A method and device for growing a super low resistance heavily doped phosphorus silicon single crystal
By dynamically compensating for phosphorus volatilization during the Czochralski growth process, and utilizing the decomposition of phosphine gas into elemental phosphorus at high temperatures and its melting into the silicon melt, the problem of insufficient resistivity caused by the easy volatilization of phosphorus was solved. This enabled the stable growth of ultra-low resistivity heavily phosphorus-doped silicon single crystals, avoiding polycrystalline and oxide accumulation and improving product quality.
Patent Information
- Application Number
- CN202611537917.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-20
AI Technical Summary
In the Czochralski method for growing heavily phosphorus-doped silicon single crystals, phosphorus is easily volatilized, making it difficult to achieve a resistivity below 0.0009 Ω·cm. Existing technologies are prone to polycrystalline risks or oxide accumulation in the furnace, making it difficult to stably obtain ultra-low resistivity heavily phosphorus-doped silicon single crystals.
Dynamic compensation for phosphorus volatilization during the Czochralski growth process is adopted. Phosphine gas is introduced into the furnace at different stages of crystal growth, causing it to decompose into elemental phosphorus at high temperature and melt into the silicon melt. The phosphorine gas flow rate is adjusted by the phosphorine system and control system to maintain a stable phosphorus content in the melt and avoid high initial doping and high furnace pressure.
Without inducing polycrystalline risks and oxide accumulation in the furnace, ultra-low resistivity heavily phosphorus-doped silicon single crystals are stably obtained, with resistivity reaching below 0.001 Ω·cm, which improves product yield and reduces the risk of crystallization difficulties.
Smart Images

Figure CN123132986A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of semiconductor silicon single crystal growth technology, specifically relating to a method and apparatus for growing ultra-low resistivity heavily phosphorus-doped silicon single crystals. Background Technology
[0002] With the rapid development of AI and new energy industries, power devices are demanding increasingly lower power consumption, which in turn requires lower resistivity of silicon substrates. Some power devices and power integrated circuits even require resistivity of heavily phosphorus-doped silicon substrates below 0.0009 Ω·cm. During the Czochralski method for growing heavily phosphorus-doped silicon single crystals, the vapor pressure of phosphorus, the dopant element, is relatively high, making it easy to volatilize from the surface of the silicon melt. This makes it difficult to maintain a low phosphorus impurity content within the silicon crystal. This method is typically suitable for conventional heavily phosphorus-doped products with resistivity in the range of 0.001-0.002 Ω·cm. Obtaining ultra-low resistivity heavily phosphorus-doped silicon single crystal products (resistivity < 0.001 Ω·cm) is very difficult, and product yield cannot be guaranteed.
[0003] Currently, the following two technical methods are mainly used to address the problem of phosphorus volatilization.
[0004] One approach is to increase the initial doping amount by adding more phosphorus source during the feeding stage to increase the phosphorus impurity content in the melt. This aims to retain a sufficient phosphorus concentration in the crystal after volatilization loss, thereby obtaining silicon single crystals with lower resistivity. However, excessive impurity concentration can disrupt the atomic arrangement structure of the silicon crystal, causing compositional supercooling at the solid-liquid interface, which can easily lead to the transformation of single-crystal silicon into polycrystalline silicon and reduce the crystallization rate.
[0005] Another approach is to increase the furnace pressure during crystal growth. By raising the furnace pressure, the volatilization rate of phosphorus from the melt surface is suppressed, thereby increasing the phosphorus impurity content in the silicon single crystal rod and obtaining silicon single crystals with lower resistivity. However, under high furnace pressure, oxides inside the furnace are difficult to be carried away by the protective gas in time, which easily leads to the accumulation of oxides on the furnace wall and the surface of hot zone components, thus affecting the crystallization process and causing crystallization difficulties.
