A multi-color retro-finished dyeing method and dyeing device for aluminum alloy
By alternating cycles of grinding and dyeing after a single anodizing process, combined with pretreatment and sealing, the problem of monotonous colors and complex processes in existing aluminum alloy dyeing methods has been solved. This method achieves a natural blend of multiple colors and a mottled, aged effect, simplifies the process, and improves product quality.
Patent Information
- Application Number
- CN202611244065.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-17
- Publication Date
- 2026-11-20
AI Technical Summary
Existing aluminum alloy dyeing methods cannot achieve a natural blending and transition of multiple colors, as well as a mottled and aged appearance. The process is complex and has poor stability, which cannot meet the needs of retro-style products.
The process involves alternating cycles of grinding and dyeing after a single anodizing process, combined with pretreatments such as alkaline etching, chemical polishing, and neutralization to remove ash. The randomness and non-uniformity of the grinding stone allow different areas to absorb different colors of dye, creating a naturally interwoven multicolor effect. The durability of the dye is ensured by sealing the pores with nickel acetate.
It achieves natural mixed coloring of three or more colors, simplifies the process, reduces equipment investment and operating costs, improves production efficiency and product yield, and presents a natural mottled and old-fashioned effect with a strong sense of age.
Smart Images

Figure CN123132969A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of metal dyeing processes, and more specifically, to a dyeing method and apparatus for creating a multi-color retro aging effect on aluminum alloys. Background Technology
[0002] Aluminum alloys, due to their advantages such as low density, high specific strength, and good corrosion resistance, are widely used in many fields such as consumer electronics, architectural decoration, transportation, and household goods. To further improve the appearance quality and decorative effect of aluminum alloy products, their surfaces are usually anodized, and then dyed on the porous oxide film formed by anodizing to obtain a variety of color surface effects.
[0003] Traditional aluminum alloy anodizing and dyeing methods involve a single anodizing and dyeing process. The aluminum alloy is anodized in a sulfuric acid solution to form a porous oxide film, then immersed in a single-color organic dye bath for dyeing. Finally, the holes are sealed to obtain a single-color finished product. While this process is simple and low-cost, the color effects are monotonous and cannot meet the market's demand for diverse aluminum alloy surface colors. Furthermore, it cannot achieve natural color blending, transitions, or a mottled, aged appearance, thus failing to meet the specific surface texture requirements of retro-style products.
[0004] To overcome the limitations of single-color processes, those skilled in the art have developed various multi-color anodizing dyeing techniques. Existing multi-color processes mainly include the following: The first method involves a multi-color dyeing process using multiple anodizing stages. This involves masking the oxide film with printing ink after the first oxidation and dyeing stage, then etching away the unmasked oxide film with alkali, followed by a second oxidation stage and further dyeing. This process requires screen printing equipment, is complex and involves numerous steps, resulting in a low yield. Another method is a two-color process that uses CNC cutting tools to remove the oxide surface after the first oxidation stage, followed by a second anodizing stage. However, because the sulfuric acid solution used in the second anodizing stage corrodes the first oxide film, the second oxidation time cannot be too long, making it impossible to achieve a deep color in the second oxidation stage, resulting in poor process stability.
[0005] The second method involves a multi-color process that uses two anodizing processes to form a double-layer oxide film, followed by electrolytic coloring. This process uses the same medium to form a double-layer oxide film on the aluminum alloy surface through two anodizing processes, followed by electrolytic coloring to obtain a multi-color alumina film. However, this process also involves two anodizing processes, making process control difficult, and the range of colors that can be obtained through electrolytic coloring is limited.
[0006] The third method involves multiple dyeing processes using a combination of photosensitive emulsion and UV curing protection. This process uses photosensitive emulsion to protect the dyed areas before dyeing the unprotected areas, achieving a multi-color effect. However, this method requires multiple steps, including emulsion coating, exposure, and development, making it complex and resulting in distinct color boundaries that cannot achieve natural color transitions or a mottled, aged effect. Summary of the Invention
[0007] The purpose of this invention is to address the shortcomings of existing technologies by providing a multi-color retro-style dyeing method for aluminum alloys, which can effectively solve the aforementioned problems.
