Preparation method and application of palladium-doped ruthenium oxide oxygen evolution electrocatalyst

By introducing palladium into the ruthenium oxide lattice and dynamically adjusting the oxygen species and ruthenium valence state, the problem of insufficient stability of ruthenium oxide-based catalysts at high current densities was solved, achieving efficient and economical electrocatalytic performance.

CN123132935APending Publication Date: 2026-11-20EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611479895.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing ruthenium oxide-based catalysts are prone to over-oxidation, lattice oxygen loss, and ruthenium dissolution under strong acid, high potential, and high current density conditions, leading to performance degradation and making it difficult to balance activity and stability.

Method used

By uniformly introducing palladium into the ruthenium oxide lattice, the local oxygen species and ruthenium valence state are dynamically adjusted to form a dynamic oxygen buffer effect, which inhibits excessive oxidation and dissolution of ruthenium.

Benefits of technology

A non-iridium anode electrocatalyst that achieves long-term stable operation at high current density has been developed. It exhibits excellent acidic oxygen evolution activity and good stability, and its preparation method is simple and inexpensive.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123132935A_ABST
    Figure CN123132935A_ABST
Patent Text Reader

Abstract

This invention provides a method for preparing and applying a palladium-doped ruthenium oxide oxygen evolution electrocatalyst. Palladium is uniformly introduced into the ruthenium oxide lattice, maintaining the overall ruthenium oxide crystal structure. During the oxygen evolution reaction, palladium sites preferentially undergo redox reactions and oxygen coordination changes, dynamically regulating local oxygen species and buffering the evolution of ruthenium valence states, thus endowing ruthenium oxide with a dynamic oxygen buffering effect, thereby inhibiting excessive oxidation and dissolution of ruthenium. The PdRuO prepared by this invention... x It exhibits both excellent acidic oxygen evolution activity and long-term stability. In a three-electrode system, 100 mA / cm²... 2 Stable operation for 1000 hours at current density; used as an anode material (2 mg / cm³). 2 The assembled proton exchange membrane electrolyzer achieved 3 A / cm at a cell voltage of 1.694 V. 2 The current density is at 1 A / cm 2 The material maintained operation for 200 hours without significant degradation, providing a practical and feasible technical route for the application of highly stable ruthenium-based non-iridium anode materials in proton exchange membrane water electrolysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrochemical catalysis technology, specifically relating to the preparation method and application of a palladium-doped ruthenium oxide oxygen evolution electrocatalyst with dynamic oxygen buffering effect. Background Technology

[0002] Proton exchange membrane (PEM) water electrolysis boasts advantages such as high current density, compact structure, and good safety, making it a crucial technology for green hydrogen production. Currently, its anodes primarily rely on iridium-based catalysts. However, iridium resources are scarce and expensive, and the membrane electrode assembly requires a high iridium loading, making it difficult to meet the demands of large-scale applications. Therefore, finding alternatives to iridium is urgently needed. Ruthenium oxide exhibits excellent acidic oxygen evolution activity and is a highly promising non-iridium anode material. However, under conditions of strong acid, high potential, and high current density, ruthenium sites are prone to over-oxidation, lattice oxygen loss, and ruthenium dissolution, leading to catalyst performance degradation.

[0003] To address the aforementioned technical challenges, existing research has actively explored various approaches to improve ruthenium oxide stability, primarily through heteroelement doping, regulating metal-oxygen bonds, suppressing lattice oxygen participation, or altering reaction pathways. However, these methods typically treat dopant elements as static structural or electronically modulating components, neglecting their valence states and oxygen coordination responses under water-rich and high-potential environments. Furthermore, due to the continuous changes in surface oxygen species during the oxygen evolution reaction, traditional static control methods struggle to balance activity and stability. Therefore, there is an urgent need to develop ruthenium oxide-based catalytic materials capable of dynamically regulating local oxygen species, suppressing excessive ruthenium oxidation, and readily scalable for large-scale preparation. Summary of the Invention

[0004] This invention addresses the aforementioned problems by providing a method for preparing and applying a palladium-doped ruthenium oxide oxygen evolution electrocatalyst with a dynamic oxygen buffering effect, thus solving the problem of insufficient stability of ruthenium-based catalysts. This catalyst material offers good economic efficiency, high oxygen evolution activity, and good stability. The preparation method is simple and it has significant application potential.

