A method for cleaning and smoothing the surface of ultrafine copper bonding wire
By combining activation, micro-etching, and alkaline washing with ultrasonic assistance, the problems of surface defects and organic residues in ultrafine copper bonding wires were solved, improving bonding quality and production efficiency, and meeting the high reliability requirements of electronic packaging.
Patent Information
- Application Number
- CN202611276545.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies cannot effectively remove processing defects and organic residues on the surface of ultrafine copper bonding wires without affecting production efficiency, resulting in a decline in bonding quality and affecting the reliability of electronic packaging.
The ultrafine copper bonding wires were treated using a combination of activation, micro-etching, and alkaline washing, with ultrasonic assistance throughout the process, followed by drying. The specific steps included using appropriate etchants and cleaning solutions, controlling the processing time and temperature to ensure rapid and uniform cleaning.
This technology achieves high cleanliness and flatness on the surface of ultrafine copper bonding wires, improving bonding quality and electronic packaging yield, reducing the requirements for drawing dies, and maintaining production efficiency.
Smart Images

Figure CN123132898A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of surface chemical subtractive cleaning process technology, specifically relating to a method for cleaning and smoothing the surface of ultrafine copper bonding wires. Background Technology
[0002] Ultrafine copper bonding wires, with diameters ranging from tens to hundreds of micrometers, are commonly used for wire bonding and are a key material for achieving high-density electronic packaging. The manufacturing of ultrafine copper wires requires clean casting, dozens or even hundreds of drawing passes, and final annealing, ultrasonic cleaning, and electroplating (optional). During the precision drawing process, drawing scratches are inevitably generated due to the contact between the drawing die and the copper wire. Simultaneously, organic lubricants are added during drawing, and some of these lubricants can enter the drawing scratches, causing surface contamination, such as… Figure 1 As shown.
[0003] Current cleaning methods using ultrasonic cleaning agents such as anhydrous ethanol can partially remove surface oil and impurities, but they cannot eliminate pulling marks and lubricants that have seeped into the surface, resulting in organic residue. Regardless of whether gold or palladium plating is subsequently applied, surface defects and organic residue will affect the burning and bonding quality of the bonding wire during use, leading to safety hazards and reduced reliability. While etchants with strong oxidizing and acidic properties can completely remove surface pulling defects and residues, they can easily cause excessive material reduction, such as... Figure 2 As shown.
[0004] In the surface treatment process of copper products, micro-etching and alkaline washing are common methods for removing surface oxide layers, oil stains, and impurities. Existing technologies have relatively mature process solutions for the surface treatment of copper foil. For example, patent CN118726978A discloses a micro-etching method for reducing the surface roughness of copper foil, which includes steps such as micro-etching and alkaline washing. The processing time is 3-8 minutes, and it is suitable for the surface treatment of sheet-like copper products such as copper foil. Due to the thinness and limited length of the copper foil, offline or batch processing methods can be used, and the longer processing time has a relatively controllable impact on overall production efficiency.
[0005] However, the geometry of ultrafine copper bonding wires differs fundamentally from that of copper foil. Bonding wires typically have diameters in the micrometer range, and individual wires can reach lengths of hundreds or even thousands of meters, exhibiting an overall slender shape. This structural characteristic dictates that surface treatment can only employ rapid, continuous online cleaning methods, with the wires sequentially passing through each processing station under the drive of a traction device. Excessive processing time significantly increases the wire's coiling time on the equipment, forcing a reduction in traction speed and severely impacting production efficiency. Therefore, the online cleaning time for bonding wires is usually controlled to within a few seconds, an order of magnitude difference compared to the several minutes required for copper foil processing. Furthermore, the specific surface area of microfine copper wires is far greater than that of copper foil of the same mass, resulting in higher surface activity and greater sensitivity to the concentration, temperature, and reaction time of the treatment solution. Achieving effective removal of the surface oxide layer and contaminants within an extremely short online processing time, while avoiding excessive corrosion that could lead to uneven wire diameter or deterioration of surface roughness, places extremely high demands on the speed, uniformity, and controllability of the processing technology. Existing copper foil surface treatment processes cannot meet the production efficiency requirements of ultra-fine copper wires.
