Grain seed crystal induction and multi-stage temperature control method

By employing grain seeding and multi-stage temperature control methods, the problems of disordered grain orientation and low aspect ratio in traditional directional solidification processes have been solved, enabling the preparation of high-performance columnar polycrystalline silicon. This improves the mechanical properties and thermal conductivity of the material, meeting the high stability requirements of advanced etching processes.

CN123132991APending Publication Date: 2026-11-20BEIFANG UNIV OF NATITIES +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611436337.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Traditional directional solidification processes have defects in nucleation mechanisms and temperature control, resulting in disordered grain orientation, low aspect ratio, and high internal defect density in columnar polycrystalline silicon, which cannot meet the high stability requirements of advanced etching processes.

Method used

High-performance columnar polycrystalline silicon is formed by employing a grain seeding and multi-stage temperature control method, including crucible pretreatment and seeding layer laying, raw material loading and furnace atmosphere preparation, heating and melting and half-melt shape preservation control, multi-stage temperature-controlled directional solidification growth and multi-stage annealing and cooling. By precisely controlling the temperature gradient and pull-down rate, high-performance columnar polycrystalline silicon is formed.

Benefits of technology

This improved the aspect ratio and orientation deviation control of columnar polycrystalline silicon, enhanced the material's hardness and thermal conductivity, improved the stability and lifespan of plasma etching, and enabled the independent and controllable production of high-end semiconductor silicon materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123132991A_ABST
    Figure CN123132991A_ABST
Patent Text Reader

Abstract

The application discloses a crystal grain seed crystal induction and multi-stage temperature control method and belongs to the technical field of directional solidification preparation of columnar polycrystalline silicon. In view of the problems of random nucleation of the traditional full melting process, disordered grain orientation, low length-diameter ratio, large temperature gradient fluctuation, heat stress concentration and low yield caused by coarse temperature adjustment, the application adopts a square quartz ceramic crucible with a 30-40mm round corner at the bottom, sprays a Si3N4 coating on the inner wall and lays a spherical high-purity polycrystalline silicon seed crystal on the bottom to form an induction layer; complete melting of the upper silicon material and semi-melting of the bottom seed crystal are realized through gradient heating; a 25-step heat insulation bottom plate down-drawing program is adopted, the down-drawing rate is controlled according to the four-stage gradient control, a stable longitudinal temperature gradient of 3-8 DEG C / mm is constructed to guide the directional growth of the crystal; and finally, the heat stress is released through multi-stage annealing and the crystal is drawn out. The method can improve the length-diameter ratio of the columnar crystal to 18:1, control the orientation deviation within 10 DEG, significantly reduce the defect density and improve the mechanical, thermal and resistivity uniformity of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for controlling the temperature of seed crystals, and more particularly to a method for inducing and controlling seed crystals at multiple levels. Background Technology

[0002] As the global semiconductor industry evolves towards advanced processes such as 7nm and 5nm, the large-scale application of 12-inch wafers places stringent demands on the material properties of dry-etched chamber silicon components (exhaust rings, spray heads, focusing rings, etc.). Columnar polycrystalline silicon, with its large-size forming capability, ordered grain boundary structure, and balanced mechanical / thermal / electrical properties, has become the core substrate material for large-size semiconductor silicon components and a key foundational material supporting advanced process chip manufacturing. Directional solidification is the core process for preparing columnar polycrystalline silicon, guiding crystal growth along the heat flow direction by constructing a vertical temperature gradient to achieve columnar crystal structure formation. Traditional directional solidification processes have inherent defects in both nucleation mechanism and temperature control, which are the core bottlenecks restricting the improvement of columnar polycrystalline silicon performance.

[0003] (1) The traditional process adopts the full melting mode of "complete melting followed by cooling and crystallization". After the silicon material is completely melted, the bottom is in a random nucleation state, and the size, density and initial orientation of the crystal nuclei cannot be controlled. Under this mode, a large number of disordered grain boundaries will be generated at the bottom of the silicon ingot. As the solid-liquid interface advances, the columnar crystals tend to diverge to both sides when they grow upward, which eventually results in disordered grain orientation, low aspect ratio (generally only 12:1~15:1), large fluctuation in grain size, and high density dislocations will rapidly proliferate with disordered grain boundaries. The internal defect density of the material is high, which directly restricts the hardness, thermal conductivity and processing performance.

[0004] (2) The traditional ingot casting process only sets 5 steps for pulling down the heat insulation base plate, with large distance intervals and uneven actual pulling speed, resulting in violent fluctuations in the longitudinal temperature gradient and unstable solid-liquid interface morphology. On the one hand, interface fluctuations will aggravate solute segregation and disordered distribution of impurities, resulting in insufficient resistivity uniformity; on the other hand, sudden changes in temperature gradient will cause internal thermal stress concentration, increasing the probability of defects such as dislocations and microcracks, ultimately leading to low product yield (less than 65% in China, while the international advanced level reaches 95%) and poor batch stability.

[0005] (3) Due to the limitations of nucleation and temperature control processes, the overall performance of domestic columnar polycrystalline silicon products is significantly lacking: the columnar crystals have large orientation deviations and insufficient aspect ratios, resulting in severe anisotropy of the material's mechanical properties and making them prone to edge chipping and microcracks during processing; the thermal conductivity, hardness, and other indicators are not up to international advanced levels, and the components have short service life in high-temperature plasma environments; the resistivity uniformity is insufficient, with a radial tolerance of approximately ±0.3Ω. cm cannot meet the high stability requirements of advanced etching processes.