[0008] To achieve the above requirements, the technical solution adopted by the present invention to solve its technical problem is as follows: On one hand, the present invention provides a method for dyeing aluminum alloy in multiple colors to create a vintage look, which includes the following steps: Pretreatment: The aluminum alloy is pretreated to obtain a clean surface. Anodizing: The pretreated aluminum alloy is immersed in an anodizing solution for anodizing, forming a porous oxide film on the surface of the aluminum alloy; First dyeing: The anodized aluminum alloy is placed in the first dyeing bath for dyeing treatment, so that the porous oxide film adsorbs the first color dye; One-time grinding: The aluminum alloy after one-time dyeing is put into a grinding machine for grinding to remove the original dye color from the surface of the aluminum alloy; Secondary dyeing: The aluminum alloy after the first grinding is placed into the second dyeing bath for dyeing treatment, so that the areas where the color was ground off can absorb the second color dye. Secondary grinding: The aluminum alloy after secondary dyeing is placed in a grinding machine for grinding, which removes one or two of the dyeing colors from the surface of the aluminum alloy. Three-stage dyeing: The aluminum alloy after the second grinding is placed into the third dyeing bath for dyeing treatment, so that the areas where the color was ground off again can absorb the third color dye. Hole sealing treatment: Hole sealing treatment is performed on aluminum alloys after three dyeing processes; Baking: The sealed aluminum alloy is baked and dried to obtain aluminum alloy products with a multicolored mottled and old-fashioned surface.
[0009] The staining method of the present invention, wherein the pretreatment includes the following steps: Cleaning: Place the aluminum alloy in a degreasing bath at a temperature of 50~60℃ for degreasing treatment. After completion, wash with water until the surface of the aluminum alloy is clean. Then place the aluminum alloy in an oven at a temperature of 60~70℃ to dry for 20~30 minutes. Sandblasting: After cleaning and drying, the aluminum alloy is placed in a dry automatic sandblasting machine for sandblasting treatment. The sand type is 120~170# pickaxe sand, and the sandblasting pressure is 3~4kg. Hanging: The sandblasted aluminum alloy is hung on the titanium hanger; Alkali etching: The aluminum alloy after hanging is placed in an alkaline bath at a temperature of 55~65℃ to remove the natural oxide film. The alkaline etching time is 15~30 seconds. After completion, it is washed with water to neutralize until the aluminum alloy surface is clean. Chemical polishing: The alkaline-etched aluminum alloy is placed in a tank with phosphoric acid as the main medium at a temperature of 80~90℃ for chemical polishing treatment for 30~60 seconds. Neutralization and ash removal: The chemically polished aluminum alloy is neutralized and ash removed in a nitric acid + ash removal agent ash removal system at room temperature for 1~5 minutes.
[0010] The dyeing method of the present invention includes a descaling agent comprising nitric acid, manganese nitrate, sodium sulfate, and a corrosion inhibitor.
[0011] In the staining method of the present invention, in the anodic oxidation step, the anodic oxidation solution includes a sulfuric acid solution with a concentration of 190~210g / L, the anodic oxidation voltage is 16V, the anodic oxidation time is 60~80min, and the anodic oxidation temperature is 17~19℃.
[0012] In the dyeing method of the present invention, in the first dyeing step, the dyeing bath solution is an organic dye at room temperature, and the dyeing time is 1~5 minutes; after dyeing, the aluminum alloy is cleaned in a pure water bath and then dried in an oven at 60~70℃.
[0013] In the dyeing method of the present invention, in the first grinding and second grinding steps, grinding stones with specifications of 20×20mm and 30×30mm are placed in the grinding machine. The two specifications of grinding stones are mixed in a 1:1 volume ratio. The mixed grinding stones occupy half of the volume of the grinding machine. Water is added to the grinding machine until the water level submerges the grinding stones by 2-4cm. After sealing the grinding machine, it is turned on and rotated for 2-6 minutes. After grinding is completed, the aluminum alloy is taken out and cleaned with clean water.
[0014] In the dyeing method of the present invention, in the secondary and tertiary dyeing steps, the dyeing bath solution is an organic dye at room temperature, and the dyeing time is 3-10 minutes; after dyeing, the aluminum alloy is cleaned in a pure water bath and then dried in an oven at 60-70°C.
