A method for growing rare earth garnet single crystal material on a recycled substrate
By using a block substrate with a thickness of 4mm to 8mm and grinding and polishing it after each growth, the problem of the difficulty in recycling garnet substrates was solved, enabling the repeated use of rare earth garnet single crystal materials and reducing raw material costs and process modification costs.
Patent Information
- Application Number
- CN202611476263.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-20
AI Technical Summary
In existing liquid phase epitaxy methods, garnet substrates are thin and difficult to recycle, resulting in high raw material costs. Furthermore, existing recycling solutions are complex and costly.
Using a block substrate with a thickness of 4mm to 8mm, a rare earth garnet single crystal material layer is grown by liquid phase epitaxy. After each growth, the substrate is restored by grinding and polishing, enabling multiple reuses, simplifying process steps and reducing costs.
It significantly reduces the raw material cost of single rare earth garnet crystal materials, grows rare earth garnet crystal materials with a thickness of 0.7-1.2mm, has a low cracking rate, a simple process flow, is suitable for existing production lines, and reduces the cost of process modification.
Smart Images

Figure CN123132989A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of liquid phase epitaxial single crystal growth technology, specifically to a method for growing rare earth garnet single crystal materials using a reusable substrate. Background Technology
[0002] Rare earth garnet single crystal thin film magneto-optical materials are usually prepared by liquid phase epitaxy. This method involves immersing one side of a garnet substrate (such as calcium magnesium zirconium doped gadolinium gallium garnet substrate, abbreviated as SGGG substrate; or gadolinium gallium garnet substrate, abbreviated as GGG substrate) into a supersaturated solution, and controlling the supercooling by programmed cooling to allow rare earth garnet single crystals to be epitaxially precipitated at the substrate contact interface.
[0003] In existing technologies, the garnet substrates (GGG or SGGG) used in liquid phase epitaxy are typically 3-inch sheet substrates with a thickness of approximately 0.5 mm, or 4-inch sheet substrates with a thickness of 0.5 mm / 1.0 mm. Due to the thinness of the sheet substrates, they are difficult to recycle after each liquid phase epitaxial growth, essentially making them disposable items. In recent years, the continuous rise in international rare earth raw material prices has significantly increased the procurement cost of garnet substrates, becoming a major factor restricting the large-scale application of liquid phase epitaxy. Therefore, how to achieve multiple reuses of garnet substrates and reduce the raw material cost per unit product is a pressing technical problem to be solved in this field.
[0004] While there are existing technologies that allow for substrate reuse by introducing a bilayer graphene release layer on the substrate surface (such as Chinese patent CN115537915B), this approach requires the additional preparation of a graphene interlayer, involves complex process steps, and has high production costs, thus limiting its practical application in large-scale production. Summary of the Invention
[0005] To address the problems of thin sheet-like garnet substrates, difficulty in recycling after each growth, and high raw material costs in existing liquid phase epitaxy methods, this invention proposes a crystal growth method that reuses substrates. This method can reuse bulk substrates multiple times to grow rare earth garnet single crystals on a single substrate, thereby significantly reducing the raw material cost of a single rare earth garnet single crystal.
[0006] This invention provides a method for growing rare-earth garnet single-crystal materials using a reusable substrate, comprising growing a rare-earth garnet single-crystal material layer on a garnet single-crystal substrate by liquid-phase epitaxy, specifically including the following steps: (1) The garnet single crystal substrate is a block substrate with a thickness of 4mm~8mm. The block substrate is fixed by a substrate clamp. After preheating the block substrate, the block substrate is brought into contact with a supersaturated molten phase. Rare earth garnet single crystal material layer is grown on the growth surface of the block substrate by liquid phase epitaxy. The supercooling condition ΔT of liquid phase epitaxy is controlled in the range of 5~15℃.