[0006] Therefore, how to develop a surface chemical cleaning method that can be carried out by the current ultra-fine copper wire cleaning line without sacrificing production efficiency, so as to efficiently eliminate surface processing defects and residues of ultra-fine copper wire and achieve rapid, uniform and controllable cleaning treatment of the surface of micro-fine copper wire, is an urgent technical problem to be solved. Summary of the Invention
[0007] The main objective of this invention is to provide a method for making the surface of ultrafine copper bonding wire clean and smooth, so as to overcome the defects of the prior art.
[0008] To achieve the aforementioned objectives, the technical solution adopted by this invention includes: The first aspect of the present invention provides a method for cleaning and smoothing the surface of ultrafine copper bonding wires, comprising: The ultrafine copper bonding wire to be treated is activated, micro-etched and alkaline washed in sequence, and ultrasonic assistance is applied to the ultrafine copper bonding wire throughout the entire process. Finally, it is dried to achieve surface cleaning and smoothing of the ultrafine copper bonding wire.
[0009] A second aspect of the invention provides an ultrafine copper bonding wire obtained by the method.
[0010] Compared with the prior art, the present invention has at least the following beneficial effects: The method provided by this invention can be performed using existing bonding wire cleaning lines and is suitable for pure copper wires of various sizes, including high-purity copper bonding wires with diameters of 15-100 μm, and is particularly suitable for ultrafine copper alloy wires with diameters of 15-20 μm. Using this method, processing defects on the surface of ultrafine copper wires can be eliminated, while surface contamination and organic residues are removed, significantly improving the quality of ball bonding and sintering, ultimately increasing the yield and long-term reliability of electronic packaging, and reducing the requirements for ultrafine copper wire drawing dies.
[0011] The ultrafine copper bonding wire obtained by the method provided by this invention has ultra-high cleanliness and flatness, significantly improves the sintering and bonding quality, and the size of the ultrafine copper bonding wire remains basically unchanged before and after the treatment. Attached Figure Description
[0012] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0013] Figure 1 This is a surface morphology diagram of ultrafine copper bonding wire after drawing in the prior art; Figure 2 This is a surface morphology diagram of an ultrafine copper bonding wire that has been over-etched in the prior art; Figure 3 This is a surface morphology diagram of the ultrafine copper bonding wire after processing in Example 1 of the present invention; Figure 4 This is a surface morphology diagram of the ultrafine copper bonding wire after processing in Example 2 of the present invention; Figure 5 This is a surface morphology diagram of the ultrafine copper bonding wire after processing in Example 3 of the present invention; Figure 6 This is a surface morphology diagram of the ultrafine copper bonding wire after treatment in Comparative Example 1 of the present invention; Figure 7 This is a surface morphology diagram of the ultrafine copper bonding wire after treatment in Comparative Example 2 of the present invention; Figure 8 This is a surface morphology diagram of the ultrafine copper bonding wire after treatment in Comparative Example 3 of the present invention; Figure 9 This is a surface morphology diagram of the ultrafine copper bonding wire after treatment in Comparative Example 4 of this invention. Detailed Implementation
[0014] In view of the problems existing in the above-mentioned prior art, after in-depth research, a method for cleaning and smoothing the surface of ultrafine copper bonding wires is provided. This method mainly involves developing an etchant of moderate strength based on conventional etching techniques, combined with precise time control and appropriate pre- and post-processing, to eliminate surface processing defects and residues in the ultrafine copper wires without over-etching.
[0015] The following will provide a further explanation of the technical solution, its implementation process, and its principles.
[0016] The first aspect of the present invention provides a method for cleaning and smoothing the surface of ultrafine copper bonding wires, comprising: The ultrafine copper bonding wire to be treated is activated, micro-etched and alkaline washed in sequence, and ultrasonic assistance is applied to the ultrafine copper bonding wire throughout the entire process. Finally, it is dried to achieve surface cleaning and smoothing of the ultrafine copper bonding wire.