[0015] In the dyeing method of the present invention, when four or more colors are required, after three dyeing operations are completed, a grinding and dyeing operation is repeated until the required number of colors is reached before sealing. In the sealing process, a sealing agent is used to seal the aluminum alloy after multiple dyeing processes. The sealing temperature is 90-95℃ and the sealing time is 60-100 minutes. The sealing agent includes 10-15 g / L of nickel acetate blocking salt.
[0016] In the dyeing method of the present invention, in the baking step, the aluminum alloy after the sealing treatment is placed in an oven at 60~70℃ and baked for 20~30 minutes to dry the water stains on the surface of the aluminum alloy.
[0017] On the other hand, the present invention also provides a dyeing device for multi-color retro aging of aluminum alloy, wherein the dyeing device applies any of the dyeing methods described above.
[0018] Compared with the prior art, the present invention has the following significant advantages: The present invention, through the core process design of "one-time anodizing + multiple grinding-dyeing alternating cycle", can achieve natural mixed coloring of three or more colors with only one anodizing, completely avoiding the problems of film corrosion, poor process stability and difficulty in dyeing dark colors caused by multiple anodizing in traditional multi-color processes. At the same time, it completely eliminates the need for complex auxiliary processes such as screen printing masking, photosensitive emulsion coating, exposure and development, which greatly simplifies the process flow, reduces equipment investment and operating costs, and improves production efficiency and product yield. More importantly, this invention utilizes a grinding process to perform non-uniform and selective physical and mechanical removal of the dyed oxide film, allowing different areas exposed at different grinding stages to adsorb different colors of dye in subsequent dyeing. Due to the randomness and non-repeatability of the contact between the grinding stone and the surface microstructure, the color areas form an interwoven, permeable, and overlapping distribution pattern without clear boundaries. In addition, the micro-texture formed by sandblasting pretreatment works synergistically with the grinding process, resulting in a final surface that exhibits a natural, mottled, and aged effect that is impossible to achieve with existing technologies. The color layers are rich, and each product has a unique random texture. Furthermore, this invention ensures the uniformity of the oxide film through a comprehensive pretreatment process involving alkaline etching, chemical polishing, and neutralization to remove ash. The high-temperature sealing with nickel acetate ensures the long-lasting durability and corrosion resistance of the dye. Moreover, the number of colors can be flexibly expanded according to needs. It is suitable for retro-finishing surface treatment of aluminum alloy products in various fields such as consumer electronics, architectural decoration, and home furnishings, and has good prospects for industrial application. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the present invention will be further described below in conjunction with the accompanying drawings and embodiments. The drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Figure 1 This is a flowchart of a multi-color retro aging dyeing method for aluminum alloys according to the present invention. Detailed Implementation
[0020] The terms "first," "second," "third," and "fourth," etc., used in the specification, claims, and accompanying drawings of this invention are used to distinguish different objects, not to describe a specific order. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or apparatus that includes a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to these processes, methods, products, or apparatuses.
[0021] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0022] "Multiple" refers to two or more. "And / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A alone, A and B simultaneously, or B alone. The character " / " generally indicates that the preceding and following related objects have an "or" relationship.
[0023] Furthermore, the terms indicating orientation, such as "up," "down," "left," "right," "upper end," "lower end," and "longitudinal," are all based on the posture and position of the device or equipment described in this solution during normal use.
[0024] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, a clear and complete description will be provided below in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the protection scope of the present invention.
[0025] A preferred embodiment of the present invention provides a method for dyeing aluminum alloy in multiple colors to create a vintage, distressed finish, such as... Figure 1 As shown, it includes the following steps: Step 1: Pre-processing Aluminum alloys undergo pretreatment to obtain a clean surface. Pretreatment is a fundamental step to ensure the quality of subsequent anodizing and dyeing. Its purpose is to remove oil, natural oxide film, and impurities from the aluminum alloy surface, resulting in a uniform micro-roughness that facilitates the uniform growth of the subsequent oxide film. Specifically, the pretreatment in this embodiment includes the following steps: (1) Cleaning: The aluminum alloy is placed in a degreasing tank at a temperature of 50~60℃ for degreasing treatment to remove processing oil and dirt from the surface of the aluminum alloy. The degreasing time can be adjusted according to the degree of oil on the surface of the aluminum alloy, until the surface oil is completely removed. After completion, the aluminum alloy is taken out and placed in a water washing tank for washing with running pure water until the surface of the aluminum alloy is clean, and the surface is visually free of oil and the water film is continuous and unbroken. Then the cleaned aluminum alloy is placed in an oven at a temperature of 60~70℃ for drying for 20~30 minutes to remove surface moisture and prevent water stains from affecting the uniformity of sandblasting during subsequent sandblasting.