[0007] (2) After growth, the obtained rare earth garnet single crystal material layer is separated from the bulk substrate by wire cutting, while retaining a rare earth garnet single crystal material with a thickness of 0.1 mm to 0.3 mm as a retention layer. Preferably, the thickness of the retention layer is 0.1 mm to 0.3 mm.
[0008] (3) The retained layer is removed by grinding and polishing to restore the growth surface of the bulk substrate to meet the liquid phase epitaxial growth conditions, so as to obtain a reusable bulk substrate.
[0009] (4) Repeat steps (1) to (3) to achieve multiple reuses of the bulk substrate.
[0010] The substrate fixture is provided with a fixture heat-conducting plate and a fixture support foot. The fixture heat-conducting plate is slidably sleeved onto the fixture support foot through a through hole. The growth coefficient is the ratio of the thickness of the bulk substrate to the thickness of the rare earth garnet single crystal material layer, and the growth coefficient ranges from 6 to 10.
[0011] Preferably, the thickness of the heat-conducting sheet in the clamp is 1-2 mm.
[0012] Furthermore, the substrate fixture also includes a stabilizing bracket and a connecting rod; one end of the connecting rod is connected to the liquid phase epitaxy equipment to realize the lifting and rotation of the substrate fixture, and the other end is connected to the fixture support foot and fixed by the stabilizing bracket.
[0013] Preferably, the growth thickness of the rare earth garnet single crystal material layer is 0.7 mm to 1.2 mm.
[0014] Furthermore, in step (3), the thickness of the loss caused to the bulk substrate by each grinding and polishing removal operation is 0.1mm-0.2mm.
[0015] Furthermore, the bulk substrate is made of calcium magnesium zirconium doped gadolinium gallium garnet or gadolinium gallium garnet, and the crystal orientation of the rare earth garnet single crystal material layer is consistent with the crystal orientation of the bulk substrate.
[0016] Further, in step (1), the oxide raw materials and flux are added to the crucible and heated to the crystal growth temperature at a heating rate of 5~10℃ / min. After stirring for 6~8h, the stirring rod is removed and the temperature is maintained for another 5~6h. After the material is melted, the block substrate is brought into contact with the melt to start growing the rare earth garnet single crystal material layer.
[0017] Further, in step (1), after fixing the bulk substrate to the substrate fixture, the bulk substrate is preheated for 20-30 minutes. After the temperature stabilizes, the descent program is started to bring the bulk substrate into contact with the molten phase.
[0018] Preferably, the bulk substrate is prepared by the following steps: S1, synthesizing polycrystalline material: pre-treating the raw materials, preparing a polycrystalline material mixed precursor, ball milling and sieving the precursor in an inert atmosphere, performing a first calcination to obtain initial polycrystalline material grains, and then performing a second calcination to obtain polycrystalline material; S2, feeding the polycrystalline material into a furnace for melting, taking a seed crystal with the same crystal orientation as the rare earth garnet single crystal material layer, and performing bulk substrate crystal growth; S3, crystal introduction: eliminating dislocations introduced during seed crystal contact by a necking method; S4, shoulder formation: controlling the shoulder angle to gradually increase the crystal diameter to the target diameter; S5, constant diameter growth: maintaining the target diameter, continuing to grow until the thickness of the constant diameter region reaches 4mm~9mm; S6, tailing: heating and increasing the pulling rate to reduce the crystal diameter until the crystal diameter is less than 10mm before extraction; S7, processing: cutting off the tail, grinding and polishing the bottom of the constant diameter region to meet the conditions for liquid phase epitaxial growth.
[0019] Preferably, the crystal orientation deviation of the bulk substrate is <0.5°; the surface roughness Ra is ≤1nm; and the total thickness deviation TTV is ≤6μm.