[0006] Therefore, there is an urgent need for a growth method that can effectively compensate for phosphorus volatilization and stably obtain ultra-low resistivity heavily phosphorus-doped silicon single crystals without causing polycrystalline risks or oxide accumulation in the furnace. Summary of the Invention
[0007] To address the shortcomings of existing technologies, this invention provides a method and apparatus for growing ultra-low resistivity heavily phosphorus-doped silicon single crystals. By dynamically compensating for phosphorus volatilization at different stages of crystal growth, the phosphorus content in the melt is kept stable, thereby obtaining ultra-low resistivity heavily phosphorus-doped silicon single crystals.
[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows: a method for growing ultra-low resistivity heavily phosphorus-doped silicon single crystals, wherein silicon single crystals are grown in a single crystal furnace using the Czochralski method. After the crystal growth enters the constant diameter growth stage, phosphine gas is introduced into the furnace. The phosphine gas decomposes into elemental phosphorus and hydrogen in the high-temperature environment inside the furnace. The elemental phosphorus melts into the silicon melt in the furnace atmosphere, continuously compensating for the phosphorus element lost in the silicon melt due to surface volatilization. The hydrogen gas is discharged together with the protective gas inside the furnace.
[0009] Furthermore, during the crystal growth stages of crystal initiation and shoulder formation, phosphine gas is introduced into the furnace to compensate for the phosphorus loss in the silicon melt due to surface volatilization.
[0010] Furthermore, the flow rate of phosphine gas is dynamically adjusted according to the crystal growth process to match the amount of elemental phosphorus replenished with the amount of phosphorus volatilized and lost in the silicon melt.
[0011] Furthermore, the phosphine gas flow rate ranges from 1 to 20 slpm.
[0012] Furthermore, the formula for determining whether phosphorus is in dynamic equilibrium within a single crystal furnace is: Phosphine supply rate = Crystal solidification carry-away rate + Melt surface volatilization rate.
[0013] The present invention also proposes a growth apparatus for ultra-low resistivity heavily phosphorus-doped silicon single crystals, including a single crystal furnace and a control system, and further including a phosphine system. The phosphine system includes an independent phosphine gas cylinder and an independent phosphine gas pipeline. The independent phosphine gas cylinder is located outside the single crystal furnace. One end of the independent phosphine gas pipeline is connected to the outlet of the independent phosphine gas cylinder, and the other end is connected to the gas inlet on the single crystal furnace.
[0014] Furthermore, a mass flow meter is connected to the independent phosphine gas supply pipeline. The mass flow meter is communicatively connected to the control system, and the control system dynamically adjusts the phosphine gas flow rate by adjusting the mass flow meter according to the crystal growth process.
[0015] Furthermore, the air inlet is positioned above the surface of the molten silicon inside the single crystal furnace.
[0016] Furthermore, the air inlet is located on the throat flange of the single crystal furnace.
[0017] Furthermore, the air inlet includes an air inlet port and an air outlet port. The air inlet port is set to one and is located on the outer diameter surface of the throat flange of the single crystal furnace. The air outlet ports are set to 3-8 and are evenly distributed along the circumference on the inner diameter surface of the throat flange. The air inlet port and all the air outlet ports are connected by a built-in pipeline set in the throat flange. The independent phosphine gas supply pipeline is connected to the air inlet port.
[0018] The beneficial effects of the present invention are as follows: 1. The present invention dynamically introduces phosphine gas during the crystal growth seeding stage, shoulder formation stage, shoulder turning stage, and equal diameter stage, and uses the elemental phosphorus generated by the decomposition of phosphine in the furnace to continuously replenish the phosphorus element lost due to volatilization in the silicon melt. This can maintain the phosphorus content of the melt without relying on excessive initial doping, which is beneficial to avoid the problems of component undercooling and polycrystalline caused by excessive impurity concentration.
[0019] 2. This invention compensates for phosphorus volatilization by dynamically replenishing phosphorus in the gas phase, without relying on increasing the furnace pressure to suppress phosphorus volatilization. It can maintain relatively reasonable furnace pressure conditions, which is conducive to the timely removal of oxides in the furnace by the protective gas, alleviating the accumulation of oxides on the furnace wall and hot zone components, and reducing the risk of crystallization difficulties.