[0005] The technical principle of this invention is as follows: Palladium is uniformly introduced into the ruthenium oxide lattice, and the material as a whole maintains the ruthenium oxide crystal structure. During the oxygen evolution reaction, the palladium sites preferentially undergo redox and oxygen coordination changes, dynamically regulating local oxygen species and buffering the evolution of ruthenium valence state, thus endowing ruthenium oxide with a dynamic oxygen buffering effect, thereby inhibiting excessive oxidation and dissolution of ruthenium.

[0006] Based on the above research, the technical solution adopted in this invention is as follows:

[0007] In a first aspect, the present invention provides a method for preparing a palladium-doped ruthenium oxide oxygen evolution electrocatalyst, comprising the following steps:

[0008] (1) Dissolve hydrated ruthenium chloride in deionized water to form a precursor solution with a concentration of 10 g / L;

[0009] (2) Mix palladium salt, sodium nitrate and potassium nitrate with the solution in step (1), dissolve them in anhydrous ethanol and water to form a solution, and stir magnetically for 20 to 50 minutes;

[0010] (3) Remove the solvent from the mixed solution obtained in step (2) by rotary evaporation at 60~80℃ (preferably 70℃), and dry it in a vacuum oven at 55~65℃ (preferably 60℃) for 10~14 hours;

[0011] (4) Place the gray-green powder obtained in step (3) in a muffle furnace at 320~400℃ (preferably 360℃) for 20~40 minutes, and then take it out and cool it to room temperature in the air.

[0012] (5) The black product obtained in step (4) is washed multiple times with deionized water and anhydrous ethanol, and finally dried in a vacuum oven at 55~65℃ (preferably 60℃) for 10~14 hours.

[0013] (6) Transfer the black powder obtained in step (5) to a quartz crucible and calcine it in a muffle furnace at 400°C for 4 to 6 hours.

[0014] Preferably, in step (1), ruthenium chloride hydrate is selected from ruthenium trichloride hydrate; a compound formed by the combination of ruthenium trichloride (RuCl3) and an indefinite number of water molecules (xH2O), the chemical formula of which is usually written as RuCl3·xH2O.

[0015] In step (2), the palladium salt is selected from any one of palladium chloride, palladium nitrate, palladium sulfate, tetrachloropalladium salt and tetraamminepalladium salt, with palladium chloride and palladium nitrate being preferred.

[0016] Furthermore, the mass ratio between palladium salt and hydrated ruthenium chloride is 1~4:16~17; the mass ratio between sodium nitrate and potassium nitrate is 3:2; and the mass ratio between palladium salt and sodium nitrate is 5~24:1.

[0017] Furthermore, the ratio between anhydrous ethanol and water is not limited, but is determined by the ability to dissolve palladium salt. It is preferred to have more ethanol and less water to facilitate subsequent rotary evaporation to remove the solvent.

[0018] In a second aspect, the present invention provides a palladium-doped ruthenium oxide oxygen evolution electrocatalyst PdRuO prepared by the above method. x .

[0019] The obtained product was characterized by X-ray diffraction patterns, which showed that PdRuO x The characteristic diffraction peaks at angles of 27.8°, 35.2°, and 54.5° correspond to the (1 1 0), (1 0 1), and (2 1 1) crystal planes of ruthenium oxide (PdRuO) crystals. xNo new crystalline phase was formed; SEM and TEM results showed that its microstructure exhibited a plate-like structure formed by the accumulation of nanoparticles, with the catalyst mainly exposing the (2 1 0), (1 0 1), and (2 1 1) crystal planes. PdRuO x It maintains good ruthenium oxide lattice characteristics.

[0020] Performance testing results show that, under positive conditions, palladium responds more significantly to anodic oxidation, while the valence state change of ruthenium is largely buffered, inhibiting ruthenium peroxidation. Compared to commercially available ruthenium oxide materials, the PdRuO prepared in this invention exhibits superior performance. x The required potential conditions to achieve the same current density are lower, and the current density operation is more stable.