[0026] (2) Sandblasting: The cleaned and dried aluminum alloy is placed in a dry automatic sandblasting machine for sandblasting treatment. The abrasive type is 120~170# abrasive, and the sandblasting pressure is 3~4 kg (i.e., the sandblasting pressure is 3~4 kg / cm). 2 Sandblasting creates a uniform micro-texture on the aluminum alloy surface, increasing the adhesion between the subsequent oxide film and the substrate. Furthermore, by controlling the surface roughness, it influences the visual effect after dyeing, resulting in a more natural aged look. After sandblasting, compressed air can be used to blow away any loose sand.
[0027] (3) Hanging: Hang the sandblasted aluminum alloy on a special titanium hanger. The titanium hanger has good corrosion resistance and conductivity, which can stably conduct electricity during the subsequent anodizing process and will not cause metal ion contamination to the bath solution. When hanging, ensure good contact between the aluminum alloy and the hanger to ensure uniform current distribution during anodizing.
[0028] (4) Alkali etching: The aluminum alloy after hanging is placed in an alkaline bath at a temperature of 55~65℃ to remove the natural oxide film. The alkaline etching time is 15~30 seconds. The alkaline etching treatment can remove the oxide film that naturally forms on the surface of the aluminum alloy during sandblasting and storage, and further remove residual impurities on the surface, exposing the fresh aluminum substrate. After alkaline etching, the aluminum alloy is taken out and placed in a water washing tank for water washing and neutralization until the surface of the aluminum alloy is clean. The water washing can be carried out by two or more countercurrent rinsings to ensure that the alkaline solution is completely removed.
[0029] (5) Chemical polishing: The alkaline-etched aluminum alloy is placed in a tank with phosphoric acid as the main medium at a temperature of 80~90℃ for chemical polishing treatment for 30~60 seconds. Chemical polishing can eliminate microscopic scratches and rough peaks on the surface of the aluminum alloy through chemical dissolution, so that the surface can obtain a certain gloss and smoothness, which is conducive to the uniform formation of the oxide film in the subsequent process. After chemical polishing, the aluminum alloy is taken out and placed in a water washing tank for thorough washing.
[0030] (6) Neutralization and Desiccation: After chemical polishing, impurities such as intermetallic compounds on the surface of aluminum may dissolve and float to the surface, forming ash or spots, affecting the purity and uniformity of the subsequent oxide film. To solve this problem, the chemically polished aluminum alloy is neutralized and desiccated in a desiccation system of nitric acid and desiccant at room temperature for 1-5 minutes. In this embodiment, the desiccant includes, but is not limited to, nitric acid, manganese nitrate, sodium sulfate, and corrosion inhibitors. In actual operation, the component ratio of the desiccant can be selected adaptively according to the material of the aluminum alloy. After desiccation, the aluminum alloy is removed and thoroughly washed with water, thus completing the previous treatment.
[0031] Step 2: Anodizing The pretreated aluminum alloy is immersed in an anodizing solution for anodizing, forming a porous oxide film on the surface of the aluminum alloy.
[0032] In this embodiment, the specific process parameters for the anodizing step are as follows: the anodizing solution is a sulfuric acid solution with a concentration of 190~210 g / L, the anodizing voltage is 16V, the anodizing time is 60~80 min, and the anodizing temperature is 17~19℃. Under these conditions, a porous oxide film with moderate thickness and uniform porosity can be formed on the aluminum alloy surface. This oxide film has a honeycomb structure with regularly distributed pores, providing sufficient adhesion sites for the subsequent adsorption and fixation of dye molecules. During the anodizing process, compressed air or mechanical stirring is required to ensure uniform temperature and concentration distribution of the bath solution, and a cooling system is used to control the bath solution temperature within the process range. After anodizing, the aluminum alloy is removed and thoroughly cleaned in a water washing tank to remove residual sulfuric acid solution from the surface.