[0017] In some embodiments, the ultrafine copper bonding wire is a high-purity (99.999% purity) copper bonding wire with a diameter of 15~100 μm.
[0018] In some preferred embodiments, the ultrafine copper bonding wire is a high-purity copper bonding wire with a diameter of 15~20 μm.
[0019] In some implementations, the method specifically includes: unwinding an ultrafine copper bonding wire drawn to a target diameter and annealed, passing it sequentially through an activation zone, a micro-etching zone, and an alkaline washing zone, and performing ultrasonic assistance on the ultrafine copper bonding wire during the process, and finally drying and coiling the ultrafine copper bonding wire in a drying zone.
[0020] In some embodiments, the activation specifically includes: in the activation zone, the ultrafine copper bonding wire is activated at 40~60°C for 0.3~0.5 s using an activation zone cleaning solution; The activation zone cleaning solution includes a nitric acid-ethanol solution, wherein the concentration of nitric acid in the activation zone cleaning solution is 0.6~1.2 mol / L. Through activation treatment, most of the organic residue and surface oxide layer of the ultrafine copper bonding wire can be removed, exposing a fresh metal surface that can react rapidly with the etching solution in the next process.
[0021] In some embodiments, the micro-etching specifically includes: within the micro-etching zone, using a micro-etching zone etching solution to micro-etch the activated ultrafine copper bonding wire at 60~80℃ for 0.6~1.0 s.
[0022] Furthermore, the etching solution for the micro-etching area is a sulfuric acid solution containing a strong oxidant, wherein the concentration of the sulfuric acid solution in the micro-etching area etching solution is 0.7~1.5 mol / L, and the concentration of the strong oxidant in the micro-etching area etching solution is 1.0~2.0 mol / L; The strong oxidizing agent includes at least one of permanganate, dichromate, hypochlorite, chlorite, chlorate, and perchlorate, and the metal ion of the salt includes sodium or potassium. Through micro-etching, a rapid redox reaction can be achieved on the surface of the ultrafine copper bonding wire, especially at scratches and indentations, thus eliminating surface defects in the ultrafine copper bonding wire.
[0023] In some implementations, the alkaline washing specifically includes: in the alkaline washing zone, using an alkaline washing zone cleaning solution to perform alkaline washing treatment on the micro-etched ultrafine copper bonding wire at 30~50℃ for 0.3~0.5 s; The alkaline washing solution is an aqueous solution containing an alkaline substance, including KOH or NaOH, with a concentration of 0.5~1.5 mol / L. Alkaline washing eliminates potential etching solution residues and prevents re-oxidation or localized oxidation of the ultrafine copper bonding wires by the acidic etching solution during micro-etching.
[0024] In some embodiments, the ultrasonic assistance specifically includes: during the activation, micro-etching, and alkaline washing processes, applying ultrasonic power of 10-30W to the ultrafine copper bonding wire. Ultrasonic assistance accelerates the detachment of substances from the surface of the ultrafine copper bonding wire in each processing step, thus speeding up the reaction rate.
[0025] In some embodiments, the drying specifically includes: drying the alkaline-washed ultrafine copper bonding wire at a temperature of 50-80 ºC for 2-4 seconds in a nitrogen-hydrogen mixed atmosphere; wherein the nitrogen-hydrogen mixed atmosphere is a mixture of nitrogen and hydrogen, and the volume fraction ratio of nitrogen to hydrogen is 90-95%:5-10%. This drying process prevents the ultrafine copper bonding wire from being re-oxidized and also avoids the residue of cleaning solution in the alkaline washing zone.