[0020] 3. By using a mass flow meter in conjunction with a control system, the flow rate of phosphine can be adjusted according to the crystal growth process, which can dynamically match the changes in phosphorus volatilization rate and help maintain the stability of phosphorus content in the melt. Attached Figure Description
[0021] Figure 1 This is a schematic diagram of the overall structure of the ultra-low resistivity heavily phosphorus-doped silicon single crystal growth device described in Example 1; Figure 2 This is a cross-sectional elevation view of the single crystal furnace in the ultra-low resistivity heavily phosphorus-doped silicon single crystal growth apparatus described in Example 1. Figure 3 This is a schematic diagram of the throat flange of the ultra-low resistivity heavily phosphorus-doped silicon single crystal growth device described in Example 1; Figure 4 To compare the resistivity variation curve of Experiment 1 with crystal length; Figure 5 To compare the resistivity variation curve of Experiment 2 with crystal length; Figure 6 To compare the resistivity variation curve of Experiment 3 with crystal length; Figure 7 To compare the resistivity variation curve with crystal length in Experiment 4; The markings in the diagram are: 1. Independent phosphine gas cylinder, 2. Independent phosphine gas pipeline, 3. Mass flow meter, 4. Inlet port, 5. Single crystal furnace, 6. Control system, 7. Crystal rod, 8. Heat shield, 9. Graphite crucible, 10. Silicon melt, 11. Throat flange, 12. Outlet port, 13. Internal piping. Detailed Implementation
[0022] The present invention will be further described in detail below with reference to the embodiments, but this should not be construed as limiting the invention in any way.
[0023] Example 1
[0024] like Figure 1-3As shown, the growth apparatus for ultra-low resistivity heavily phosphorus-doped silicon single crystals of the present invention includes a single crystal furnace 5, a phosphine system, and a control system 6.
[0025] The single crystal furnace 5 is equipped with a graphite crucible 9 and a heat shield 8, and its internal structure adopts a conventional structure. The phosphine system includes an independent phosphine gas cylinder 1, an independent phosphine gas supply pipe 2, and a mass flow meter 3. The independent phosphine gas cylinder 1 is located outside the single crystal furnace 5. One end of the independent phosphine gas supply pipe 2 is connected to the outlet of the independent phosphine gas cylinder 1, and the other end is connected to the inlet on the single crystal furnace 5, for supplying phosphine gas into the single crystal furnace 5. The inlet 4 is positioned higher than the surface of the silicon melt 10 inside the single crystal furnace 5, so that the phosphine gas decomposes into elemental phosphorus and hydrogen upon heating inside the furnace. The elemental phosphorus melts into the silicon melt to compensate for the phosphorus element lost due to volatilization in the silicon melt. In this embodiment, the inlet is located on the side of the throat flange 11 at the top of the single crystal furnace 5. The mass flow meter 3 is also connected to the independent phosphine gas supply pipe 2 to control the flow rate of the phosphine gas. Preferably, the mass flow meter 3 and the control system 6 are communicatively connected. The control system 6 controls the mass flow meter 3 to turn on when the crystal enters the crystal growth stage, the shoulder formation stage, the shoulder turning stage, and the constant diameter stage, so as to introduce phosphine gas into the single crystal furnace 5, and adjusts the flow rate of phosphine gas according to the crystal growth process.
[0026] Specifically, such as Figure 3 As shown, the air inlet includes an inlet port 4 and an outlet port 12. There is one inlet port 4, located on the outer diameter surface of the throat flange 11 of the single crystal furnace 5. There are 3-8 outlet ports 12, evenly distributed circumferentially on the inner diameter surface of the throat flange 11. The inlet port 4 and all the outlet ports 12 are connected by an internal pipeline 13 located within the throat flange 11. The independent phosphine gas supply pipeline 2 is connected to the inlet port 4. Phosphine gas enters the internal pipeline 13 through the inlet port 4, disperses, and is released into the single crystal furnace 5 through different outlet ports 12.