[0021] Furthermore, PdRuO was tested using a proton exchange membrane electrolyzer system. x Electrocatalytic performance of PdRuO x The material was used as an anode catalyst in a proton exchange membrane water electrolyzer, demonstrating an electrode material efficiency of 3 A / cm in the proton exchange membrane electrolyzer. 2 The battery voltage was only 1.694 V, indicating that PdRuO x The material exhibits high catalytic activity under high current density in a proton exchange membrane electrolyzer and can operate efficiently and stably for more than 200 hours without significant degradation.

[0022] Based on this, in a third aspect, the present invention provides the application of palladium-doped ruthenium oxide oxygen evolution electrocatalyst, specifically its application in the preparation of electrocatalytic oxygen evolution reaction materials and proton exchange membrane electrolyzer anode materials.

[0023] In a fourth aspect, the present invention provides an electrocatalytic oxygen evolution reaction apparatus, wherein the above-mentioned palladium-doped ruthenium oxide oxygen evolution electrocatalyst is loaded on the working electrode.

[0024] The preferred preparation method is as follows: Weigh the catalyst PdRuO x The powder was dispersed in isopropanol and deionized water, and then 5 wt.% Nafion® solution was added. The catalyst slurry was ultrasonically dispersed at 30°C using an ultrasonic cleaner. Subsequently, the catalyst slurry was drop-coated onto a glassy carbon electrode and allowed to air dry to obtain the working electrode.

[0025] In a fifth aspect, the present invention provides a proton exchange membrane electrolyzer anode, comprising a carrier and an anode material loaded on the carrier in a certain manner, wherein the anode material comprises the above-mentioned palladium-doped ruthenium oxide oxygen evolution electrocatalyst.

[0026] The preferred preparation method is as follows: The catalyst is dispersed in a mixed solution of isopropanol and deionized water in a certain proportion. Then, 5 wt% Nafion® solution is added, and the mixture is ultrasonically crushed in a low-temperature water bath to obtain a homogeneous catalyst slurry. The anode catalyst slurry is then directly sprayed onto both sides of a Gore proton exchange membrane. After drying, the resulting membrane electrode material is hot-pressed at 140°C and 2 tons of pressure for 2-3 minutes.

[0027] In a sixth aspect, the present invention provides a proton exchange membrane electrolyzer containing the anode described in the fifth aspect above.

[0028] The role and effect of invention

[0029] (1) To date, most ruthenium oxide-based acidic oxygen evolution electrocatalysts mainly rely on static doping regulation, which is difficult to cope with the continuously changing surface oxygen environment during actual proton exchange membrane water electrolysis. This invention proposes a dynamic oxygen buffering mechanism mediated by oxygen-responsive palladium sites. By preferentially generating palladium valence state and oxygen coordination response, the ruthenium valence state is stabilized and its excessive oxidation and dissolution are suppressed, thereby obtaining a non-iridium anode electrocatalyst that can operate stably for a long time at high current densities.

[0030] (2) PdRuO prepared using the present invention x It exhibits both excellent acidic oxygen evolution activity and long-term stability. In a three-electrode system, 100 mA / cm²... 2 Stable operation for 1000 hours at current density; used as an anode material (2 mg / cm³). 2 The assembled proton exchange membrane electrolyzer achieved 3 A / cm at a cell voltage of 1.694 V. 2 The current density is at 1 A / cm 2 The material maintained operation for 200 hours without significant degradation, providing a practical and feasible technical route for the application of highly stable ruthenium-based non-iridium anode materials in proton exchange membrane water electrolysis.

[0031] (3) The preparation method of the present invention is simple, practically operable, low in cost, environmentally friendly in terms of raw materials, reduces the use of harmful solvents, has low energy consumption in the reaction process, short reaction steps, and is easy to scale up industrially. Attached Figure Description

[0032] Figure 1 The X-ray diffraction patterns are shown for the materials in Examples 1, 2, and Comparative Example 1, where Example 1 is the prepared PdRuO x Materials: Example 2 is the prepared RuO2 material, and Comparative Example 1 is a commercially available ruthenium oxide material.

