally contradictory at the same molecular level—high volatility means weak interaction between molecules and the metal surface, making it difficult to form a stable lubricating film; while strong adsorption means that molecules are difficult to detach from the surface and enter the gas phase. Therefore, in existing technologies, lubrication and vapor-phase corrosion inhibition functions are usually designed as independent systems. More importantly, it is widely believed in the industry that lubricating oil molecules can damage the corrosion inhibition film; that is, after lubricating oil molecules physically cover the metal surface, they will occupy the adsorption sites of corrosion inhibitor molecules, preventing the formation of coordination bonds between the polar groups such as N and O in the corrosion inhibitor molecules and the metal surface, resulting in a significant reduction in corrosion inhibition efficiency. Therefore, those skilled in the art not only do not actively combine the two, but also consciously avoid it.

[0045] It should be noted that in the following embodiments, the gallnut extract and garlic extract are powdered extracts obtained by Soxhlet extraction with anhydrous ethanol. Specifically, the gallnuts / garlic are washed clean, dried in an oven at 50°C for 24 hours, then crushed in an agate mortar and sieved to obtain coarse powder. 5g of the coarse powder is weighed and placed in a 250mL round-bottom flask, 150mL of anhydrous ethanol is added, and Soxhlet extraction is performed at 65°C for 3 hours. After cooling, the mixture is filtered, and the filtrate is collected. The filtrate is concentrated by rotary evaporation at 50°C, and the resulting concentrate is transferred to a vacuum drying oven at 60°C and dried for 24 hours to remove excess solvent. The dried extract is then ground into powder again to obtain powdered gallnut extract / powdered garlic extract, which is then sealed and stored in a desiccator for later use.

[0046] In the following examples, the acetaminophen, L-glutamine, polyethylene glycol monomethyl ether, ethyl oleate, ethyl lactate, diatomaceous earth, and fumed silica are all commercially available reagents.

[0047] Example 1

[0048] A composition that combines vapor phase corrosion inhibition and lubrication functions includes:

[0049] Corrosion-inhibiting components: acetaminophen 8g, L-glutamine 8g, gallnut extract 12g, garlic extract 12g;

[0050] Lubricating components: 10g polyethylene glycol monomethyl ether, 10g ethyl oleate, 20g diatomaceous earth, and 20g fumed silica.

[0051] The method for preparing the composition includes the following steps:

[0052] (1) Preparation of corrosion inhibitory component: Mix 8g of acetaminophen, 8g of L-glutamine, 12g of gallnut extract and 12g of garlic extract, grind and sieve to obtain corrosion inhibitory component powder;

[0053] (2) Preparation of lubricating components: After mixing 10g of polyethylene glycol monomethyl ether and 10g of ethyl oleate evenly, add them to 20g of diatomaceous earth and 20g of fumed silica by atomization spraying. After adsorption at room temperature for 20-30 minutes, take them out, grind and sieve them to obtain porous adsorbent carrier powder loaded with volatile lubricant.

[0054] (3) Compounding: The corrosion inhibitor powder obtained in step (1) is mixed with the lubricating powder obtained in step (2), ground and passed through a 120-mesh sieve to obtain the composition that has both vapor phase corrosion inhibition and lubrication functions.

[0055] Example 2

[0056] A composition that combines vapor phase corrosion inhibition and lubrication functions includes:

[0057] Corrosion-inhibiting components: 15g acetaminophen, 15g L-glutamine, 15g gallnut extract, 15g garlic extract;

[0058] Lubricating components: 15g ethyl lactate, 15g diatomaceous earth, 10g fumed silica.

[0059] The preparation method of the composition described in this embodiment is the same as that in Example 1, except that the proportions of each component are different.

[0060] Example 3

[0061] A composition that combines vapor phase corrosion inhibition and lubrication functions includes:

[0062] Corrosion-inhibiting components: 15g acetaminophen, 3g L-glutamine, 16g gallnut extract, 16g garlic extract;

[0063] Lubricating components: 18g ethyl oleate, 32g fumed silica.