[0033] Step 3: First staining The anodized aluminum alloy is immersed in a first dyeing bath for dyeing, allowing the porous oxide film to adsorb the first color dye. In this embodiment, the dyeing bath is a room-temperature organic dye, and the dyeing time is 1-5 minutes. The specific dyeing time is adjusted adaptively according to the desired color depth; the deeper the desired color, the longer the dyeing time. After dyeing, the aluminum alloy is removed and placed in a clean pure water bath to wash away surface dye, and then dried in an oven at 60-70°C. The drying process fixes the initially adsorbed dye molecules and provides a dry surface for subsequent grinding processes, facilitating uniform control of the grinding effect. After one dyeing, the pores of the porous oxide film are uniformly filled with the first color dye, and the aluminum alloy as a whole exhibits the first color.
[0034] Step 4: First grinding The aluminum alloy after one dyeing process is placed in a grinding machine for grinding to remove the original dye color from the surface of the aluminum alloy.
[0035] In this embodiment, the core mechanism of the grinding process lies in the irregular mechanical friction and collision between the grinding stone and the aluminum alloy surface. Due to the uneven raised areas on the microscopic surface of the aluminum alloy, the grinding stone preferentially contacts and grinds away the oxide film coloring layer on the raised areas, while the recessed areas are less covered by the grinding stone, and the coloring layer is retained. This selective grinding action results in the uneven removal of the first color, exposing part of the oxide film substrate or aluminum substrate. In this embodiment, grinding stones with specifications of 20×20mm and 30×30mm are placed in the grinding machine. The two specifications of grinding stones are mixed in a 1:1 volume ratio, and the mixed grinding stones occupy half of the volume of the grinding machine. Water is added to the grinding machine until the water level submerges the grinding stones by 2-4cm. After sealing the grinding machine, it is turned on and rotated for 2-6 minutes. After grinding is completed, the aluminum alloy is removed and cleaned with clean water. It's worth noting that mixing different sizes of grinding stones can produce grinding marks of varying sizes. Larger grinding stones provide stronger grinding force, primarily targeting higher, raised areas, while smaller grinding stones can work on relatively small surface structures. The synergistic effect of both makes the grinding result richer, more natural, and less mechanical. Grinding time should be controlled within the range of 2-6 minutes. Too short a time will result in insufficient removal of material and minimal color change; too long a time may over-remove material or even damage the underlying oxide film, affecting subsequent dyeing results.
[0036] Step 5: Secondary staining The aluminum alloy, after the first grinding, is placed in a second dyeing bath for dyeing, allowing the areas where the original color was removed to absorb the second color dye. In this embodiment, the dyeing bath solution is a room-temperature organic dye, and the dyeing time is 3-10 minutes, which is adjusted according to the desired color depth. After dyeing, the aluminum alloy is removed, placed in a clean pure water bath to wash away surface dye, and then dried in an oven at 60-70°C. It should be noted that the second dyeing time (3-10 minutes) is usually longer than the first dyeing time (1-5 minutes). This is because after the first grinding, the oxide film in some areas has been thinned, and the dye adsorption rate has changed. Appropriately extending the time helps the second color dye to fully penetrate the pores of the oxide film exposed by the grinding. After the second dyeing, the areas exposed by the grinding absorb the second color dye and exhibit the second color, while the areas not ground by the first dyeing retain the first color, thus forming a mixed effect of two colors coexisting on the aluminum alloy surface. Furthermore, the boundary between the two colors exhibits a natural transition without a clear boundary due to the randomness and irregularity of the grinding process itself.
[0037] Step 6: Secondary grinding The aluminum alloy, after secondary dyeing, is placed in a grinding machine for grinding to remove a portion of the first and / or second color dyeing on the surface. In this embodiment, the process parameters for secondary grinding are the same as for primary grinding: 20×20mm and 30×30mm grinding stones are placed in the grinding machine, mixed in a 1:1 volume ratio, with the mixed stones occupying half the volume of the grinding machine. Water is added to the grinding machine until it submerges the grinding stones by 2-4cm. The grinding machine is sealed and turned on for 2-6 minutes. After grinding, the aluminum alloy is removed and cleaned with water. The mechanism of secondary grinding is the same as primary grinding. However, since the aluminum alloy surface now has both first and second color dyeing areas, the randomness of grinding means that some areas may have the first color removed, exposing the oxide film substrate; some areas may have the second color removed, exposing the first color layer; and some areas may have both colors removed simultaneously, exposing the underlying oxide film or even the aluminum substrate. This multiple random superposition effect results in a richer and more unrepeatable removal of surface color, leading to a more natural color. After grinding, the surface is rinsed with water.