[0027] Example 2
[0028] This embodiment provides a detailed description of the growth method for ultra-low resistivity heavily phosphorus-doped silicon single crystals according to the present invention. The method uses the growth apparatus for ultra-low resistivity heavily phosphorus-doped silicon single crystals described in Embodiment 1 and includes the following steps: S1. Loading and melting: The silicon material is loaded into the graphite crucible 9 of the single crystal furnace 5. After the single crystal furnace 5 is evacuated, a protective gas is introduced and heated to melt the silicon material to form a silicon melt 10. Initial doping is performed using a quartz bell jar.
[0029] S2. Crystal pulling and shoulder formation: Crystal pulling and shoulder formation are carried out according to the conventional Czochralski method. At this stage, the control system can choose whether to introduce phosphine gas.
[0030] S3. Dynamic Phosphine Supplementation During the Constant Diameter Stage: When crystal growth enters the constant diameter stage, the control system 6 sends a control signal, the mass flow meter 3 is activated, and phosphine gas is introduced into the furnace through the independent phosphine gas supply pipe 2 and the gas outlet port 12. After entering the furnace, the phosphine gas decomposes into elemental phosphorus and hydrogen under the high-temperature environment inside the furnace, when the temperature reaches the range of 375℃ to 400℃. The elemental phosphorus produced by decomposition melts into the silicon melt 10 in the furnace atmosphere, continuously compensating for the phosphorus element lost in the silicon melt 10 due to surface volatilization. The hydrogen produced by decomposition is discharged along with the protective gas inside the furnace.
[0031] S4. Dynamic Flow Rate Adjustment: During the constant diameter growth process, the control system 6 sets the phosphine flow rate according to the crystal growth process stage to adjust the opening of the mass flow meter 3, correspondingly adjusting the phosphine gas flow rate to match the replenishment of elemental phosphorus with the volatilization loss of phosphorus in the silicon melt 10, maintaining the phosphorus content in the melt within the doping element concentration range corresponding to the target resistivity. The phosphine gas flow rate range is 1-20 slpm.
[0032] S5. Finishing: After the constant diameter growth is completed, the control system 6 sends a signal to shut down the mass flow meter 3, stops the flow of phosphine gas, and completes the finishing and cooling process according to the conventional process.
[0033] Using the above method, it is possible to continuously and dynamically compensate for the volatilization loss of phosphorus in the silicon melt during the crystal growth stages of crystal seeding, shoulder formation, shoulder turning, and constant diameter stages, and stably obtain ultra-low resistivity heavily phosphorus-doped silicon single crystals without relying on excessive initial doping and high furnace pressure.
[0034] In the above method, when the following conditions are met: phosphorus supply rate of phosphine = crystal solidification carry-away rate + melt surface volatilization rate, it can be determined that the phosphorus element in the furnace is in steady-state equilibrium.
[0035] Steady-state phosphorus concentration in melt (including volatiles): ; Steady-state phosphorus concentration in crystal rods: ; Phosphine system compensation for phosphorus atom velocity: ; Phosphine system gas supply rate: ; N M =C L +C S ; Where: v is the crystal growth rate, A C It is the cross-sectional area of the crystal, k eff It is the effective segregation coefficient (phosphorus k) eff ≈0.35), E is the evaporation coefficient of phosphorus in silicon melt, A L It is the free surface area of the melt, C SIt is the concentration of phosphorus atoms in the crystal (which can be obtained from a table), N A It is Avogadro's constant, 6.022 × 10⁻⁶. 23 / mol.
[0036] In some implementations, the control system adjusts the flow rate of phosphine gas accordingly to compensate for the volatilization loss of phosphorus in the silicon melt, based on the changes in the volatilization rate of phosphorus caused by variations in process conditions such as crucible rotation, furnace pressure, pulling speed, liquid outlet distance, and argon flow rate.
[0037] The following comparative experiments illustrate how the present invention can effectively reduce the resistivity of the product and obtain ultra-low resistivity heavily phosphorus-doped silicon single crystals with a resistivity of <0.001Ω·cm.