[0064] The preparation method of the composition described in this embodiment is the same as that in Example 1, except that the proportions of each component are different.

[0065] Example 4

[0066] A composition that combines vapor phase corrosion inhibition and lubrication functions includes:

[0067] Corrosion-inhibiting components: 7g acetaminophen, 7g L-glutamine, 19g gallnut extract, 19g garlic extract;

[0068] Lubricating components: 8g ethyl oleate, 8g ethyl acetate, 32g fumed silica.

[0069] The preparation method of the composition described in this embodiment is the same as that in Example 1, except that the proportions of each component are different.

[0070] Example 5

[0071] A composition that combines vapor phase corrosion inhibition and lubrication functions includes:

[0072] Corrosion-inhibiting components: acetaminophen 4g, L-glutamine 8g, gallnut extract 14g, garlic extract 14g;

[0073] Lubricating components: 10g polyethylene glycol monomethyl ether, 10g ethyl oleate, 20g diatomaceous earth, and 20g fumed silica.

[0074] The preparation method of the composition described in this embodiment is the same as that in Example 1, except that the proportions of each component are different.

[0075] Comparative Example 1

[0076] This comparative example only added acetaminophen for testing and contained no other substances.

[0077] Comparative Example 2

[0078] This comparative experiment only added gallnut extract and contained no other substances.

[0079] Comparative Example 3

[0080] This comparative example only added a common vapor phase corrosion inhibitor, urea, for testing and contained no other substances.

[0081] Performance testing

[0082] (1) Reduced volatile matter experiment

[0083] Each single-component vapor phase corrosion inhibitor powder was weighed out at 0.02 g and placed in a clean PTFE petri dish with a diameter of 5 cm. The dish was then placed in an oven at 50 °C and heated continuously for 72 h. The volatility of the corrosion inhibitor was determined based on the weight loss rate. The results are shown in Table 1 below.

[0084] Table 1. Volatility properties of garlic extract, gallnut extract, glutamine, and acetaminophen

[0085] corrosion inhibitor Volatilization rate (%) Garlic extract 50.08 Gallnut extract 42.30 glutamine 9.71 acetaminophen 7.74

[0086] As can be seen from Table 1, the volatility of garlic extract and gallnut extract is significantly higher than that of acetaminophen and L-glutamine, indicating that natural plant extracts are short-acting vapor phase corrosion inhibitors (fast onset and short protection period), while acetaminophen and L-glutamine are long-acting vapor phase corrosion inhibitors (slow onset and long protection period).

[0087] (2) Electrochemical experiments

[0088] Electrochemical tests were performed using a classic three-electrode system, with a working electrode made of metallic material, a counter electrode made of a 1cm×1cm platinum sheet, and a reference electrode made of saturated calomel electrode.

[0089] Figure 1 This is the polarization curve of copper in natural seawater solution. From... Figure 1 As can be seen, without the addition of any corrosion inhibitor, the self-corrosion current density of copper metal is relatively large and the corrosion rate is relatively high, indicating that copper metal undergoes significant corrosion in the simulated marine atmospheric environment.

[0090] Figure 2 The polarization curves of copper in natural seawater solution with 1 g / L corrosion inhibitor are shown. Figure 2 As can be seen, after adding the corrosion inhibitor, the self-corrosion potential changes within 85mV, indicating that the corrosion inhibitor is a mixed inhibitor; the polarization curve shows a leftward shift, indicating that the corrosion inhibitor simultaneously inhibits the anodic dissolution and cathodic depolarization processes of copper metal; the corrosion potential shifts positively, indicating a weakening of the metal ionization tendency; the self-corrosion current density decreases significantly, indicating that a protective film has formed on the copper surface, effectively slowing down the corrosion rate of the metal, with a corrosion inhibition efficiency of over 80%.