[0026] In some more specific implementations, the method specifically includes the following steps: The ultrafine copper bonding wire, drawn to the target diameter and annealed, is unwound and sequentially passed through an activation zone, a micro-etching zone, and an alkaline washing zone. During each of these processes, the ultrafine copper bonding wire undergoes ultrasonic-assisted treatment at a power of 10-30W. Finally, it is dried in a drying zone and coiled into a roll. The activation zone uses a nitric acid-ethanol solution for cleaning, with a passage time of 0.3-0.5 seconds and a processing temperature of 40-60 °C. The micro-etching zone uses a sulfuric acid solution with added strong oxidant, with a passage time of 0.6-1.0 seconds and a processing temperature of 60-80 °C. The alkaline washing zone uses a KOH or NaOH aqueous solution, with a passage time of 0.3-0.5 seconds and a processing temperature of 30-50 °C. Under precise tension control, the finished wire is rewound onto a spool for final inspection of dimensions and surface defects. Only qualified wires are released from the warehouse.
[0027] A second aspect of the invention provides an ultrafine copper bonding wire obtained by the method.
[0028] The technical solution of the present invention will be further described below with reference to the embodiments. Where specific experimental steps or conditions are not specified in the embodiments, they can be performed according to the conventional experimental steps or conditions described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available. Other unmentioned raw materials and instruments are all conventionally selected and do not involve the core technical means of the present invention.
[0029] Example 1 Unwind the annealed copper bonding wire with a diameter of 18 μm. The process involves passing through an activation zone, where the cleaning solution is a nitric acid-ethanol solution with a nitric acid concentration of 0.8 mol / L. The process takes 0.4 seconds and is carried out at a temperature of 50 °C. The etching process involves passing through a micro-etching zone. The etching solution in the micro-etching zone is a sulfuric acid solution with added strong oxidant, sodium hypochlorite. The concentration of the strong oxidant in the etching solution in the micro-etching zone is 1.5 mol / L, and the concentration of H2SO4 solution in the etching solution in the micro-etching zone is 1.0 mol / L. The passage time is 0.8 seconds, and the micro-etching treatment temperature is 70 ℃. The alkaline washing zone uses NaOH aqueous solution with a concentration of 0.9 mol / L, a transit time of 0.5 seconds, and an alkaline washing temperature of 35 ℃. Ultrasonic-assisted treatment: The copper bonding wires are ultrasonically treated with a power of 20 W throughout the entire process of activation zone, micro-etching zone and alkaline washing zone. Finally, the wire is dried and coiled in a drying zone at 60 ºC for 3 seconds in a nitrogen-hydrogen mixture (95% N2 + 5% H2 by volume). The surface morphology of the obtained copper bonding wire is as follows. Figure 3 As shown. Compared to Figure 1The surface morphology of the ultrafine copper bonding wire after drawing is shown in this embodiment. The surface morphology of the copper bonding wire after treatment has extremely high cleanliness and smoothness. Compared with the copper bonding wire before treatment, the diameter of the copper bonding wire remains basically unchanged, at approximately 18 μm.
[0030] Example 2 Unwind the annealed copper bonding wire with a diameter of 20 μm. The process involves passing through an activation zone, where the cleaning solution is a nitric acid-ethanol solution with a nitric acid concentration of 0.9 mol / L. The process takes 0.35 seconds and is carried out at a temperature of 45 °C. The etching process involved passing through a micro-etching zone. The etching solution in the micro-etching zone was a sulfuric acid solution with added strong oxidant, potassium permanganate, and the concentration of the strong oxidant in the etching solution was 1.2 mol / L. The concentration of H2SO4 solution in the etching solution was also 1.2 mol / L. The passage time was 0.7 seconds, and the micro-etching temperature was 60 ℃. The alkaline washing zone uses KOH aqueous solution with a concentration of 0.8 mol / L, a transit time of 0.4 seconds, and an alkaline washing temperature of 45 ℃. Ultrasonic-assisted treatment: The copper bonding wires are ultrasonically treated with a power of 15 W throughout the entire process of activation zone, micro-etching zone and alkaline washing zone. Finally, the coils are dried and wound in a drying zone at a temperature of 70 ºC for 2.5 s in an atmosphere of nitrogen-hydrogen mixture (90% N2 + 10% H2 by volume).