[0033] Figure 2 PdRuO prepared in Example 1 x Scanning electron micrograph of the material.

[0034] Figure 3 PdRuO prepared in Example 1 x Aberration-corrected high-angle annular dark-field scanning transmission microscope image of the material.

[0035] Figure 4 PdRuO prepared in Examples 1, 2, and 3 x The in-situ X-ray absorption near-edge structure spectra of the palladium K-edge and ruthenium K-edge are shown in the image, along with their magnified images. Comparative Example 2 shows PdRuO2 after applying a voltage of 1.3 V. x Material, Comparative Example 3 is PdRuO after applying a voltage of 1.5 V. x Material.

[0036] Figure 5 The figures show the linear sweep voltammetry curves of the materials in Examples 1 and 2 and Comparative Example 1 in the three-electrode testing system, where Example 1 is the prepared PdRuO x Materials: Example 2 is the prepared RuO2 material, and Comparative Example 1 is a commercially available ruthenium oxide material.

[0037] Figure 6 Examples 1, 2, and Comparative Example 1 in the three-electrode test system were tested at a current density of 100 mA cm⁻¹. −2 The constant current curves at various times are shown, with Example 1 being the prepared PdRuO. x Materials: Example 2 is the prepared RuO2 material, and Comparative Example 1 is a commercially available ruthenium oxide material.

[0038] Figure 7 PdRuO prepared in Example 1 x Current density-voltage curves of the material used as an anode catalyst in a proton exchange membrane water electrolysis device.

[0039] Figure 8 PdRuO prepared in Example 1 x The materials and Example 2 use the prepared RuO2 material as the anode catalyst for proton exchange membrane water electrolysis at a current density of 1 A cm⁻¹. −2 The constant current curve at that time. Detailed Implementation

[0040] Experimental methods in the following examples, unless otherwise specified, are generally performed under standard conditions or as recommended by the manufacturer. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of skill in the art. Furthermore, any methods and materials similar or equivalent to those described herein may be used in this invention. The preferred embodiments and materials described herein are for illustrative purposes only.

[0041] The "range" disclosed in this document takes the form of a lower limit and an upper limit. It can be one or more lower limits and one or more upper limits, respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower and upper limits define the boundaries of the particular range. All ranges that can be defined in this way are inclusive and composable; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60–120 and 80–110 are listed for a specific parameter, it is expected that ranges of 60–110 and 80–120 are also expected. Furthermore, if the minimum range values ​​are listed as 1 and 2, and if the maximum ranges are listed as 3, 4, and 5, then the following ranges are all expected: 1–2, 1–4, 1–5, 2–3, 2–4, and 2–5.

[0042] In this invention, unless otherwise specified, the numerical range "a~b" represents an abbreviation of any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0~5" means that all real numbers between "0~5" have been listed in this document, and "0~5" is simply an abbreviation of these numerical combinations.

[0043] In this invention, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined to form new technical solutions.

[0044] In this invention, unless otherwise specified, all the technical features and preferred features mentioned herein can be combined to form new technical solutions.

[0045] The preferred embodiments of the present invention will be described in detail below with reference to specific examples. However, it should be understood that those skilled in the art can make reasonable changes, improvements and combinations to these embodiments without departing from the scope defined by the claims, thereby obtaining new specific implementation methods. These new specific implementation methods obtained through changes, improvements and combinations are also included within the protection scope of the present invention.

[0046] I. Preparation and Application of Palladium-Doped Ruthenium Oxide Evolution Electrocatalyst with Dynamic Oxygen Buffering Effect

[0047] Example 1

[0048] 1. Preparation of palladium-doped ruthenium oxide oxygen evolution electrocatalyst with dynamic oxygen buffering effect

[0049] (1) Dissolve 166 mg of ruthenium trichloride hydrate in 16.6 ml of deionized water to form a precursor solution;

[0050] (2) Mix 20 mg palladium chloride, 1.6988 g sodium nitrate and 1.1325 g potassium nitrate with the solution in step (1), dissolve in anhydrous ethanol and water to form a solution, and stir magnetically for 30 minutes;

[0051] (3) Remove the solvent from the mixed solution obtained in step (2) by rotary evaporation at 70°C, and dry it in a vacuum oven at 60°C for 12 hours;

[0052] (4) Place the gray-green powder obtained in step (3) in a muffle furnace at 360°C for 30 minutes, and then take it out and cool it to room temperature in the air.