[0038] Step 7: Three stainings The aluminum alloy, after secondary grinding, is placed in a third dyeing bath for dyeing, allowing the areas where the color was ground off to absorb the third color dye. In this embodiment, the dyeing bath solution is a room-temperature organic dye, and the dyeing time is 3-10 minutes, which is adjusted according to the desired color depth. After dyeing, the aluminum alloy is removed and placed in a clean pure water bath to wash away any surface dye. After secondary grinding and a third dyeing, the newly exposed oxide film pores absorb the third color dye, exhibiting the third color, while the areas with the first and second colors that were not ground off remain unchanged. Thus, the aluminum alloy surface simultaneously possesses the first, second, and third colors. Due to the randomness and unevenness of each grinding process, the three colors are naturally mixed and interspersed, without clear boundaries, forming a mottled, vintage effect.
[0039] When four or more colors are required, simply repeat the grinding and dyeing process after three dyeing cycles, following the "grinding → dyeing" cycle until the desired number of colors is achieved. Each additional grinding-dyeing cycle adds a new color layer to the surface, increasing the richness and depth of the colors.
[0040] Step 8: Sealing the holes Aluminum alloys that have undergone three or more dyeing processes are subjected to a sealing treatment. The purpose of the sealing treatment is to seal the micropores of the oxide film, firmly encapsulating the dye molecules inside the pores of the oxide film, preventing the dye from falling off or fading during subsequent use, and at the same time improving the corrosion resistance and wear resistance of the oxide film.
[0041] In this embodiment, the sealing treatment specifically involves applying a sealing agent to the aluminum alloy after multiple dyeing processes. The sealing temperature is 90-95°C, and the sealing time is 60-100 minutes. The sealing agent comprises 10-15 g / L of nickel acetate blocking salt. Under high temperature conditions, nickel ions hydrolyze to generate nickel hydroxide precipitate, which fills the micropores of the oxide film, achieving effective sealing. After sealing, the aluminum alloy is removed and thoroughly cleaned in a water washing tank.
[0042] Step 9: Baking After sealing the holes, the aluminum alloy is placed in an oven at 60-70℃ and baked for 20-30 minutes to dry the water stains on the surface, resulting in an aluminum alloy product with a multicolored, mottled, and aged effect. It is worth noting that the baking temperature should not be too high to avoid heat damage to the organic dyes, which may cause discoloration or fading.
[0043] Example 2: This invention also provides a dyeing device for multi-color retro aging of aluminum alloys. The dyeing device applies the dyeing method described in Example 1, and specifically uses the following equipment: (1) Degreasing tank, used to hold degreasing liquid for degreasing aluminum alloy to remove surface oil stains. The degreasing tank is equipped with a heating device and a temperature control system to control the temperature of the tank liquid at 50~60℃.
[0044] (2) A water washing tank is installed after the degreasing tank and is used to wash the degreased aluminum alloy to remove the residual degreasing liquid on the surface. The water washing tank consists of multiple overflow water washing tanks connected in series and adopts a counter-current rinsing method to improve the washing efficiency and save water.
[0045] (3) An oven is installed after the water washing tank to dry the washed aluminum alloy and remove surface moisture. The oven is a hot air circulating oven with an adjustable temperature range from room temperature to 200℃. In this scheme, the temperature is set to 60~70℃.
[0046] (4) A dry automatic sandblasting machine, located after the oven, is used to sandblast dried aluminum alloys. The dry automatic sandblasting machine includes a sandblasting chamber, a sand recovery system, a dust removal system, and a control system. It uses 120~170# abrasive as the sandblasting medium, and the sandblasting pressure is 3~4 kg / cm². 2 .
[0047] (5) Titanium hangers are used to hang aluminum alloys in subsequent processes, ensuring that the aluminum alloys remain stable and fixed during transfer between tanks. The titanium hangers are made of titanium alloy material, which has excellent electrical conductivity and corrosion resistance.