[0031] The surface morphology of the copper bonding wire is obtained as follows Figure 4 As shown. Compared to Figure 1 The surface morphology of the ultrafine copper bonding wire after drawing is shown in this embodiment. The surface morphology of the copper bonding wire after treatment has extremely high cleanliness and smoothness. Compared with the copper bonding wire before treatment, the diameter of the copper bonding wire remains basically unchanged, at approximately 20 μm.
[0032] Example 3 Unwind the annealed copper bonding wire with a diameter of 20 μm. The process involves passing through an activation zone, where the cleaning solution is a nitric acid-ethanol solution with a nitric acid concentration of 0.7 mol / L. The process takes 0.5 seconds and is carried out at a temperature of 60 °C. The etching process involves passing through a micro-etching zone. The etching solution in the micro-etching zone is a sulfuric acid solution with added strong oxidant, potassium chlorate. The concentration of the strong oxidant in the etching solution in the micro-etching zone is 2.0 mol / L, and the concentration of H2SO4 solution in the etching solution in the micro-etching zone is 1.4 mol / L. The passage time is 1.0 second, and the micro-etching treatment temperature is 75 ℃. The alkaline washing zone uses NaOH aqueous solution with a concentration of 0.7 mol / L, a transit time of 0.5 seconds, and an alkaline washing temperature of 45 ℃. Ultrasonic-assisted treatment: The copper bonding wires are ultrasonically treated with a power of 25 W throughout the entire process of activation zone, micro-etching zone and alkaline washing zone. Finally, the coils are dried and wound in a drying zone at a temperature of 80 ºC for 3 seconds in a nitrogen-hydrogen mixture (92% N2 + 8% H2 by volume).
[0033] The surface morphology of the copper bonding wire is obtained as follows Figure 5 As shown. Compared to Figure 1 The surface morphology of the ultrafine copper bonding wire after drawing is shown in this embodiment. The surface morphology of the copper bonding wire after treatment has extremely high cleanliness and smoothness. Compared with the copper bonding wire before treatment, the diameter of the copper bonding wire remains basically unchanged, at approximately 20 μm.
[0034] Example 4 Unwind the annealed copper bonding wire with a diameter of 15 μm. The process involves passing through an activation zone where the cleaning solution is a nitric acid-ethanol solution with a nitric acid concentration of 0.6 mol / L. The process takes 0.5 seconds and is carried out at a temperature of 60 °C. The etching process involves passing through a micro-etching zone. The etching solution in the micro-etching zone is a sulfuric acid solution with added strong oxidant, sodium chlorite. The concentration of the strong oxidant in the etching solution in the micro-etching zone is 1 mol / L, and the concentration of H2SO4 solution in the etching solution in the micro-etching zone is 1.2 mol / L. The passage time is 1 second, and the micro-etching treatment temperature is 80 ℃. The alkaline washing zone uses NaOH aqueous solution with a concentration of 0.5 mol / L, a transit time of 0.5 seconds, and an alkaline washing temperature of 50 ℃. Ultrasonic-assisted treatment: The copper bonding wires are ultrasonically treated with a power of 30 W throughout the entire process of activation zone, micro-etching zone and alkaline washing zone. Finally, the coils are dried and wound in a drying zone at a temperature of 50 ºC for 4 seconds in a nitrogen-hydrogen mixture (92% N2 + 8% H2 by volume).
[0035] The copper bonding wire treated in this embodiment exhibits extremely high cleanliness and smoothness. Compared to the copper bonding wire before treatment, its diameter remains essentially unchanged, approximately 15 μm.