[0053] (5) The black product obtained in step (4) was washed multiple times with deionized water and anhydrous ethanol, and finally dried in a vacuum oven at 60°C for 12 hours.

[0054] (6) Transfer the black powder obtained in step (5) to a quartz crucible and calcine it in a muffle furnace at 400°C for 5 hours.

[0055] 2. Application of palladium-doped ruthenium oxide oxygen evolution electrocatalysts with dynamic oxygen buffering effect in electrocatalytic oxygen evolution reactions.

[0056] PdRuO was tested using a three-electrode system. x The electrocatalytic oxygen evolution performance was assessed. Using a silver / silver chloride electrode as the reference electrode and a platinum mesh as the counter electrode, 5 mg of catalyst powder was added to 460 μL of isopropanol, followed by 40 μL of 5 wt.% Nafion® solution. The mixture was sonicated for 30 minutes to obtain a uniformly dispersed catalyst slurry. 5 μL of this slurry was then drop-coated onto a glassy carbon electrode using a microsyringe and allowed to air dry to obtain the working electrode. The electrolyte solution was 0.5 M H₂SO₄ solution, and the test temperature was 25°C. The activity of the material was evaluated using a CHI 760E electrochemical workstation via linear sweep voltammetry at a scan rate of 5 mV / s. −1 .

[0057] 3. Application of palladium-doped ruthenium oxide oxygen evolution electrocatalyst with dynamic oxygen buffering effect in proton exchange membrane oxygen evolution reaction.

[0058] The electrocatalytic performance of PdRuOx was tested using a proton exchange membrane electrolyzer system. PdRuOx powder was used as the anode catalyst, and commercially available 40 wt% Pt / C powder was used as the cathode catalyst. 30 mg of the powdered catalyst from Example 1 was weighed and added to a mixture of isopropanol and deionized water containing 162 μL of 5 wt% Nafion® solution to prepare the anode catalyst slurry. 8 mg of commercially available 40% Pt / C was then weighed and added to a mixture of isopropanol and deionized water containing 43 μL of 5 wt% Nafion® solution to prepare the cathode catalyst slurry. Both slurries were ultrasonically crushed in a low-temperature water bath for 30 minutes to obtain a homogeneous catalyst slurry. The anode and cathode catalyst slurries were then directly sprayed onto both sides of a Gore proton exchange membrane. After drying, the resulting membrane electrode material was hot-pressed at 140°C and 2 tons of pressure for 2 minutes. The anode catalyst loading was 2 mg / cm³. 2 The porous transport layers for the anode and cathode were made of titanium plates and carbon paper, respectively. The prepared porous transport layers for the anode and cathode, along with the membrane electrode materials, were assembled into a proton exchange membrane electrolyzer for testing. Electrochemical tests were conducted on a single-cell testing platform, with the cell temperature controlled at 60℃ or 80℃. Deionized water, preheated for 3 hours, was supplied to the anode at a flow rate of 30 mL / min and purified by a purification column before being recycled.

[0059] Example 2

[0060] Repeat the steps of Example 1, except that palladium chloride powder is not added to the preparation of the precursor solution.

[0061] Example 3

[0062] Repeat the steps of Example 1, except that the mass of palladium chloride powder in the preparation of the precursor solution is 10 mg.

[0063] Example 4

[0064] Repeat the steps of Example 1, except that the mass of palladium chloride powder in the preparation of the precursor solution is 40 mg.

[0065] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made within the scope of the claims of the present invention should be included in the scope of the present invention.

[0066] Comparative Example 1

[0067] Commercially available ruthenium oxide was used as the anode catalyst for water electrolysis, and the electrocatalytic oxygen evolution performance test conditions were the same as in Example 1.

[0068] Comparative Example 2

[0069] Repeat the steps of Example 1, except that a voltage of 1.3 V is applied to the synthesized catalyst material.