[0006] Against this backdrop, developing a novel directional solidification process that combines seed-induced nucleation with multi-level precise temperature control, thereby controlling the initial state of the grains from the formation source and stabilizing the crystal growth environment during the process, is the core technological direction for overcoming the aforementioned bottlenecks and preparing high-performance columnar polycrystalline silicon. Summary of the Invention

[0007] This invention provides a method for inducing grain seed crystals and multi-level temperature control, aiming to solve the problem of how to prepare high-performance columnar polycrystalline silicon through multi-level temperature control.

[0008] To achieve the above objectives, the specific plan is as follows:

[0009] A method for inducing seed crystals and multi-stage temperature control, including the following steps:

[0010] S1, Crucible pretreatment and seed crystal induction layer laying: A square quartz ceramic crucible with rounded corners at the bottom is selected. A Si3N4 coating is uniformly sprayed on the inner wall of the crucible as a release layer and heterogeneous nucleation control layer. Spherical granular high-purity polycrystalline silicon seed crystals are uniformly laid at the bottom of the crucible to form a seed crystal induction layer.

[0011] S2, Raw material loading and furnace atmosphere preparation: Load electronic-grade high-purity polycrystalline silicon raw material into the crucible, and add dopants according to the target resistivity requirements; close the ingot casting furnace chamber, evacuate to high vacuum and then fill with a protective atmosphere to maintain a slightly positive pressure environment inside the furnace;

[0012] S3, Heating and Melting and Half-Melting Shape Preservation Control: Gradually increase the heater power to raise the furnace temperature to 1420~1450℃, ensuring that the upper silicon material in the crucible is completely melted to form a uniform silicon melt; By dynamically adjusting the heater power in real time, the temperature at the bottom of the crucible is stably controlled at 1360~1380℃, so that the bottom seed crystal layer is kept in a half-melted state.

[0013] S4, Multi-stage Temperature-Controlled Directional Solidification Growth: Employing a 25-step insulated base plate pull-down process, a stable longitudinal temperature gradient of 3~8℃ / mm is constructed within the silicon melt by gradient-controlling the downward movement rate of the insulated base plate, guiding the crystal to grow directionally from bottom to top along the temperature gradient. The entire process is divided into four stages of speed control.

[0014] The solidification ratio is 0-25%, corresponding to a pull-down distance of 0-8cm, and a pull-down rate of 1.3-1.5cm / h.

[0015] The solidification ratio is 25% to 50%, corresponding to a pull-down distance of 8 to 18 cm, and the pull-down rate is 1.1 to 1.3 cm / h.

[0016] The solidification ratio is 50% to 85%, corresponding to a pull-down distance of 18 to 22 cm, and a pull-down rate of 0.9 to 1.1 cm / h.

[0017] The solidification ratio is 85%–100%, and the pull-down rate is 0.6–0.8 cm / h.

[0018] S5, multi-stage annealing and cooling: After the silicon ingot is completely solidified, the heater power is gradually reduced in 3 to 5 stages to perform multi-stage secondary annealing on the silicon ingot, gradually releasing the thermal stress accumulated during crystal growth; after the temperature inside the furnace naturally cools to room temperature, the vacuum is broken, air is introduced, and the furnace is opened to take out the complete columnar polycrystalline silicon ingot.

[0019] Further, in step S1, the quartz ceramic crucible is a square quartz ceramic crucible of a G5 type ingot casting furnace with a specification of 840mm×840mm×510mm; the bottom of the crucible is provided with a 30~40mm rounded corner.

[0020] Further, in step S1, the particle size of the Si3N4 coating is 35μm; spherical granular high-purity polycrystalline silicon seed crystals with a thickness of 2~4cm are uniformly laid at the bottom of the crucible, the seed crystal particle size is controlled at 1~3mm, the nucleation density is 40~60 particles / cm³, and the seed crystal purity is ≥7N.

[0021] Furthermore, in step S1, a polycrystalline silicon baffle is placed vertically on the side wall of the crucible.

[0022] Furthermore, in step S2, the total charge of a single furnace is 600~650kg; the dopant is boron or phosphorus, and the amount added is calculated based on the segregation theory to achieve customized control of the resistivity range.

[0023] Furthermore, in step S2, the protective atmosphere is high-purity argon.

[0024] Furthermore, in step S3, real-time temperature and melting state monitoring are performed through optical observation at the top of the crucible and thermocouple TC2 at the bottom of the crucible, and the heater power is dynamically adjusted to maintain the semi-molten state of the bottom seed crystal.

[0025] Furthermore, in step S3, the specific implementation process of the gradient increase heater power includes: low temperature preheating stage, rapid heating stage, full melting and heat preservation stage, and semi-melting steady-state control stage, corresponding to 25~1200℃, 1200℃~1410℃, 1410~1450℃, and 1360~1380℃, respectively.

[0026] Furthermore, in step S4, the 25-step heat insulation base plate pull-down program starts from a pull-down distance of 4cm, and is set at intervals of 0.9cm up to a pull-down endpoint of 22cm, thereby achieving smooth and stable pull-down rate control.