[0048] (6) Alkali tank, set after the sandblasting process, is used to hold alkaline etching solution to remove the natural oxide film from aluminum alloy. The alkaline tank is equipped with a heating device and a temperature control system to control the temperature of the solution at 55~65℃.
[0049] (7) Chemical polishing tank, located after the alkaline tank, is used to hold a chemical polishing solution with phosphoric acid as the main medium for chemical polishing of aluminum alloys. The chemical polishing tank is equipped with a heating device and a temperature control system to control the temperature of the solution at 80~90℃.
[0050] (8) Neutralization and ash removal tank, located after the chemical polishing tank, is used to contain a ash removal system of nitric acid and ash removal agent to neutralize and remove ash residue and spots from the surface of aluminum alloy after chemical polishing. The neutralization and ash removal tank operates at room temperature.
[0051] (9) Anodizing tank, located after the neutralization and descaling tank, is used to hold sulfuric acid anodizing solution with a concentration of 190~210g / L to anodize aluminum alloys to form a porous oxide film. The anodizing tank is equipped with a DC power supply (voltage adjustable to 16V), cooling coils or heat exchangers (used to control the temperature of the solution at 17~19℃) and a stirring device (used to ensure uniform temperature and concentration of the solution).
[0052] (10) The first dyeing tank, the second dyeing tank, and the third dyeing tank are arranged sequentially after the anodizing tank and are used to hold the organic dyeing solutions of the first color, the second color, and the third color, respectively, for dyeing the aluminum alloy. Each dyeing tank is an independently set room temperature dyeing tank and is equipped with a pH meter and a stirring device.
[0053] (11) A grinding machine, located between each dyeing process, is used to hold grinding stones and water to grind the dyed aluminum alloy to remove the dye color from some areas of the aluminum alloy surface. The grinding machine is a roller-type grinding machine, which contains grinding stones of 20×20mm and 30×30mm in size. The two sizes of grinding stones are mixed in a 1:1 volume ratio, and the mixed grinding stones occupy half of the volume of the grinding machine. Water is added to the grinding machine until the water level submerges the grinding stones by 2-4cm. The grinding machine is equipped with a rotation drive device and a timing control device, and the rotation time is set to 2-6 minutes.
[0054] (12) Sealing tank, set after the final dyeing process, is used to hold the sealing agent and seal the aluminum alloy after dyeing. The sealing tank is equipped with a heating device and a temperature control system to control the temperature of the tank solution at 90~95℃.
[0055] The aluminum alloy is transferred between processes via manual transfer or automated conveying devices, such as conveyor systems and robotic arms, between the aforementioned tanks and equipment. Each washing tank is located after its corresponding treatment tank and is used to clean the aluminum alloy promptly after each chemical treatment step.
[0056] It is worth noting that the equipment used above are all common surface treatment equipment in the field. Their specific models, specifications, and materials can be conventionally selected and adapted by those skilled in the art according to actual production scale and process requirements. The core improvement of this invention lies in the multi-color dyeing process and grinding-dyeing cycle operation in Example 1, rather than the specific structure of the equipment itself. Therefore, as long as the functions required by each step of this invention can be achieved, any commercially available or conventional equipment in the field can be applied to this invention and falls within the scope of protection of this invention. Therefore, the above-mentioned equipment should not be construed as a limitation on the device scheme of this invention. Those skilled in the art, after reading the method steps of Example 1 and combining them with common knowledge in the field, can determine the equipment type and basic configuration corresponding to each step without creative effort. It should be understood that those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the scope of protection of the appended claims.
Claims
1. A method for dyeing aluminum alloy in multiple colors to create a vintage, distressed finish, characterized in that... This includes the following steps: Pretreatment: The aluminum alloy is pretreated to obtain a clean surface. Anodizing: The pretreated aluminum alloy is immersed in an anodizing solution for anodizing, forming a porous oxide film on the surface of the aluminum alloy; First dyeing: The anodized aluminum alloy is placed in the first dyeing bath for dyeing treatment, so that the porous oxide film adsorbs the first color dye; One-time grinding: The aluminum alloy after one-time dyeing is put into a grinding machine for grinding to remove the original dye color from the surface of the aluminum alloy; Secondary dyeing: The aluminum alloy after the first grinding is placed into the second dyeing bath for dyeing treatment, so that the areas where the color was ground off can absorb the second color dye. Secondary grinding: The aluminum alloy after secondary dyeing is placed in a grinding machine for grinding, which removes one or two of the dyeing colors from the surface of the aluminum alloy. Three-stage dyeing: The aluminum alloy after the second grinding is placed into the third dyeing bath for dyeing treatment, so that the areas where the color was ground off again can absorb the third color dye. Hole sealing treatment: Hole sealing treatment is performed on aluminum alloys after three dyeing processes; Baking: The sealed aluminum alloy is baked and dried to obtain aluminum alloy products with a multicolored mottled and old-fashioned surface.