[0070] Comparative Example 3

[0071] Repeat the steps of Example 1, except that a voltage of 1.5 V is applied to the synthesized catalyst material.

[0072] II. Performance Testing and Comparison

[0073] The palladium-doped ruthenium oxide electrocatalyst PdRuO2 with dynamic oxygen buffering effect prepared in Example 1 was used. x XRD analysis was performed on RuO2 prepared in Example 2 and commercial ruthenium oxide from Comparative Example 1. The X-ray diffraction patterns were obtained by... Figure 1 As shown, the characteristic diffraction peaks at angles of 27.8°, 35.2°, and 54.5° correspond to the (1 1 0), (1 0 1), and (2 1 1) crystal planes of rutile-type ruthenium oxide crystals. x No new crystalline phase was formed.

[0074] Figure 2 This demonstrates the palladium-doped ruthenium oxide oxygen evolution electrocatalyst PdRuO2 with dynamic oxygen buffering effect prepared in Example 1. x Scanning electron micrographs of the material. Figure 2 As can be seen, the catalyst exhibits a sheet-like structure formed by the accumulation of nanoparticles.

[0075] Figure 3 This demonstrates the palladium-doped ruthenium oxide oxygen evolution electrocatalyst PdRuO2 with dynamic oxygen buffering effect prepared in Example 1. x Aberration-corrected high-angle annular dark-field scanning transmission microscopy image of the material. Figure 3 It can be seen that the catalyst mainly exposes the (2 1 0), (1 0 1) and (2 1 1) crystal planes, PdRuO x It maintains good ruthenium oxide lattice characteristics.

[0076] Figure 4 PdRuO prepared in Examples 1, 2, and 3 x The in-situ X-ray absorption near-edge structure spectra of the palladium K-edge and ruthenium K-edge are shown in the image, along with their magnified images. Comparative Example 2 shows PdRuO2 after applying a voltage of 1.3 V. x Material, Comparative Example 3 is PdRuO after applying a voltage of 1.5 V. x Materials. From Figure 4It can be seen that after applying a voltage of 1.5 V, the K absorption edge of ruthenium shifts by only 0.25 eV, while the K absorption edge of palladium shifts by 1.45 eV. This indicates that palladium responds more significantly to the anodic oxidation environment, while the valence state change of ruthenium is largely buffered, inhibiting the peroxidation of ruthenium.

[0077] Figure 5 The figures show the linear sweep voltammetry curves of the materials in Examples 1 and 2 and Comparative Example 1 in the three-electrode testing system, where Example 1 is the prepared PdRuO x Materials: Example 2 uses the prepared RuO2 material, and Comparative Example 1 uses commercially available ruthenium oxide material. Figure 5 It can be seen that Example 1 can achieve 10 mA cm⁻¹ at a potential of 1.447 V. −2 The current density required in Example 2 is 1.509 V, while Example 2 requires a potential of 10 mA cm⁻¹. −2 The current density required for Comparative Example 1 is 1.516 V, which would require a potential of 10 mA cm⁻¹. −2 The current density.

[0078] Figure 6 Examples 1, 2, and Comparative Example 1 in the three-electrode test system were tested at a current density of 100 mA cm⁻¹. −2 The constant current curves at various times are shown, with Example 1 being the prepared PdRuO. x Materials: Example 2 uses the prepared RuO2 material, and Comparative Example 1 uses commercially available ruthenium oxide material. Figure 6 It can be seen that in Example 1, at 100 mA cm⁻¹ −2 It can operate stably for 1000 hours at a given current density, with a voltage decay rate of 0.131 mV / h. −1 Example 2 and Comparative Example 1 were tested at 100 mA cm⁻¹. −2 It can only operate stably for 25 hours at the specified current density.

[0079] Figure 7 PdRuO prepared in Example 1 x Current density-voltage curves of the material used as an anode catalyst in a proton exchange membrane water electrolysis device. Figure 7 It can be seen that, at 80°C, the electrode material prepared in Example 1, in a proton exchange membrane electrolyzer, yielded a 3 A cm⁻¹ solution. −2 The battery voltage was only 1.694 V, indicating that PdRuO x The material exhibits high catalytic activity under high current density in a proton exchange membrane electrolyzer.