[0091] (3) Test of vapor phase corrosion inhibition performance

[0092] The composition samples obtained in Examples 1-5 and Comparative Examples 1-3 were placed in weighing bottles and then placed in wide-mouth bottles containing a 35wt% glycerol seawater solution. After evaporation for one day, a clean copper alloy metal sheet was suspended in the wide-mouth bottle and sealed with plastic wrap to ensure that the bottom of the metal sheet did not contact the solution. To simulate the condensation effect of a real marine atmospheric environment, the sample was heated at 50°C for 8 hours and then placed at room temperature for 16 hours, with a total experimental duration of 30 days. The mass of the alloy sample was weighed before and after the experiment using the weight loss test method, and the corrosion inhibition efficiency was calculated by the mass difference. The test results are shown in Table 2 below. At the same time, to compare the effect of the lubricating component on the corrosion inhibition performance, corrosion inhibition component powder (without lubricating component) prepared in each example was also used in the above experiment. The comparison results of the corrosion inhibition efficiency under the two conditions are shown in Table 2 below.

[0093] Table 2. Corrosion inhibition performance test results of Examples 1-5 and Comparative Examples 1-3

[0094] Serial Number Corrosion inhibition efficiency (excluding lubricating components) (%) Corrosion inhibition efficiency (including lubricating components) (%) Vapor phase corrosion level Example 1 85.43 86.19 1 Example 2 80.33 81.42 1 Example 3 84.32 86.03 1 Example 4 82.31 84.12 1 Example 5 80.87 82.05 1 Comparative Example 1 63.34 —— 2 Comparative Example 2 55.23 —— 2 Comparative Example 3 54.42 —— 2 Blank group —— —— 3

[0095] As shown in Table 2, in all embodiments, regardless of whether a lubricating component is added, the corrosion inhibition efficiency of the composition reaches over 80%, and the vapor phase corrosion level is Grade 1, meeting the rust prevention requirements in a marine atmospheric environment. Comparing the data from the "without lubricating carrier" and "with lubricating carrier" sets, it can be found that the corrosion inhibition efficiency is further improved after adding the lubricating component, increasing from 85.43% to 86.19% in Example 1. This result indicates that the lubricating component not only does not damage the integrity of the corrosion inhibition film, but also produces a synergistic effect with it—this may be because the lubricant molecules, after being slowly released through the porous adsorption carrier, volatilize to the metal surface with the corrosion inhibitor, achieving co-adsorption and orderly arrangement. The long alkyl chain provides a lubricating hydrophobic barrier, and the polar corrosion inhibitory groups anchor the metal, simultaneously reducing friction and inhibiting corrosion, thereby improving the overall rust prevention performance.

[0096] Figure 3 Photographs of the appearance of copper sheets without any protective composition after a 30-day corrosion weight loss test (blank control group). From Figure 3 As can be seen, obvious corrosion products appeared on the surface of the copper sheet, presenting as uneven dark rust spots, with green copper rust appearing in some areas, indicating that the copper sheet underwent severe corrosion in the simulated marine atmospheric environment.

[0097] Figure 4 Photographs of the copper sheet after a 30-day corrosion weight loss test, showing the appearance of the copper sheet used in the vapor phase corrosion inhibition performance test of the composition of Example 2. Figure 4 As can be seen, the copper sheet protected by the composition of Example 2 has a smooth surface with no obvious corrosion marks, maintaining the original metallic luster of copper. This indicates that the composition of the present invention has excellent corrosion protection effect on copper alloys in a simulated marine atmospheric environment. Figure 3 and Figure 4 The comparison clearly shows that the composition of the present invention can effectively inhibit the corrosion of copper metal in the marine atmosphere.

[0098] (4) Lubrication performance test

[0099] After the copper sheets were subjected to vapor phase corrosion inhibition performance tests for different durations (initial, two weeks, and four weeks), they were removed and the surface corrosion products were retained without any treatment. They were then directly subjected to friction and wear tests to simulate the working conditions in actual use when the metal surface has a protective film or corrosion products and is directly subjected to friction. The friction coefficient and volume wear rate of the blank copper sheet without vapor phase corrosion inhibition treatment, as well as the test pieces of each embodiment and comparative example, were compared. The test results are shown in Table 3 below.