[0020] Compared with the prior art, the present invention has achieved the following beneficial effects: 1. This invention replaces the traditional sheet substrate with a thickness of about 0.50 mm with a block substrate with a specific thickness (preferably 4 mm to 8 mm), and restores the substrate growth surface by grinding and polishing after each growth cycle. This allows the same substrate to be reused 20 to 30 times in multiple growth cycles, solving the problem that thick substrates cannot be reused and significantly reducing the substrate raw material cost per unit product.
[0021] 2. In existing technologies, a 0.5mm thick SGGG substrate can only be used once, resulting in a rare-earth garnet single-crystal film thickness of no more than 500 micrometers, and a high cracking rate. This invention, using a bulk SGGG substrate, can grow rare-earth garnet single-crystal materials with a thickness of 0.7-1.2mm, with an even lower cracking rate; after deducting 200-300 micrometers of cutting loss, an optimal product thickness of 0.5-1.0mm can be obtained.
[0022] 3. This method does not require the preparation of an additional intermediate release layer such as bilayer graphene on the substrate surface. The process is simple, and all operation steps are compatible with existing conventional liquid phase epitaxial production equipment and processes. It can be directly promoted and applied on existing production lines with only tooling improvements and process adjustments, which reduces the cost of process modification and technical threshold. Attached Figure Description
[0023] Figure 1 This is a schematic diagram of a rare earth garnet single crystal material grown on a bulk substrate and its surface via liquid-phase epitaxial growth.
[0024] Figure 2 This is a schematic diagram of the substrate fixture of the present invention.
[0025] Figure 3 yes Figure 2 A photograph of the actual substrate fixture.
[0026] Figure 4 yes Figure 3 A photograph of the actual heat-conducting plate in the middle clamp.
[0027] Figure 5 This is a graph showing the relationship between the thickness of the grown film, the difficulty coefficient of process control, and the yield rate of the product.
[0028] Figure 6 This is a photograph of rare earth garnet single crystal material grown on the surface of a bulk substrate using the preparation method of this invention.
[0029] Labeling Explanation: 100, bulk substrate; 200, rare earth garnet single crystal material layer; 300, substrate clamp; 1, clamp heat-conducting plate; 2, clamp support foot; 3, stabilizing bracket; 4, connecting rod; 5, protruding part. Detailed Implementation
[0030] The technical solution of the present invention is illustrated below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not preclude the existence of other method steps before or after the combined steps, or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the present invention. Furthermore, unless otherwise stated, the numbering of each method step is merely a convenient tool for identifying each method step, and not for limiting the order of the method steps or defining the scope of the present invention. Changes or adjustments to their relative relationships, without substantially altering the technical content, should also be considered within the scope of the present invention.
[0031] Example 1 This embodiment uses a calcium magnesium zirconium doped gadolinium gallium garnet (SGGG) bulk substrate 100 as an example to illustrate the growth process of the bulk substrate 100 and the complete method for liquid phase epitaxial growth of rare earth garnet single crystal material layer 200 on the bulk substrate 100.
[0032] (1) Growth process of SGGG bulk substrate 100 Step S101, Polycrystalline Material Synthesis: The raw materials are pretreated to prepare a polycrystalline material mixed precursor. The precursor is ball-milled and sieved in an inert atmosphere and then calcined once to obtain the initial polycrystalline material grains. The initial polycrystalline material grains are then calcined a second time to finally obtain the desired polycrystalline material.
[0033] In step S102, the obtained polycrystalline material is fed into the furnace for melting, and a seed crystal with the same crystal orientation as the rare earth garnet single crystal material layer 200 is taken for SGGG crystal growth.
[0034] Step S103, crystal introduction: The necking method is used to eliminate dislocations introduced during seed crystal contact, ensuring the quality of the crystals grown subsequently.
[0035] Step S104, shoulder formation: Control the shoulder angle to gradually increase the crystal diameter to the target diameter. Ensure that there is no large fluctuation in diameter during the shoulder formation process by adjusting the temperature field or process.
[0036] Step S105, constant diameter growth: Maintain the target diameter and continue growing until the constant diameter length reaches 9mm.