[0080] Figure 8 PdRuO prepared in Example 1 xThe RuO2 material prepared in Example 2 was used as the anode catalyst for proton exchange membrane water electrolysis at a current density of 1 A cm⁻¹. −2 The constant current curve at that time. (From...) Figure 8 It can be seen that the electrode material prepared in Example 1 can operate efficiently and stably in a proton exchange membrane electrolyzer for more than 200 hours without significant degradation, while the electrode material prepared in Example 2 shows significant performance degradation after 10 hours of operation, indicating that the catalyst has significant potential in the practical application of proton exchange membrane electrolysis for hydrogen production.

[0081] The undescribed parts of this invention are the same as or implemented using existing technology. The applicant declares that this invention is illustrated through the above specific embodiments, but the invention is not limited to the above detailed methods, i.e., it does not mean that the invention must rely on the above detailed methods to be implemented. Those skilled in the art should understand that any improvements to this invention, equivalent substitutions of raw materials for the product of this invention, additions of auxiliary components, and selection of specific methods all fall within the protection and disclosure scope of this invention.

Claims

1. A method for preparing a palladium-doped ruthenium oxide oxygen evolution electrocatalyst, characterized in that, Includes the following steps: (1) Dissolve hydrated ruthenium chloride in deionized water to form a precursor solution with a concentration of 10 g / L; (2) Mix palladium salt, sodium nitrate and potassium nitrate with the solution in step (1), dissolve them in anhydrous ethanol and water to form a solution, and stir magnetically for 20 to 50 minutes; (3) Remove the solvent from the mixed solution obtained in step (2) by rotary evaporation at 60~80℃, and dry it in a vacuum oven at 55~65℃ for 10~14 hours; (4) Place the gray-green powder obtained in step (3) in a muffle furnace at 320~400℃ and keep it warm for 20~40 minutes, then take it out and cool it to room temperature in the air. (5) The black product obtained in step (4) is washed multiple times with deionized water and anhydrous ethanol, and finally dried in a vacuum oven at 55~65℃ for 10~14 hours. (6) Transfer the black powder obtained in step (5) to a quartz crucible and calcine it in a muffle furnace at 400°C for 4 to 6 hours.

2. The method for preparing the palladium-doped ruthenium oxide oxygen evolution electrocatalyst according to claim 1, characterized in that, In step (1), hydrated ruthenium chloride is selected from ruthenium trichloride hydrate.

3. The method for preparing the palladium-doped ruthenium oxide oxygen evolution electrocatalyst according to claim 1, characterized in that, In step (2), the palladium salt is selected from any one of palladium chloride, palladium nitrate, palladium sulfate, tetrachloropalladium salt and tetraamminepalladium salt.

4. The method for preparing the palladium-doped ruthenium oxide oxygen evolution electrocatalyst according to claim 1, characterized in that, The mass ratio between palladium salt and hydrated ruthenium chloride is 1~4:16~17; the mass ratio between sodium nitrate and potassium nitrate is 3:2; and the mass ratio between palladium salt and sodium nitrate is 5~24:

1.

5. A palladium-doped ruthenium oxide oxygen evolution electrocatalyst, characterized in that, It is prepared by the method described in any one of claims 1 to 4.

6. The application of the palladium-doped ruthenium oxide oxygen evolution electrocatalyst according to claim 5 in the preparation of electrocatalytic oxygen evolution reaction materials or proton exchange membrane electrolyzer anode materials.

7. An electrocatalytic oxygen evolution reaction apparatus, characterized in that, Its working electrode is loaded with the palladium-doped ruthenium oxide oxygen evolution electrocatalyst as described in claim 5.

8. An anode for a proton exchange membrane electrolyzer, characterized in that, It includes a support and an anode material loaded on the support in a certain manner, said anode material including the palladium-doped ruthenium oxide oxygen evolution electrocatalyst of claim 5.

9. A proton exchange membrane electrolyzer, characterized in that, Its anode is selected from the anode of the proton exchange membrane electrolyzer described in claim 8.