[0100] Table 3. Test results of friction and wear performance of Examples 1-5 and Comparative Examples 1-3.

[0101]

[0102] As shown in Table 3, the friction coefficients of each comparative group increased significantly with the extension of test time, indicating that the surface condition of the copper sheets without effective protection continued to deteriorate under the combined effects of corrosion and friction. In the absence of a lubricating carrier, the friction coefficients of each embodiment also increased with test time, indicating that the solid friction-reducing effect of the corrosion inhibitor adsorbent film alone is insufficient to maintain long-term stability, and this solid film gradually ruptures and fails under continuous alternating stress. In contrast, with the addition of a lubricating carrier, the friction coefficients of each embodiment decreased significantly and tended to stabilize with the extension of test time. The volumetric wear rate was also much lower than that of the group without a lubricating carrier, indicating that the porous adsorbent carrier achieved a slow and continuous release of volatile lubricant, continuously replenishing the lubricating film at the friction interface, and synergistically forming a stable composite film layer with the corrosion inhibitor adsorbent film, thereby maintaining excellent lubrication stability during long-term service.

[0103] Even without added lubricating components, the corrosion inhibitor itself still exhibits a certain friction-reducing effect, likely due to the physicochemical properties of the corrosion inhibitor's adsorbed film. After adsorbing onto the metal surface, the corrosion inhibitor molecules form a protective film, altering the contact state of the friction interface. This transforms the dry friction with the friction surface into interfacial friction with the boundary film, thereby reducing the coefficient of friction and decreasing the degree of frictional wear. Furthermore, the N, O, and S heteroatoms and their long alkyl chains commonly found in corrosion inhibitor molecules possess polarity and hydrophobicity, enabling them to form a low-shear-strength molecular layer on the metal surface, providing a boundary lubrication effect similar to a "solid lubricant." Particularly noteworthy are the tannins and gallic acid in gallnut extract and the sulfur-containing compounds in garlic extract; these molecules themselves possess polarity and interfacial activity, forming a shear-sensitive molecular layer between friction pairs. Comparative Examples 1-3 and Examples 1-5 all exhibited lower coefficients of friction than the control group when no lubricating carrier was present, demonstrating that the corrosion inhibitor adsorbed film does indeed have a certain solid-state friction reduction effect. However, this friction reduction effect falls under the category of solid boundary lubrication, which depends on the integrity and stability of the film. When the solid film develops microcracks or local peeling under continuous alternating stress, it cannot repair itself. Therefore, the coefficient of friction increases with the extension of the test time (e.g., in Example 1, it increased from 0.125 after two weeks to 0.152 after four weeks). The key to this invention lies in introducing a porous carrier to load a volatile lubricant. Utilizing its continuous and slow release characteristic, it co-adsorbs and arranges in an orderly manner with the corrosion inhibitor component on the metal surface, forming a self-healing liquid lubricating film. This upgrades unstable solid-state friction reduction to long-term stable solid-liquid composite lubrication, thereby achieving a significant reduction and long-term stability of the coefficient of friction.

[0104] The reason for its long-term stability is speculated to be that the corrosion inhibitor slowly migrates to the metal interface along with the lubricating component. The N and O heteroatoms in the corrosion inhibitor form chemical adsorption with the metal surface through coordination bonds. The low-molecular-weight polar oily agents, short-chain esters, and light fractions in the lubricating component co-vaporize and condense on the metal surface. The outward-oriented alignment of non-polar alkyl groups provides a low-friction barrier, while polar groups anchor the metal to inhibit corrosion. Through molecular structure matching and ratio control, an ordered co-adsorption composite film is achieved, forming a composite interface layer. When friction occurs, this composite film can effectively reduce the coefficient of friction. Even if the lubricating film is partially worn down by friction, the lubricant molecules continuously released by the porous carrier can replenish and repair it in time, achieving a "repair as you wear" self-repair effect, thus maintaining excellent lubrication stability during long-term service. Simultaneously, by controlling the lubricant release rate through the carrier, the gaseous components can migrate to the metal interface to continuously replenish the film, further isolating the penetration of corrosive media. Therefore, the corrosion inhibition efficiency increases rather than decreases after the addition of the lubricating component (e.g., from 85.43% to 86.19% in Example 1), exhibiting a synergistic effect of corrosion inhibition and lubrication.