[0037] Step S106, Finishing: Reduce the crystal diameter at a certain angle by increasing the temperature and speed until the crystal diameter is less than 10mm, then remove it.
[0038] Step S107, Processing: Take the grown crystal, cut off the tail, and grind and polish the bottom of the equal diameter section to obtain a block substrate 100, so that it meets the conditions for liquid phase epitaxial growth of rare earth garnet single crystal material layer 200, including but not limited to: ① crystal orientation deviation < 0.5°; ② surface roughness Ra ≤ 1nm; ③ no scratches, pits or other defects on the surface; ④ total thickness deviation TTV ≤ 6μm.
[0039] (2) Liquid phase epitaxial growth of rare earth garnet single crystal material on bulk substrate 100 The bulk substrate used, such as 100 Figure 1 As shown, the thickness is 4mm~8mm, and it is suitable for diameters of 3 inches or 4 inches.
[0040] The oxide raw materials and flux for growing rare-earth garnet single crystals are placed in a crucible and heated to the crystal growth temperature, for example, 1200-1600℃, at a heating rate of 5-10℃ / min. The mixture is then stirred in a stirring apparatus for 6-8 hours, removed from the apparatus, and held at that temperature for another 5-6 hours until the material is fully cured. Oxide raw materials include bismuth oxide, iron oxide, and rare-earth oxides. Fluxes include boron oxide and silicon oxide.
[0041] The substrate fixture 300 used in this invention includes a fixture heat-conducting plate 1 with a thickness of 1-2 mm, fixture support feet 2, a stabilizing bracket 3, and a connecting rod 4. One end of the connecting rod 4 is connected to the liquid phase epitaxy equipment to realize the lifting and rotation of the substrate fixture 300, and the other end is connected to the fixture support feet 2 and fixed by the stabilizing bracket 3. The fixture heat-conducting plate 1 has several through holes along the circumferential direction, and the fixture support feet 2 pass through the through holes, with the fixture heat-conducting plate 1 slidably sleeved on the fixture support feet 2. (See reference...) Figures 2 to 4 The substrate fixture 300 shown, wherein Figure 2 This is a structural diagram. Figure 3 A photograph of the actual substrate fixture 300. Figure 4 This is a photograph of the heat-conducting plate 1 in the substrate fixture 300. In use, the bulk substrate 100 is placed on the protrusion 5 of the fixture support foot 2. The protrusion 5 contacts the bottom of the bulk substrate 100 for positioning and support, while the side of the bulk substrate 100 that does not contact the molten metal directly contacts the heat-conducting plate 1. The heat-conducting plate 1 can move vertically to accommodate bulk substrates 100 of different thicknesses. The structure of this substrate fixture 300 ensures the bulk substrate 100 maintains a stable posture during high-temperature growth, while optimizing the thermal field distribution and reducing stress concentration caused by uneven temperature gradients, thereby effectively suppressing crystal cracking. Furthermore, the heat-conducting plate 1 is made of platinum and materials compatible with the growth atmosphere, possessing both good thermal conductivity and chemical inertness, preventing impurities from contaminating the melt.
[0042] The SGGG bulk substrate 100 is fixed on Figure 2 On the substrate fixture 300 shown, through the fixture heat-conducting plate 1 on the substrate fixture 300, when the block substrate 100 contacts the molten liquid surface, some of the fixture support feet 2 will also contact the molten liquid. The heat of the molten liquid is quickly transferred to the fixture heat-conducting plate 1 and then to the upper surface of the block substrate 100. At this time, the heat of the upper and lower surfaces of the block substrate 100 is conducted together, which makes the heating of the block substrate 100 more uniform and can reduce the difference in the coefficient of thermal expansion of the block substrate 100.