[0027] Furthermore, in step S5, a four-stage annealing process is employed, with the cooling rate and temperature controlled at each stage as follows:

[0028] First stage: Control the cooling rate to 2~3℃ / min, and keep it at a constant temperature for 2~3 hours after reaching 1250~1300℃;

[0029] Second stage: Control the cooling rate to 1.5~2℃ / min, and after reaching 1000~1100℃, maintain the temperature for 1.5~2 hours;

[0030] Third stage: Control the cooling rate to 1~1.5℃ / min, and after reaching 600~800℃, maintain the temperature for 1~1.5h.

[0031] Fourth stage: Control the cooling rate at 0.8~1℃ / min, and after reaching 300~400℃, allow the furnace to cool naturally to room temperature.

[0032] In summary, the present invention has the following advantages over the prior art:

[0033] (1) Through the comparative test of crucible fillet radius, the influence of crucible fillet radius on the solid-liquid distribution ratio, solid-liquid interface shape and stress distribution was investigated. The optimal crucible fillet radius of 30~40mm was obtained, which made the grain seeding and multi-stage temperature control process more accurate.

[0034] (2) The invention independently designed the ingot furnace heat insulation bottom plate pulling process, increasing the number of steps from 5 to 25, forming a stable temperature gradient (3-8℃ / mm), enabling the columnar crystal length-to-diameter ratio to reach 18:1, and controlling the orientation deviation within 10°. The produced polycrystalline silicon ingots achieve a Vickers hardness of 8.01 GPa and a thermal conductivity of 185 W / (m·K) at 25℃, which is higher than the hardness and thermal conductivity levels of conventional polycrystalline silicon ingots, greatly improving the stability and service life of plasma etching. This technology promotes the directional solidification of polycrystalline silicon from "experience-based control" to "precise and adjustable", providing a leading process solution for the independent control of high-end semiconductor silicon materials. Attached Figure Description

[0035] The accompanying drawings, which are included to provide a further understanding of the invention and form part of this invention, illustrate exemplary embodiments of the invention and are used to explain the invention, but do not constitute an undue limitation of the invention. In the drawings:

[0036] Figure 1 A flowchart of a method for inducing crystal seeding and multi-stage temperature control;

[0037] Figure 2 For crucible shapes with different corner radii;

[0038] Figure 3 The temperature distribution at different crucible radii at T=1000 min (X=50 mm).

[0039] Figure 4 The average temperature at different X-position planes with different crucible fillet radii (T=1000 min).

[0040] Figure 5 The temperature distribution at different crucible radii at T=500 min (X=50 mm);

[0041] Figure 6 The temperature distribution at different crucible radii at T=1200 min (X=50 mm).

[0042] Figure 7 The average temperature at different X-position planes under different crucible fillet radii (T=1200 min).

[0043] Figure 8 The thermal stress distribution under different crucible fillet radii;

[0044] Figure 9 The relationship between the fillet radius of different crucibles and the maximum stress value;

[0045] Figure 10 For the movement of the insulating base plate in the directional solidification system;

[0046] Figure 11 Curves showing the relationship between different insulation base plate positions and time;

[0047] Figure 12 Temperature distribution at different insulated base plate pull-down speeds (X=400 mm);

[0048] Figure 13 Solid-liquid phase distribution at different thermal insulation base plate pull-down speeds;

[0049] Figure 14 Solid-liquid phase distribution at different thermal insulation base plate pull-down speeds (II);

[0050] Figure 15 The stress distribution at different pulling speeds of the insulation base plate at T=500 min;

[0051] Figure 16 The stress distribution at different pulling speeds of the insulation base plate at T=2000 min;

[0052] Figure 17 Stress distribution at different pull-down speeds of the insulation base plate;

[0053] Figure 18 Comparison of measured and simulated TC2 temperature values ​​for the original and optimized schemes;

[0054] Figure 19 This refers to the crystallization part of the polycrystalline silicon ingot furnace purification process.

[0055] Figure 20 An optimized solution for the crystallization part. Detailed Implementation

[0056] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0057] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the exemplary embodiments of the invention. As used herein, the singular form may also include the plural form unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0058] Unless otherwise specifically stated, the relative arrangement, numerical expressions, and values ​​of the components and steps set forth in these embodiments do not limit the scope of the invention. It should also be understood that, for ease of description, the dimensions of the various parts shown in the drawings are not drawn to actual scale. Techniques, methods, and devices known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques, methods, and devices should be considered part of the specification. In all examples shown and discussed herein, any specific values ​​should be interpreted as merely exemplary and not as limitations. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters in the following figures denote similar items; therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.

[0059] like Figure 1 As shown, this invention provides a method for grain seeding and multi-level temperature control, including the following steps:

[0060] S1, Crucible pretreatment and seed crystal induction layer laying: A square quartz ceramic crucible with rounded corners at the bottom is selected. A Si3N4 coating is uniformly sprayed on the inner wall of the crucible as a release layer and heterogeneous nucleation control layer. Spherical granular high-purity polycrystalline silicon seed crystals are uniformly laid at the bottom of the crucible to form a seed crystal induction layer.

[0061] As a preferred option, a square quartz ceramic crucible (typical size 880×880×510mm) suitable for G5 type ingot furnace is selected. The bottom of the crucible cavity is provided with a radius of 30~40mm to optimize the heat field distribution and alleviate stress concentration.

[0062] As a preferred option, the Si3N4 coating has a particle size of 35μm; spherical granular high-purity polycrystalline silicon seed crystals with a thickness of 2~4cm are uniformly laid at the bottom of the crucible, with the seed crystal particle size controlled at 1~3mm and the nucleation density at 40~60 particles / cm³, forming a uniform seed crystal induction layer; the seed crystal purity is ≥7N to avoid contamination by external impurities.