[0038] Comparative Experiment 1 This comparative experiment included a control group and an experimental group, both using the ultra-low resistivity heavily phosphorus-doped silicon single crystal growth apparatus described in Example 1. The control group no longer introduced phosphine gas, while the experimental group introduced phosphine gas at a flow rate of 2 smol / L. The parameters for both groups were: hot zone size 24 inches, feed amount 100 kg, growth of 8-inch silicon single crystals, argon gas flow rate 50 smol / L, crucible rotation 8 rpm, crystal rotation 12 rpm, furnace pressure set to 90 Torr, initial red phosphorus doping amount 500 g, and crystal growth rate 25-35 mm / hr.
[0039] Test results: such as Figure 4 As shown, the lowest resistivity of the control group product was 0.99 mΩ·cm, or 0.00099 Ω·cm; at the same crystal length, the resistivity of the experimental group product was 0.95 mΩ·cm, or 0.00095 Ω·cm. Furthermore, at any length during crystal growth, the resistivity of the experimental group product was consistently lower than that of the control group product.
[0040] Comparative Experiment 2 The ultra-low resistivity heavily phosphorus-doped silicon single crystal growth apparatus described in Example 1 was used, with a control group and an experimental group established for the same purpose. The parameters for both experimental groups were: hot zone size 24 inches, feed rate 100 kg, growth of 8-inch silicon single crystals, argon flow rate 50 slpm, crucible rotation 8 rpm, crystal rotation 12 rpm, furnace pressure set to 90 Torr, initial red phosphorus doping amount 550 g, and crystal growth rate 25-35 mm / hr. The control group was not purged with phosphine gas, while the experimental group was purged with phosphine gas at a flow rate of 3.5 slpm.
[0041] Test results: such as Figure 5As shown, the lowest resistivity of the control group product was 0.94 mΩ·cm, or 0.00094 Ω·cm; at the same crystal length, the resistivity of the experimental group product was 0.91 mΩ·cm, or 0.00091 Ω·cm. Furthermore, at any length during crystal growth, the resistivity of the experimental group product was consistently lower than that of the control group product.
[0042] Comparative Test 3 The ultra-low resistivity heavily phosphorus-doped silicon single crystal growth apparatus described in Example 1 was used, with a control group and an experimental group established for the same purpose. The parameters for both experimental groups were: thermal zone size 24 inches, feed rate 100 kg, growth of 8-inch silicon single crystals, argon gas flow rate 50 slpm, crucible rotation 8 rpm, crystal rotation 12 rpm, furnace pressure set to 90 Torr, initial red phosphorus doping amount 590 g, and crystal growth rate 25-35 mm / hr. In the control group, phosphine gas was no longer introduced, while in the experimental group, phosphine gas was introduced at a flow rate of 5 slpm.
[0043] Test results: such as Figure 6 As shown, the lowest resistivity of the control group product was 0.92 mΩ·cm, or 0.00092 Ω·cm; at the same crystal length, the resistivity of the experimental group product was 0.91 mΩ·cm, or 0.00091 Ω·cm. Furthermore, at any length during crystal growth, the resistivity of the experimental group product was consistently lower than that of the control group product.
[0044] Comparative Test 4 In the above three comparative experiments, the phosphine gas flow rate of the experimental group was a constant value. In this embodiment, the phosphine gas flow rate of the experimental group is no longer fixed, but the phosphine flow rate is adjusted according to the crystal length. Finally, the resistivity is compared with the control group.
[0045] The experimental parameters for the control group and the experimental group were as follows: hot zone size 24 inches, feed amount 100 kg, growth of 8-inch silicon single crystal, argon flow rate 50 slpm, crucible rotation 8 rpm, crystal rotation 12 rpm, furnace pressure setting 90 Torr, initial red phosphorus doping amount 600 g, and crystal growth rate 25-35 mm / hr.
[0046] The process parameters for the experimental group are detailed in the table below. The phosphine flow rate increases with the increase of crystal length.
[0047]
[0048] Test results: such as Figure 7As shown, the lowest resistivity of the control group product was 0.91 mΩ·cm, or 0.00091 Ω·cm; at the same crystal length, the resistivity of the experimental group product was 0.86 mΩ·cm, or 0.00086 Ω·cm. Furthermore, at any length during crystal growth, the resistivity of the experimental group product was consistently lower than that of the control group product.