[0043] The lowering mechanism is activated to preheat the bulk substrate 100 at the furnace opening for 20-30 minutes at a temperature of 500-600℃. After the temperature of the crystal growth furnace crucible stabilizes, the lowering mechanism is activated again to bring the bulk substrate 100 into contact with the molten phase, thus initiating the growth of the rare earth garnet single crystal material layer 200. After growth is completed, the substrate is cooled down, and then the bulk substrate 100 and the rare earth garnet single crystal material layer 200 grown on its surface are removed.
[0044] Following the above steps, when the thickness of the bulk substrate 100 is 7 mm, rare earth garnet single crystal material layers 200 of different thicknesses are grown by controlling the process undercooling condition ΔT. The process undercooling condition ΔT is controlled within the range of 3–25 °C, and the larger the thickness of the rare earth garnet single crystal material layer 200, the smaller the process undercooling ΔT is. The results are shown in Table 1. When the growth thickness of the rare earth garnet single crystal material layer 200 is less than 0.7 mm, the undercooling is large and the growth rate is fast, completing the growth in a short time. However, rapid growth exacerbates the stress mismatch and thermal expansion mismatch between the substrate and the film, resulting in a lower number of intact films. The inventors attempted to grow a thicker rare-earth garnet single crystal material layer 200, and found that if the growth thickness exceeded 1.2 mm, the process difficulty increased significantly; when the thickness exceeded 1.3 mm, a complete rare-earth garnet single crystal material layer 200 could not be obtained. In this case, the supercooling was reduced to an extremely low level and the growth rate was the slowest. However, after the thickness exceeded the limit, the accumulation of lattice mismatch stress and thermal expansion mismatch stress between the substrate 100 and the substrate increased. After exceeding the critical thickness, cracking, dislocation slip, and film surface undulations would occur. At the same time, the thickness uniformity and composition gradient control became more difficult to control, which would directly lead to cracking.
[0045] The inventors attempted to expand the range of film thickness by adjusting process parameters such as supercooling ΔT and substrate lattice constant to adapt to the stress and thermal expansion coefficient during film growth. However, they found that the yield did not change significantly after these adjustments, and the process adjustment became more difficult. Figure 5 As shown, Figure 5 This is a graph showing the relationship between the film thickness, process control difficulty, and yield of the present invention. Given a fixed substrate thickness, the process control difficulty increases dramatically when growing a rare-earth garnet single-crystal material layer 200 with a thickness greater than 1.3 mm. Figure 5 (The difficulty coefficient is expressed as a factor of difficulty). Therefore, this method is applicable to growing rare-earth garnet single-crystal material layers with a thickness of 0.7-1.2 mm. The difficulty coefficient is a proportional constant that correlates the growth thickness with the control of process parameters, ranging from 0 to 100%, with a larger value indicating greater difficulty in achieving the desired result. Process parameter control considers substrate diameter, substrate thickness, undercooling ΔT, and substrate lattice constant, among other factors.
[0046] Table 1. Growth of rare earth garnet single crystal material layers of different thicknesses.
[0047] Example 2, Influence of Bulk Substrate Thickness This embodiment examines the liquid phase epitaxial growth results of different bulk substrate thicknesses 100. Using the growth method of the bulk substrate 100 in Example 1, SGGG bulk substrates 100 with thicknesses of 1 mm, 2 mm, 4 mm, 6 mm, 8 mm, and 10 mm and diameters of 3 inches were grown. Subsequently, the obtained bulk substrates 100 were subjected to liquid phase epitaxial growth to prepare rare earth garnet single crystal material layers 200 with a thickness of 0.9 mm. The number of substrates grown in each group was 10. The results are shown in Table 2.
[0048] For ease of comparison, this embodiment mainly analyzes the results of growing a 0.9 mm thick rare earth garnet single crystal material layer 200 on a bulk substrate of different thicknesses. Similar experimental results can be obtained for rare earth garnet single crystal material layers 200 of other thicknesses.