[0063] As a preferred option, a polycrystalline silicon baffle is placed vertically on the side wall of the crucible to prevent the silicon material from falling and damaging the seed crystal layer during subsequent loading and melting, thus ensuring the integrity of the nucleation substrate.

[0064] S2, Raw material loading and furnace atmosphere preparation: Load electronic-grade high-purity polycrystalline silicon raw material into the crucible, and add dopants according to the target resistivity requirements. Close the ingot casting furnace chamber, evacuate to a high vacuum, and then fill with a protective atmosphere to maintain a slightly positive pressure environment inside the furnace, avoiding silicon oxidation and the introduction of impurities such as carbon and oxygen at high temperatures.

[0065] As a preferred option, the total charge of a single furnace is 600~650kg; the dopant is boron or phosphorus, and the amount added is calculated based on the segregation theory to achieve customized control of the resistivity range.

[0066] As a preferred option, the protective atmosphere is high-purity argon.

[0067] High-purity argon refers to argon gas with a purity higher than that of industrial argon (99.99%). Its purity standard in China's GB / T4842-2017 standard for pure argon, high-purity argon, and ultra-pure argon is specified as ≥99.999%, with a total impurity content not exceeding 10 ppm, including ≤1 ppm moisture and ≤0.5 ppm hydrogen. In comparison, industrial argon has a purity of 99.99% and a total impurity content ≤100 ppm, while ultra-pure argon can reach a purity of 99.9999% and a total impurity content ≤1 ppm.

[0068] S3, Heating and Melting and Half-Melting Shape Preservation Control: Gradually increase the heater power to raise the furnace temperature to 1420~1450℃, ensuring that the upper silicon material in the crucible is completely melted to form a uniform silicon melt; By dynamically adjusting the heater power in real time, the temperature at the bottom of the crucible is stably controlled at 1360~1380℃, so that the bottom seed crystal layer is kept in a half-melted state.

[0069] As a preferred method, real-time temperature and melting state monitoring is performed through top optical observation and TC2 thermocouple at the bottom of the crucible, and the heater power is dynamically adjusted to maintain the semi-molten state of the bottom seed crystal.

[0070] As a preferred embodiment, the specific implementation process of the gradient-based heater power enhancement is as follows:

[0071] 1. First gradient: Low temperature preheating stage (room temperature (default 25℃) → 1100~1200℃).

[0072] Power strategy: Apply 25%~35% of the rated power, and slowly increase the temperature at low power;

[0073] Heating rate: Controlled at 3~5℃ / min, and hold at the target temperature for 30~60min after reaching the target temperature;

[0074] Process objective: To remove moisture and impurities adsorbed on the silicon nitride coating and silicon material surface, while ensuring uniform heating of the quartz ceramic crucible, avoiding thermal shock cracking caused by rapid heating, and reducing thermal stress on the crucible.

[0075] 2. Second gradient: rapid heating phase (around 1200℃→1410℃).

[0076] Power strategy: Increase to 60%~75% of rated power to accelerate the heating rate;

[0077] Heating rate: Increased to 8~12℃ / min, rapidly approaching the melting point of silicon (approximately 1410℃).

[0078] Process objective: To enable the silicon material in the upper part of the crucible to quickly reach the melting temperature and shorten the overall melting cycle; at this stage, the melting state of the silicon material is observed through the top optical window, and the temperature of the thermocouple TC2 at the bottom of the crucible is tracked simultaneously.

[0079] 3. Third gradient: Full melting and heat preservation stage (stable at 1410~1450℃).

[0080] Power strategy: Reduce power to 50%~60% of rated power, stop continuous heating, and enter constant temperature insulation mode;

[0081] Heat preservation time: 2~4 hours;

[0082] Process objective: To ensure that the silicon material in the upper part of the crucible is completely melted to form a uniform silicon melt and eliminate the temperature difference inside the melt; during this stage, the temperature of the bottom TC2 is strictly controlled not to exceed 1380℃ through power fine-tuning to avoid the complete melting of the bottom seed crystal layer.

[0083] 4. Fourth gradient: semi-melting steady-state regulation stage.

[0084] Power strategy: Fine dynamic adjustment within the range of 45% to 55% of rated power, with an adjustment accuracy of ±1% to 2% of rated power;

[0085] Control objective: To precisely stabilize the temperature at the bottom of the crucible at 1360~1380℃, so that the bottom seed crystal layer is in a semi-molten state of "surface micro-melting and overall solid phase retention";

[0086] Control basis: Combining the bottom temperature feedback of the TC2 thermocouple with the melt pool depth and remaining solid height observed by the top optical observation, the heater power is finely adjusted in real time to maintain the solid-liquid interface stable inside the seed crystal layer, providing a uniform nucleation substrate for subsequent directional solidification.

[0087] S4, Multi-stage Temperature-Controlled Directional Solidification Growth: This process replaces the traditional 5-step coarse adjustment process with a 25-step refined heat-insulated base plate pull-down procedure. By gradient-controlling the heat-insulated base plate's downward movement rate, a stable longitudinal temperature gradient of 3~8℃ / mm is constructed within the silicon melt, guiding the crystal to grow directionally from bottom to top along the temperature gradient. The entire process is precisely speed-controlled in four stages.