[0036] Example 5 Unwind the annealed copper bonding wire with a diameter of 50 μm. The process involves passing through an activation zone, where the cleaning solution is a nitric acid-ethanol solution with a nitric acid concentration of 1 mol / L. The process takes 0.5 seconds and is carried out at a temperature of 55 °C. The etching process involved passing through a micro-etching zone. The etching solution in the micro-etching zone was a sulfuric acid solution with added strong oxidant, sodium perchlorate. The concentration of the strong oxidant in the etching solution in the micro-etching zone was 1.7 mol / L, and the concentration of H2SO4 solution in the etching solution in the micro-etching zone was 0.7 mol / L. The passage time was 0.8 seconds, and the micro-etching treatment temperature was 65 ℃. The alkaline washing zone uses NaOH aqueous solution with a concentration of 1.2 mol / L, a transit time of 0.4 seconds, and an alkaline washing temperature of 45 ℃. Ultrasonic-assisted treatment: The copper bonding wires are ultrasonically treated with a power of 10 W throughout the entire process of activation zone, micro-etching zone and alkaline washing zone. Finally, the coils are dried and wound in a drying zone at a temperature of 50 ºC for 4 seconds in a nitrogen-hydrogen mixture (94% N2 + 6% H2 by volume).
[0037] The copper bonding wire treated in this embodiment exhibits extremely high cleanliness and smoothness. Compared to the copper bonding wire before treatment, its diameter remains essentially unchanged, approximately 50 μm.
[0038] Example 6 Unwind the annealed copper bonding wire with a diameter of 100 μm. The process involves passing through an activation zone where the cleaning solution is a nitric acid-ethanol solution with a nitric acid concentration of 1.2 mol / L. The process takes 0.3 seconds and is carried out at a temperature of 40 °C. The etching process involves passing through a micro-etching zone. The etching solution in the micro-etching zone is a sulfuric acid solution with added strong oxidant, sodium dichromate. The concentration of the strong oxidant in the etching solution in the micro-etching zone is 2 mol / L, and the concentration of H2SO4 solution in the etching solution in the micro-etching zone is 1.5 mol / L. The passage time is 0.6 seconds, and the micro-etching treatment temperature is 60 ℃. The alkaline washing zone uses NaOH aqueous solution with a concentration of 1.5 mol / L, a transit time of 0.3 seconds, and an alkaline washing temperature of 30 ℃. Ultrasonic-assisted treatment: The copper bonding wires are ultrasonically treated with a power of 20 W throughout the entire process of activation zone, micro-etching zone and alkaline washing zone. Finally, the coils are dried in a drying zone at a temperature of 50 ºC for 3 seconds in a nitrogen-hydrogen mixture (95% N2 + 5% H2 by volume).
[0039] The copper bonding wire treated in this embodiment exhibits extremely high cleanliness and smoothness. Compared to the copper bonding wire before treatment, its diameter remains essentially unchanged, approximately 100 μm.
[0040] Comparative Example 1 The difference between this comparative example and Example 1 is that the copper bonding wire does not pass through the activation region, while the remaining steps are the same as in Example 1.
[0041] The copper bonding wire obtained in this comparative example has poor surface etching uniformity, and the surface morphology of the copper bonding wire is as follows: Figure 6 As shown.
[0042] Comparative Example 2 The difference between this comparative example and Example 1 is that the copper bonding wire does not pass through the micro-etching area, while the remaining steps are the same as in Example 1.
[0043] The surface processing defects of the copper bonding wire obtained in this comparative example were basically not eliminated; drawing scratches still existed. The surface morphology of the copper bonding wire was as follows: Figure 7 As shown.
[0044] Comparative Example 3 The difference between this comparative example and Example 1 is that the copper bonding wire does not pass through the alkaline washing zone, while the remaining steps are the same as in Example 1.
[0045] The copper bonding wire obtained in this comparative example has oxidation caused by etchant residue on its surface. The surface morphology of the copper bonding wire is as follows: Figure 8 As shown.
[0046] Comparative Example 4 The difference between this comparative example and Example 1 is that the copper bonding wire is not subjected to ultrasonic-assisted treatment, while the remaining steps are the same as in Example 1.
[0047] The final copper bonding wire etched in this comparative example showed poor surface cleanliness and defect removal, with the surface morphology of the copper bonding wire as follows: Figure 9 As shown.
[0048] In addition, the present invention has also conducted experiments with other raw materials, process operations and process conditions described in this specification, with reference to the foregoing embodiments, and has obtained relatively ideal results in all cases.