[0049] As shown in Table 2, the growth of the rare earth garnet single crystal material layer 200 is unsatisfactory regardless of the thickness of the bulk substrate 100. Specifically, when using a bulk substrate 100 with a thickness of 1mm-2mm, the temperature gradient inside and on the surface of the substrate increases significantly during liquid phase epitaxial growth due to its small heat capacity and short heat diffusion path. This leads to increased supercooling at the interface, accelerated nucleation rate, and the easy occurrence of structural defects such as twins and polycrystalline structures in the epitaxial layer. The rare earth garnet single crystal material layer 200 is also prone to breakage and cannot form a complete thin film.
[0050] Using a 10mm thick bulk substrate 100 results in excessive thermal inertia. While the substrate can provide a stable temperature field, a thicker substrate will store more strain energy in the epitaxial layer as elastic strain. Once the critical thickness is exceeded, it will relax by forming a high density of mismatched dislocations, thereby affecting the electrical and optical integrity of the epitaxial layer. Therefore, it is difficult to control the undercooling ΔT and the substrate compatibility in the process of growing rare earth garnet single crystal material layer 200. The resulting rare earth garnet single crystal material layer 200 has quality deviation, with only 2 complete films.
[0051] A bulk substrate 100 with a thickness of 4 mm to 8 mm provides a stable and uniform thermal field, effectively suppressing the increase of interfacial undercooling and helping to maintain a smooth and controllable growth front, thereby promoting high uniformity of composition and thickness. The resulting number of complete films is 7-10, achieving optimal growth quality. Therefore, the substrate thickness of the bulk substrate 100 is preferably 4 mm to 8 mm. Simultaneously, this thickness range allows for multiple reuses of the substrate, balancing growth quality and the number of uses.
[0052] Table 2. Growth of rare earth garnet single crystal material layers on bulk substrates of different thicknesses.
[0053] The inventors confirmed the relationship between the growth factor X (the growth factor is the ratio of substrate thickness to film thickness) and the yield, and therefore conducted multiple verifications. The experimental results are shown in Table 3. According to the results, the optimal growth factor X is 6-10.
[0054] Table 3. Growth of rare earth garnet single crystal material layers with different growth coefficients X.
[0055] Example 3: Reuse of bulk substrates This embodiment illustrates a method for reusing the bulk substrate 100. Using the liquid phase epitaxial growth method of Example 1, a rare earth garnet single crystal material layer 200 with a thickness of about 1 mm is grown on the SGGG bulk substrate 100 with a thickness of 4 mm to 8 mm.
[0056] After growth is complete, the furnace is cooled down, and the bulk substrate 100 and the rare-earth garnet single crystal material layer 200 are removed. For example... Figure 1 As shown, a 0.5-1.0 mm thick layer of rare earth garnet single crystal material 200 is cut along the dicing line for subsequent product processing. Simultaneously, a 0.1-0.3 mm thick layer of rare earth garnet single crystal material 200 is retained on the bulk substrate 100 as a retainer layer. This is to reduce direct wear on the bulk substrate 100 during grinding and polishing, thereby extending its service life. The remaining retainer layer on the surface of the bulk substrate 100 is removed by polishing, restoring the growth surface of the bulk substrate 100 to conditions suitable for liquid phase epitaxial growth. Each grinding and polishing operation results in a loss of approximately 0.1-0.2 mm in thickness on the bulk substrate 100.
[0057] By repeating the above steps of liquid phase epitaxial growth, separation and cutting, and grinding and polishing, the bulk substrate 100 can be reused multiple times. The bulk substrate 100, with a substrate length of 4mm to 8mm, suffers a loss of approximately 0.1-0.2mm per cycle and can be reused 20-30 times. Compared to traditional disposable sheet substrates, the raw material cost per unit product can be reduced to 1 / 20 to 1 / 30. On the other hand, when the remaining thickness of the bulk substrate 100 is less than 2mm, it undergoes conventional processing and is used as a disposable substrate.