[0049] Combination Figure 4-7 It can be seen that the resistivity of the product obtained by adjusting the phosphine gas flow rate with the crystal length is lower than that of the product obtained by adjusting the phosphine gas flow rate, and the decrease is more significant compared with the control group.
[0050] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Those skilled in the art should understand that modifications or equivalent substitutions can be made to the specific implementation of the present invention with reference to the above embodiments. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention are within the protection scope of the pending claims.
Claims
1. A method for growing ultra-low resistivity heavily phosphorus-doped silicon single crystals, comprising growing silicon single crystals in a single crystal furnace using the Czochralski method, characterized in that, After the crystal growth enters the constant diameter growth stage, phosphine gas is introduced into the furnace. The phosphine gas decomposes into elemental phosphorus and hydrogen under the high temperature environment in the furnace. Elemental phosphorus melts into the silicon melt in the furnace atmosphere, continuously compensating for the phosphorus element lost in the silicon melt due to surface volatilization. Hydrogen is discharged along with the protective gas in the furnace.
2. The method for growing ultra-low resistivity heavily phosphorus-doped silicon single crystals according to claim 1, characterized in that, During the crystal growth stages of crystal initiation and shoulder formation, phosphine gas is introduced into the furnace to compensate for the phosphorus loss in the silicon melt due to surface volatilization.
3. The method for growing ultra-low resistivity heavily phosphorus-doped silicon single crystals according to claim 1 or 2, characterized in that, The flow rate of phosphine gas is dynamically adjusted according to the crystal growth process to match the amount of elemental phosphorus replenished with the amount of phosphorus volatilized and lost in the silicon melt.
4. The method for growing ultra-low resistivity heavily phosphorus-doped silicon single crystals according to claim 3, characterized in that, The flow rate of the phosphine gas is in the range of 1-20 slpm.
5. The method for growing ultra-low resistivity heavily phosphorus-doped silicon single crystals according to claim 3, characterized in that, The formula for determining whether phosphorus is in dynamic equilibrium in a single crystal furnace is: Phosphine supply rate = Crystal solidification carry-away rate + Melt surface volatilization rate.
6. A growth apparatus for ultra-low resistivity heavily phosphorus-doped silicon single crystals, comprising a single crystal furnace (5) and a control system (6), characterized in that, It also includes a phosphine system, which includes an independent phosphine gas cylinder (1) and an independent phosphine gas pipeline (2). The independent phosphine gas cylinder (1) is located outside the single crystal furnace (5). One end of the independent phosphine gas pipeline (2) is connected to the outlet of the independent phosphine gas cylinder (1), and the other end is connected to the gas inlet on the single crystal furnace (5).
7. The growth apparatus for ultra-low resistivity heavily phosphorus-doped silicon single crystals according to claim 1, characterized in that, The independent phosphine gas supply pipeline (2) is also connected to a mass flow meter (3). The mass flow meter (3) is connected to the control system (6) in communication. The control system (6) adjusts the mass flow meter (3) according to the crystal growth process to realize the dynamic adjustment of the phosphine gas flow rate.
8. The growth apparatus for ultra-low resistivity heavily phosphorus-doped silicon single crystals according to claim 1, characterized in that, The air inlet is positioned above the surface of the silicon melt (10) inside the single crystal furnace (5).
9. The growth apparatus for ultra-low resistivity heavily phosphorus-doped silicon single crystals according to claim 1, characterized in that, The air inlet is located on the throat flange (11) of the single crystal furnace (5).
10. The growth apparatus for ultra-low resistivity heavily phosphorus-doped silicon single crystals according to claim 9, characterized in that, The air inlet includes an air inlet port (4) and an air outlet port (12). The air inlet port (4) is set as one and is located on the outer diameter surface of the throat flange (11) of the single crystal furnace (5). The air outlet ports (12) are set as 3-8 and are evenly distributed along the circumference on the inner diameter surface of the throat flange (11). The air inlet port (4) and all the air outlet ports (12) are connected by a built-in pipe (13) located in the throat flange (11). The independent phosphine gas supply pipe (2) is connected to the air inlet port (4).