[0088] In the early stage of solidification (solidification ratio 0-25%), the corresponding pull-down distance is 0-8cm: a relatively fast pull-down rate (1.3-1.5cm / h) is adopted to quickly establish a stable longitudinal temperature gradient, induce columnar crystals to nucleate along the bottom seed crystal site and grow upward, and suppress the generation of transverse impurity crystals.

[0089] During the middle stage of solidification (solidification ratio 25%~50%), the corresponding pull-down distance is 8~18cm: a medium pull-down rate (1.1~1.3cm / h) is adopted to maintain a gently convex solid-liquid interface morphology, ensure that columnar crystals grow steadily in the vertical direction, reduce lateral divergence of grains, and improve the consistency of aspect ratio.

[0090] At the end of solidification (solidification ratio 50%~85%), corresponding to a pull-down distance of 18~22cm: slow down the pull-down rate to 0.9~1.1cm / h, reduce the temperature gradient change amplitude, reduce the accumulation of thermal stress inside the crystal, and reduce the probability of the formation of defects such as dislocations and microcracks.

[0091] When solidification reaches the top 15% region (solidification ratio 85%~100%): pull down at a rate of 0.6~0.8cm / h to achieve top resistivity compensation.

[0092] As a preferred embodiment, the 25-step refined heat insulation base plate pull-down program starts from a pull-down distance of 4cm, and is set at intervals of 0.9cm up to a pull-down endpoint of 22cm, to achieve smooth and stable pull-down rate control.

[0093] S5, Multi-stage Annealing and Cooling: After the silicon ingot is completely solidified (solidification ratio = 1), the heater power is gradually reduced in 3-5 stages to perform multi-stage secondary annealing on the silicon ingot, gradually releasing the thermal stress accumulated during crystal growth. After the furnace temperature naturally cools to room temperature, the vacuum is broken, air is introduced, and the furnace is opened to remove the complete columnar polycrystalline silicon ingot.

[0094] As a preferred option, a 4-stage annealing process (within the optimal range of 3-5 stages) is adopted as a typical scheme, with the power, temperature, and process objectives matched as follows:

[0095] 1. First stage: High temperature stress relief annealing (near the solidus line → 1250~1300℃).

[0096] Power adjustment: Smoothly reduce the rated power from 40%~45% at the end of solidification to 30%~35% of the rated power;

[0097] Temperature drop and heat preservation: Control the cooling rate at 2~3℃ / min, and maintain the temperature for 2~3 hours after reaching the target temperature;

[0098] Process function: This is the core stage of stress release. Freshly solidified silicon ingots have high dislocation density and large macroscopic internal stress, while silicon atoms above 1200℃ have strong diffusion ability and active dislocation slip and climb, which can quickly eliminate most of the macroscopic thermal stress generated during solidification, while promoting further diffusion of solute elements, reducing local segregation, and improving resistivity uniformity.

[0099] 2. Second stage: Medium-temperature structural stabilization annealing (1250~1300℃→1000~1100℃).

[0100] Power adjustment: Reduce from 30%~35% of rated power to 20%~25% of rated power;

[0101] Temperature drop and heat preservation: Control the cooling rate at 1.5~2℃ / min, and maintain the temperature for 1.5~2h after reaching the target temperature;

[0102] Processing effect: In the intermediate temperature range, the main function is to release the microscopic internal stress at grain boundaries and substructure levels, inhibit further dislocation proliferation, and stabilize the subcrystalline structure within the grains. During this stage, atomic diffusion capacity decreases; maintaining the temperature ensures sufficient stress relaxation and prevents the accumulation of residual stress.

[0103] 3. Third stage: Slow cooling during the transition from brittle to plastic (1000~1100℃→600~800℃).

[0104] Power adjustment: Reduce from 20%~25% of rated power to 10%~15% of rated power;

[0105] Temperature drop and heat preservation: Control the cooling rate to 1~1.5℃ / min, and maintain the temperature for 1~1.5h after reaching the target temperature;

[0106] Processing effect: This temperature range corresponds to the transition of silicon material from a plastic to a brittle state, which is a high-risk area for microcracks. By slowing down the cooling rate and using isothermal holding, the temperature difference between the inside and outside of the silicon ingot is reduced, avoiding thermal shock-induced surface and corner microcracks, while releasing low-temperature elastic stress.

[0107] 4. Fourth stage: Uniform transition at low temperature (600~800℃→300~400℃).

[0108] Power adjustment: Gradually reduce the power from 10%~15% of the rated power to 5%~8%, then turn off the heater and allow it to cool naturally;

[0109] Temperature drop control: The cooling rate is controlled at 0.8~1℃ / min, and then the furnace is allowed to cool naturally to room temperature.

[0110] Process function: to further homogenize the overall temperature of silicon ingots, avoid excessive temperature difference between the low temperature of the furnace wall and the surface of the silicon ingot, ensure that the silicon ingot smoothly transitions from the annealing temperature zone to room temperature, and finally exits the furnace without significant residual stress.