[0058] It is understood that the material of the bulk substrate 100 is not limited to calcium magnesium zirconium doped gadolinium gallium garnet, but can also be gadolinium gallium garnet. As long as it has good lattice matching with the rare earth garnet single crystal material layer 200, it can be reused by the method of the present invention.
[0059] Obviously, the diameter of the block substrate 100 is not limited to 3 inches, but can also be 4 inches or other specifications, and the size of the lifting clamp and crucible can be adjusted accordingly.
[0060] It is understood that the thickness of the layer retained on the surface of the bulk substrate 100 is not limited to 0.2 mm, but can be adjusted within the range of 0.1 mm to 0.3 mm according to actual process requirements, so as to protect the bulk substrate 100 body while ensuring the quality of the growth surface after grinding and polishing.
[0061] Figure 6 This is a photograph of rare earth garnet single crystal material grown on the surface of a bulk substrate 100 by the preparation method of the present invention. The rare earth garnet single crystal material layer 200 is separated from the bulk substrate 100 by wire cutting.
[0062] Comparative Example 1 follows the steps and parameters of liquid-phase epitaxial growth of rare earth garnet single crystal material on a bulk substrate 100 in Example 1, except that the heat-conducting fixture 1 is removed, i.e., a fixture without the heat-conducting fixture 1 is used to grow rare earth garnet films of different thicknesses on the surface of the bulk substrate 100. The growth results are shown in Table 4. The yield of the grown material differs significantly from that of this method. This is mainly because the bulk substrate has a large heat capacity and a slow heat diffusion rate, making it difficult to control the supercooling ΔT during liquid-phase growth. This results in a more pronounced warping of the SGGG substrate during the growth of the rare earth garnet single crystal material layer 200. The thicker the grown rare earth garnet single crystal material layer 200, the greater the stress on the SGGG substrate, ultimately leading to excessive warping and complete breakage of both the rare earth garnet single crystal material layer 200 and the SGGG substrate.
[0063] As is known to those skilled in the art, due to factors such as equipment temperature control and environmental fluctuations, lattice mismatch is commonly observed between the doped gadolinium gallium garnet substrate and the Faraday rotator during crystal growth. Therefore, micro-cracks are easily generated during liquid-phase epitaxial growth. Furthermore, the two materials have significantly different coefficients of thermal expansion. Ultimately, this leads to wafer cracking during the cooling process.
[0064] This method is achieved through... Figure 2 The fixture shown, which includes a heat-conducting plate 1, conducts heat to the bulk substrate 100, which can reduce the difference in the thermal expansion coefficient of the substrate, thus ensuring that the yield meets the requirements.
[0065] Table 4. Growth of rare earth garnet single crystal material layers of different thicknesses on conventional substrates.
[0066] The above description is only a preferred embodiment of the present invention and does not limit the technical scope of the present invention in any way. Therefore, any minor modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention shall still fall within the protection scope of the present invention.
Claims
1. A method for growing rare-earth garnet single-crystal materials using a reusable substrate, comprising growing a rare-earth garnet single-crystal material layer on a garnet single-crystal substrate by liquid-phase epitaxy, characterized in that, Specifically, the following steps are included: (1) The garnet single crystal substrate is a block substrate with a thickness of 4mm to 8mm. The block substrate is fixed by a substrate clamp. After the block substrate is preheated, the block substrate is brought into contact with a supersaturated molten phase. A rare earth garnet single crystal material layer is grown on the growth surface of the block substrate by liquid phase epitaxy. The supercooling condition ΔT of the liquid phase epitaxy is controlled in the range of 5 to 15 ℃. (2) After growth, the obtained rare earth garnet single crystal material layer is separated from the bulk substrate by wire cutting, while retaining a rare earth garnet single crystal material with a thickness of 0.1 mm to 0.3 mm as a retention layer; (3) The retained layer is removed by grinding and polishing to restore the growth surface of the bulk substrate to meet the liquid phase epitaxial growth conditions, thereby obtaining a reusable bulk substrate; (4) Repeat steps (1) to (3) to achieve multiple reuses of the bulk substrate; The substrate fixture is provided with a fixture heat-conducting plate and a fixture support foot. The fixture heat-conducting plate is slidably sleeved onto the fixture support foot through a through hole. The ratio of the thickness of the bulk substrate to the thickness of the rare earth garnet single crystal material layer is used as the growth coefficient, and the growth coefficient ranges from 6 to 10.