2. The staining method according to claim 1, characterized in that, The preprocessing includes the following steps: Cleaning: Place the aluminum alloy in a degreasing bath at a temperature of 50~60℃ for degreasing treatment. After that, wash it with water until the surface of the aluminum alloy is clean. Then place the aluminum alloy in an oven at a temperature of 60~70℃ to dry for 20~30 minutes. Sandblasting: After cleaning and drying, the aluminum alloy is placed into a dry automatic sandblasting machine for sandblasting treatment. The sand type is 120~170# pickaxe sand, and the sandblasting pressure is 3~4kg. Hanging: The sandblasted aluminum alloy is hung on the titanium hanger; Alkali etching: The aluminum alloy after hanging is placed in an alkaline bath at a temperature of 55~65℃ to remove the natural oxide film. The alkaline etching time is 15~30 seconds. After completion, it is washed with water to neutralize until the aluminum alloy surface is clean. Chemical polishing: The alkaline-etched aluminum alloy is placed in a tank with phosphoric acid as the main medium at a temperature of 80~90℃ for chemical polishing treatment for 30~60 seconds. Neutralization and ash removal: The chemically polished aluminum alloy is neutralized and ash removed in a nitric acid + ash removal agent ash removal system at room temperature for 1~5 minutes.
3. The staining method according to claim 2, characterized in that, The ash remover includes nitric acid, manganese nitrate, sodium sulfate, and a corrosion inhibitor.
4. The staining method according to claim 1, characterized in that, In the anodizing step, the anodizing solution includes a sulfuric acid solution with a concentration of 190~210g / L, the anodizing voltage is 16V, the anodizing time is 60~80min, and the anodizing temperature is 17~19℃.
5. The staining method according to any one of claims 1-4, characterized in that, In the dyeing step, the dyeing bath solution is an organic dye at room temperature, and the dyeing time is 1~5 minutes. After dyeing, the aluminum alloy is cleaned in a pure water bath and then dried in an oven at 60~70℃.
6. The staining method according to claim 1, characterized in that, In the first and second grinding steps, grinding stones of 20×20mm and 30×30mm are placed in the grinding machine. The two types of grinding stones are mixed in a 1:1 volume ratio. The mixed grinding stones occupy half of the volume of the grinding machine. Water is added to the grinding machine until the water level submerges the grinding stones by 2-4cm. After sealing the grinding machine, it is turned on and rotated for 2-6 minutes. After grinding is completed, the aluminum alloy is removed and cleaned with clean water.
7. The staining method according to claim 6, characterized in that, In the secondary and tertiary dyeing steps, the dyeing bath solution is an organic dye at room temperature, and the dyeing time is 3 to 10 minutes. After dyeing, the aluminum alloy is cleaned in a pure water bath and then dried in an oven at 60 to 70 degrees Celsius.
8. The staining method according to claim 7, characterized in that, When four or more colors are required, after completing three dyeing operations, repeat the grinding and dyeing process until the required number of colors is achieved before performing the sealing process. In the sealing process, a sealing agent is used to seal the aluminum alloy after multiple dyeing processes. The sealing temperature is 90-95℃ and the sealing time is 60-100 minutes. The sealing agent includes 10-15 g / L of nickel acetate blocking salt.
9. The staining method according to claim 7, characterized in that, In the baking step, the sealed aluminum alloy is placed in an oven at 60~70℃ and baked for 20~30 minutes to dry the water stains on the surface of the aluminum alloy.
10. A dyeing device for multi-color retro aging of aluminum alloy, characterized in that, The staining apparatus uses the staining method as described in any one of claims 1-9.