[0049] Although the invention has been described with reference to illustrative embodiments, those skilled in the art will understand that various other changes, omissions, and / or additions can be made without departing from the spirit and scope of the invention, and that elements of the embodiments can be substituted with substantially equivalents. Furthermore, many modifications can be made without departing from the scope of the invention to adapt particular situations or materials to the teachings of the invention. Therefore, this invention is not intended to be limited to the specific embodiments disclosed for carrying out the invention, but rather is intended to encompass all embodiments falling within the scope of the appended claims. Moreover, unless specifically stated otherwise, any use of the terms first, second, etc., does not indicate any order or importance, but is used to distinguish one element from another.
Claims
1. A method for cleaning and smoothing the surface of ultrafine copper bonding wire, characterized in that, include: The ultrafine copper bonding wire to be treated is activated, micro-etched and alkaline washed in sequence, and ultrasonic assistance is applied to the ultrafine copper bonding wire throughout the entire process. Finally, it is dried to achieve surface cleaning and smoothing of the ultrafine copper bonding wire.
2. The method according to claim 1, characterized in that: The ultrafine copper bonding wire is a high-purity copper bonding wire with a diameter of 15~100 μm.
3. The method according to claim 1, characterized in that, Specifically, it includes: The ultrafine copper bonding wire, drawn to the target diameter and annealed, is unwound and passed sequentially through the activation zone, micro-etching zone, and alkaline washing zone. During the process, the ultrafine copper bonding wire is subjected to ultrasonic assistance. Finally, the ultrafine copper bonding wire is dried in the drying zone and coiled.
4. The method according to any one of claims 1-3, characterized in that, The activation specifically includes: in the activation zone, the ultrafine copper bonding wire is activated at 40~60 ℃ for 0.3~0.5 s using an activation zone cleaning solution; The cleaning solution for the activation zone includes a nitric acid ethanol solution, wherein the concentration of nitric acid in the cleaning solution for the activation zone is 0.6~1.2 mol / L.
5. The method according to any one of claims 1-3, characterized in that, The micro-etching specifically includes: within the micro-etching zone, using a micro-etching zone etching solution to perform micro-etching treatment on the activated ultrafine copper bonding wire at 60~80 ℃ for 0.6~1.0 s.
6. The method according to claim 5, characterized in that: The etching solution for the micro-etching area is a sulfuric acid solution containing a strong oxidant. The concentration of the sulfuric acid solution in the micro-etching area etching solution is 0.7~1.5 mol / L, and the concentration of the strong oxidant in the micro-etching area etching solution is 1.0~2.0 mol / L. The strong oxidizing agent includes at least one of permanganate, dichromate, hypochlorite, chlorite, chlorate, and perchlorate, and the metal ion of the salt includes sodium or potassium.
7. The method according to any one of claims 1-3, characterized in that, The alkaline washing specifically includes: in the alkaline washing zone, using the alkaline washing zone cleaning solution to perform alkaline washing treatment on the micro-etched ultrafine copper bonding wire at 30~50℃ for 0.3~0.5 s; The cleaning solution in the alkaline washing zone is an aqueous solution containing alkaline substances, including KOH or NaOH, and the concentration of the alkaline substances in the cleaning solution in the alkaline washing zone is 0.5~1.5 mol / L.
8. The method according to any one of claims 1-3, characterized in that, The ultrasonic assistance specifically includes: during the activation, micro-etching and alkaline washing processes, ultrasonic assistance is applied to the ultrafine copper bonding wire using a power of 10~30 W.
9. The method according to any one of claims 1-3, characterized in that, The drying process specifically includes: drying the alkaline-washed ultrafine copper bonding wire at a temperature of 50~80 ºC for 2~4 s in a nitrogen-hydrogen mixed atmosphere in a drying zone; wherein the nitrogen-hydrogen mixed atmosphere is a mixture of nitrogen and hydrogen, and the volume fraction ratio of nitrogen to hydrogen is 90~95%:5~10%.
10. The ultrafine copper bonding wire obtained by the method of any one of claims 1-9.
Citation Information
Patent Citations
Process for reducing surface roughness of copper foil
CN118726978A