2. The method according to claim 1, characterized in that, The thickness of the heat-conducting sheet in the clamp is 1-2 mm.
3. The method according to claim 1, characterized in that, The substrate fixture also includes a stabilizing bracket and a connecting rod; one end of the connecting rod is connected to the liquid phase epitaxy equipment to realize the lifting and rotation of the substrate fixture, and the other end is connected to the fixture support foot and fixed by the stabilizing bracket.
4. The method according to claim 1, characterized in that, The growth thickness of the rare earth garnet single crystal material layer is 0.7 mm to 1.2 mm.
5. The method according to claim 1, characterized in that, In step (2), the thickness of the retained layer is 0.1 mm to 0.3 mm; in step (3), the thickness of the loss caused to the bulk substrate by each grinding and polishing removal operation is 0.1 mm to 0.2 mm.
6. The method according to claim 1, characterized in that, The bulk substrate is made of calcium magnesium zirconium doped gadolinium gallium garnet or gadolinium gallium garnet, and the crystal orientation of the rare earth garnet single crystal material layer is consistent with the crystal orientation of the bulk substrate.
7. The method according to claim 1, characterized in that, In step (1), the oxide raw materials and flux are added to the crucible and heated to the crystal growth temperature at a heating rate of 5~10℃ / min. After stirring for 6~8h, the stirring rod is removed and the temperature is maintained for another 5~6h. After the material is melted, the block substrate is brought into contact with the melt to start growing the rare earth garnet single crystal material layer.
8. The method according to claim 1, characterized in that, In step (1), after fixing the bulk substrate to the substrate fixture, the bulk substrate is preheated for 20-30 minutes. After the temperature stabilizes, the descent program is started to bring the bulk substrate into contact with the molten phase.
9. The method according to claim 1, characterized in that, The bulk substrate is prepared by the following steps: S1, synthesizing polycrystalline material: pre-treating the raw materials, preparing a polycrystalline material mixing precursor, ball milling and sieving the precursor in an inert atmosphere, performing a first calcination to obtain the initial polycrystalline material grains, and then performing a second calcination on the initial polycrystalline material grains to obtain polycrystalline material. S2. The polycrystalline material is fed into the furnace for melting, and a seed crystal with the same crystal orientation as the rare earth garnet single crystal material layer is selected for bulk substrate crystal growth; S3. Crystal introduction: Dislocations introduced during seed crystal contact are eliminated by necking method; S4. Shoulder formation: The shoulder angle is controlled to gradually increase the crystal diameter to the target diameter; S5. Constant diameter growth: The target diameter is maintained and growth continues until the thickness of the constant diameter region reaches 4mm~9mm; S6. Tail removal: The temperature is increased and the pulling rate is increased to reduce the crystal diameter until the crystal diameter is less than 10mm and then it is removed; S7. Processing: The tail is cut off, and the bottom of the constant diameter region is ground and polished to meet the conditions for liquid phase epitaxial growth.
10. The method according to claim 1, characterized in that, The bulk substrate has a crystal orientation deviation of <0.5°; a surface roughness Ra ≤1nm; and a total thickness deviation TTV ≤6μm.
Citation Information
Patent Citations
A method for repeatedly using garnet substrate in single crystal epitaxial growth
CN115537915B