[0111] Example 1: Analysis of the Influence of Crucible Corner Radius on the Physical Field of Directional Solidification Process

[0112] The crucible, as a container for molten polycrystalline silicon and a key component for heat exchange during directional solidification, significantly influences the quality of polycrystalline silicon ingots. To investigate the specific effect of the crucible's bottom fillet radius on ingot quality, this project designed three sets of comparative experiments with crucibles of different fillet radii. All crucibles used had a uniform basic size of 840 mm × 840 mm × 510 mm; the differences were created solely by varying the bottom fillet radius. The specific structures are as follows: Figure 2 As shown, by comparing and analyzing the thermal field, stress field, and solid-liquid phase distribution characteristics of the ingot casting process under different fillet radii, the influence mechanism of this parameter on the ingot quality can be clarified, providing a basis for the optimized design of the crucible structure.

[0113] (1) The influence of crucible fillet radius on temperature distribution

[0114] To investigate the effect of the radius of the bottom fillet of the crucible on the temperature distribution during the directional solidification process, this invention analyzes the thermal field characteristics under different fillet radii. Figure 3 The temperature distribution at location X=50 mm at T=1000 min is shown. Figure 4 This presents the average temperature variation curves at different X-positions on the plane when the solid-liquid phase volume fraction is 0.6. From Figure 3 and Figure 4 It can be seen that adding rounded corners to the bottom of the crucible did not change the overall trend of temperature distribution; the temperature field still maintained the typical pattern of higher temperatures near the sides and lower temperatures in the middle. Here, T represents the heating time.

[0115] (2) The influence of crucible fillet radius on the solid-liquid distribution ratio and solid-liquid interface shape

[0116] To investigate the effect of crucible fillet radius on solid-liquid distribution and interface morphology, this project analyzed the phase transition process under different fillet radii. Figure 5The solid-liquid phase distribution at position X=0.05 m at T=500 min is presented. As can be seen from the figure, the radius of the crucible fillet has a certain influence on the solid-liquid interface during the solidification stage: as the fillet radius increases, the solid-liquid interface curve becomes smoother, and the tilt angle of the solid-liquid interfaces on both sides gradually decreases. This indicates that increasing the fillet radius is beneficial for improving the solid-liquid interface distribution in the early stage of solidification, reducing interface fluctuations, and creating favorable conditions for stable crystal growth.

[0117] Figure 6 This paper presents contour plots of the solid-liquid interface changes at a position of X=50 mm at T=1200 min, under different crucible fillet radii. The results show that during the mid-solidation stage, the influence of the crucible fillet radius on the solid-liquid interface distribution significantly decreases, and the solid-liquid interface distribution under different fillet radii becomes essentially uniform. Figure 7 As can be seen from the curve, the solidification ratio gradually increases with the increase of the fillet radius during the middle stage of solidification, indicating that the increase of the fillet radius will accelerate the solidification process. However, in terms of the magnitude of the influence, its effect on the solid-liquid ratio in the middle and later stages is relatively small, indicating that the regulatory effect of this parameter on the solidification process is mainly reflected in the initial stage.

[0118] (3) The influence of crucible fillet radius on stress distribution

[0119] The stress analysis results show that the stress in polycrystalline silicon near the bottom gradually decreases as the solidification process progresses. Therefore, to accurately assess the impact of crucible fillet radius on stress distribution, selecting the thermal stress during the initial solidification stage as a representative comparison is appropriate. Figure 8 The thermal stress distribution of polycrystalline silicon at T=500 min (solidification integral of approximately 0.25) is shown under different crucible fillet radii.

[0120] The comparison results show that, without rounded corners, the maximum stress after polycrystalline silicon solidification is concentrated at the bottom corners on both sides. As the rounded corner radius increases, the location of the maximum stress shifts significantly, spreading outwards from the rounded corner symmetry line, and the stress concentration area shows a slight expansion trend. This change indicates that optimizing the rounded corner structure at the bottom of the crucible can alter the spatial characteristics of stress concentration, providing a solution for mitigating localized high stress through structural design.

[0121] Figure 9The figure shows the variation of thermal stress under different crucible corner radii. As can be seen from the figure, the maximum thermal stress of polycrystalline silicon continuously decreases with increasing crucible corner radius: when the corner radius increases from R=0 mm to R=20 mm, the maximum stress decreases from 22.89 MPa to 19.952 MPa, a decrease of 12.8%; when it increases from R=20 mm to R=30 mm, the maximum stress decreases from 19.952 MPa to 18.35 MPa, a decrease of 8%; and when it increases from R=30 mm to R=40 mm, the maximum stress decreases from 18.35 MPa to 17.39 MPa, with the decrease further narrowing to 5.2%. This trend indicates that increasing the corner radius can effectively reduce thermal stress, but the rate of reduction gradually slows down as the radius increases.

[0122] The essence of this phenomenon lies in the fact that rounded corner structures, by optimizing the stress transfer path, can disperse stress concentration in the bottom corner region, allowing the surrounding area to share the load, thereby achieving stress mitigation. However, when the rounded corner radius increases to a certain extent, the stress concentration in the bottom corner region is sufficiently alleviated, and the stress distribution in the surrounding area tends to be flat. At this point, further increasing the rounded corner radius weakens its contribution to reducing the maximum stress, thus the decrease in the maximum stress gradually diminishes. This result provides a quantitative basis for crucible structure optimization; that is, in practical applications, an appropriate rounded corner radius can be selected according to stress control requirements to improve the processing performance of columnar polycrystalline silicon ingots.