[0105] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.

Claims

1. A composition possessing both vapor phase corrosion inhibition and lubrication functions, characterized in that, The composition includes a corrosion inhibitor and a lubricating component; The corrosion inhibitor component includes a vapor phase corrosion inhibitor; The lubricating component includes a volatile lubricant and a porous adsorbent carrier, wherein the volatile lubricant is loaded on the porous adsorbent carrier.

2. The composition according to claim 1, characterized in that, The mass ratio of the corrosion inhibitor to the lubricant is 1-4:1-2.

3. The composition according to claim 1, characterized in that, Based on the mass of the lubricating component as 100%, the volatile lubricant has a mass percentage of 20wt% to 40wt%, and the porous adsorbent carrier has a mass percentage of 60wt% to 80wt%.

4. The composition according to claim 1, characterized in that, The corrosion inhibitor component comprises a long-acting vapor phase corrosion inhibitor and a short-acting vapor phase corrosion inhibitor; based on the mass of the corrosion inhibitor component as 100%, the mass percentage of the long-acting vapor phase corrosion inhibitor is 30wt% to 50wt%, and the mass percentage of the short-acting vapor phase corrosion inhibitor is 50wt% to 70wt%.

5. The composition according to claim 4, characterized in that, The long-acting vapor phase corrosion inhibitor is selected from one or two of acetaminophen and L-glutamine; the short-acting vapor phase corrosion inhibitor is selected from one or two of gallnut extract and garlic extract.

6. The composition according to claim 1, characterized in that, The volatile lubricant is selected from one or more of polyethylene glycol monomethyl ether, ethyl oleate, ethyl lactate, and ethyl acetate.

7. The composition according to claim 1, characterized in that, The porous adsorbent is selected from one or more of diatomaceous earth and fumed silica.

8. A method for preparing the composition according to any one of claims 1 to 7, characterized in that, Includes the following steps: (1) Preparation of corrosion inhibitor: The long-acting vapor phase corrosion inhibitor and the short-acting vapor phase corrosion inhibitor are mixed in proportion, ground and sieved to obtain corrosion inhibitor powder; (2) Preparation of lubricating components: After the volatile lubricant is mixed evenly, it is added to the porous adsorption carrier by atomization spraying. The adsorption is carried out at room temperature for 20 to 30 minutes, then taken out, ground and sieved to obtain porous adsorption carrier powder loaded with volatile lubricant. (3) Compounding: The corrosion inhibitor powder obtained in step (1) and the lubricating powder obtained in step (2) are mixed according to the ratio, ground and sieved to obtain the composition with both gas phase corrosion inhibition and lubrication functions.

9. The application of the composition according to any one of claims 1 to 7 in the corrosion protection and lubrication of copper alloys or copper metals in a marine atmospheric environment.

10. The application according to claim 9, characterized in that, The composition is placed directly in a closed or semi-closed cavity in powder form. After the vapor-phase corrosion inhibitor in the corrosion inhibitor component volatilizes, it is adsorbed together with the volatile lubricant in the lubricating component that volatilizes after being released by the porous adsorption carrier and forms a composite film layer on the metal surface, thereby achieving non-contact corrosion protection and lubrication and friction reduction for the moving parts in the cavity.

Citation Information

Patent Citations

  • A kind of plant type vapor phase copper corrosion inhibitor and preparation method thereof

    CN105200436B