[0123] Example 2: The Influence of the Pull-down Speed ​​of the Insulation Base Plate on the Physical Field Distribution in the Directional Solidification Process

[0124] The directional solidification system analyzed in this invention primarily achieves temperature control through the movement of an insulating base plate. Therefore, the pulling speed of the insulating base plate significantly impacts the thermal field distribution, crystal growth morphology, and final ingot quality during the directional solidification process. To explore its specific mechanism, this project comparatively analyzed the effects of different insulating base plate pulling speeds on the directional solidification quality. Figure 10 The image shows the movement and position of different insulation base plates.

[0125] Based on the characteristics of the actual production process, three different pull-down speed schemes for the heat insulation base plate were designed, such as... Figure 11 As shown.

[0126] Considering the phased requirements of the directional solidification process, the pulling speed of the insulation base plate is not a fixed value. A dynamic adjustment strategy of "fast in the early stage and slow in the later stage" is typically adopted: a stable temperature gradient is established in the early stage of solidification through a faster pulling speed, while the speed is slowed down in the later stage to reduce thermal stress accumulation. Scheme 1 shows the moving speed curve of the original production process of the directional solidification system; Schemes 2 and 3, while maintaining the consistent final position of the insulation base plate (i.e., reaching the same position at the end of the entire solidification process), increase the moving speed in the initial stage of solidification to compare the impact of initial speed changes on the solidification process.

[0127] (1) The influence of the pulling speed of the heat insulation base plate on the temperature distribution

[0128] Figure 12 The simulation results show the effect of different thermal insulation plate pulling speeds on temperature distribution. The temperature comparison reveals that, at the same time point, as the thermal insulation plate pulling speed increases from Scheme 1 to Scheme 3, the temperature gradient inside the polycrystalline silicon exhibits a significant increasing trend. The core mechanism of this phenomenon is that increasing the thermal insulation plate pulling speed accelerates the heat exchange process between the low-temperature region at the bottom and the ingot, significantly accelerating the cooling rate of the bottom region. This, in turn, leads to a larger temperature difference along the longitudinal (height) direction of the ingot, and consequently, an increased temperature gradient.

[0129] The temperature distribution cloud map clearly shows that as the pulling speed of the insulating base plate increases, the area of ​​the low-temperature region (the region with a temperature below the melting point) inside the ingot significantly expands. This characteristic directly reflects the change in solidification rate; the expansion rate of the low-temperature region is positively correlated with the advancing speed of the solidification front, indicating that accelerating the pulling speed of the insulating base plate can effectively improve the overall solidification efficiency. However, an excessive increase in the temperature gradient may lead to localized thermal stress concentration. Therefore, in process optimization, it is necessary to balance the relationship between solidification rate and stress control to avoid compromising ingot quality in pursuit of production efficiency.

[0130] (2) Effect of the pulling speed of the heat insulation base plate on the solid-liquid distribution ratio and solid-liquid interface shape

[0131] Figure 13 The results show the solid-liquid phase distribution at two time points, T=750 min and T=1200 min, under different pulling speeds of the insulation base plate.

[0132] from Figure 13As can be seen, the morphology of the solid-liquid interface changes significantly with the increase of the pulling speed of the insulating base plate. Whether in the middle stage of solidification (T=750 min) or the later stage (T=1200 min), the solid-liquid boundary curve gradually becomes flatter, indicating that the increased pulling speed of the insulating base plate accelerates the overall cooling process, especially in the polycrystalline silicon region near the heater, where the temperature drop rate is significantly faster. The convex solid-liquid interface, originally formed by the continuous heating from both heaters, gradually decreases in convexity as the cooling rate of both regions increases, ultimately resulting in a smoother overall solid-liquid interface. This smooth solid-liquid interface helps reduce solute segregation and stress concentration during crystal growth, which is beneficial for improving ingot quality.

[0133] Figure 14 The solid-liquid phase distribution results at T=1500 min and T=2000 min are shown for different insulation base plate pulling speeds. In the later stages of solidification, the degree of solid-liquid interface convexity decreases significantly with increasing insulation base plate pulling speed. Especially for Scheme 3, the solid-liquid interface curve at T=1500 min (solidification ratio approximately 0.85) is close to horizontal, and even shows slight convexity on both sides. This phenomenon is caused by the temperature dropping too quickly in the middle region during the later stages of solidification, while the top surface temperature has not decreased synchronously. The temperature decrease rate on the left and right sides is faster than that on the top. If the pulling speed is too fast, the solid-liquid interface curve will gradually change from a convex shape to a concave shape. Therefore, it is evident that a higher insulation base plate pulling speed is not necessarily better; it needs to be controlled within a reasonable range. Figure 14 Looking at the distribution at T=2000 min (solidification ratio reaches approximately 0.99), as the pull-down speed increases, the area of ​​the uncoiled region at the top left and right corners, which is ultimately surrounded by solid, gradually decreases. This indicates that increasing the pull-down speed can accelerate the solidification process in the top region. As the heater temperature gradually drops below the solidification point and the top surface begins to solidify, it promotes rapid solidification of the area near the top surface, helping to reduce the residual liquid phase in the corner areas.

[0134] (3) Analysis of the influence of the pull-down speed of the heat insulation base plate on stress distribution

[0135] Figure 15The figure shows the stress distribution contour plots at T=500 min under different base plate pulling speeds. As can be seen from the figure, in the initial solidification stage, the overall stress distribution pattern does not change significantly with increasing base plate pulling speed, but the maximum stress value shows a continuous increasing trend. This change is closely related to the evolution characteristics of the temperature field. Increasing the base plate pulling speed accelerates the cooling rate of the polycrystalline silicon bottom region, leading to a larger temperature gradient at the bottom. According to thermal stress theory, the stress magnitude is positively correlated with the temperature change and temperature gradient. Therefore, the increased temperature gradient caused by the increased base plate pulling speed directly leads to a corresponding increase in stress. This result suggests that in process design, it is necessary to balance the relationship between solidification efficiency and stress control to avoid excessive pursuit of speed leading to increased initial stress concentration.

[0136] like Figure 16 The figure shows the stress distribution cloud map at T=2000 min under different base plate pulling speeds. As can be seen from the figure, in the final stage of solidification, the maximum stress value shows a continuous upward trend with the increase of the base plate moving speed, and the location of the maximum stress is always concentrated in the corner areas on both sides, with the stress concentration range also slightly expanding. Furthermore, with the increase of the base plate moving speed, the stress in the middle region of the polycrystalline silicon bottom also shows a certain increasing trend. This is because the base plate moving speed changes significantly in the early stages, resulting in the lower and middle parts of the polycrystalline silicon having already solidified in the early stages of solidification; at the same time, the temperature of the lower and middle polycrystalline silicon continuously decreases with the increase of the base plate moving speed. However, due to the decrease in the change of the base plate moving speed in the later stages of the three schemes, the rate of temperature decrease in the upper and middle parts of the polycrystalline silicon slows down accordingly, and the temperature change at the top of the three schemes gradually becomes more gradual, leading to an increasing temperature difference between the upper and lower regions, and thus causing the bottom stress to exhibit a certain diffusion pattern.

[0137] The quantification results of stress changes in the three schemes at different times are as follows: Figure 17 As shown in the figure, the trend of the values ​​shows that during the adjustment process from Scheme 1 to Scheme 3, the maximum stress at T=500 min increased from 22.89 MPa to 28.64 MPa, an increase of 25.1%; the maximum stress at T=2000 min increased from 46.23 MPa to 53.24 MPa, an increase of 15.2%. This data indicates that the stress change was greater in the early stage than in the later stage, which corresponds perfectly to the movement trajectory characteristics of the base plate, which is "rapid movement in the early stage and slow operation in the later stage," further verifying the staged influence of the base plate's movement speed on the evolution of thermal stress.

[0138] (3) The influence of the pulling speed of the heat insulation base plate on the physical field distribution during the directional solidification process

[0139] The foregoing analysis reveals that the original production scheme still has certain defects in the solid-liquid phase distribution and stress distribution during polycrystalline silicon solidification, such as an insufficiently smooth solid-liquid interface and significant local stress concentration, which adversely affects the ingot quality. Based on the analysis of the influence of crucible fillet radius on the physical field of the directional solidification process, it has been clearly established that the crucible fillet radius and the pulling speed of the insulating base plate are key factors affecting the directional solidification process.

[0140] Through comparative verification of multiple schemes, it was found that using a crucible fillet radius of R=40 mm effectively disperses stress concentration areas and significantly reduces maximum thermal stress. Furthermore, using scheme 2 for the pull-down speed of the heat-insulating base plate not only accelerates solidification to shorten the production cycle but also smooths the solid-liquid interface curve and helps improve the stress distribution after solidification. Based on these optimization effects, the combination of "crucible fillet radius R=40 mm and heat-insulating base plate pull-down speed 2" was selected for actual production. The effectiveness of this optimization scheme will be verified by comparing the quality of the polycrystalline silicon produced in actual production, in order to improve the processing performance of columnar polycrystalline silicon ingots.

[0141] To verify the accuracy of the simulation analysis results, this project will summarize and compare the TC2 temperature curves obtained from actual tests with those calculated by simulation analysis. The results are as follows: Figure 18 As shown.

[0142] from Figure 18 As can be seen, the temperature of TC2 shows a continuous downward trend over time, with the initial temperature drop being significantly faster than the later drop, while the temperature drop gradually leveled off in the later stages. This characteristic corresponds closely to the moving speed curve of the insulating base plate. When the moving speed of the insulating base plate is relatively fast, the distance between it and the heat exchange platform continuously increases, the heat loss rate accelerates, and the temperature drops faster. Conversely, as the moving speed of the base plate slows down in the later stages, heat exchange tends to stabilize, and the temperature drop rate also slows down. Further comparison of the simulation analysis results and experimental test results shows that the temperature change trends of both are basically consistent, exhibiting the characteristic of "rapid temperature drop in the early stage and slow temperature drop in the later stage." Although there is a certain deviation between the absolute values ​​of the simulation analysis results and the experimental test results, the maximum error is about 12%, and the average error is controlled at around 8%, both within the acceptable range for engineering applications. This indicates that the simulation model established in this study can accurately reflect the temperature evolution law of the actual directional solidification process.

[0143] Example 3: Optimization of the process for pulling down the heat insulation bottom plate of the ingot casting furnace

[0144] Traditional polycrystalline casting processes employ a "complete melting followed by cooling and crystallization" model: after the polycrystalline silicon is completely melted, the bottom is cooled by lowering an insulating base plate to initiate the crystallization process. During the cooling and crystallization of the polycrystalline silicon at the bottom, it undergoes random nucleation, making it impossible to control the size and density of the nuclei, resulting in numerous random grain boundaries at the bottom of the silicon ingot. As the solid-liquid interface continues to rise, columnar crystals grow upwards along the temperature gradient, and high-density dislocations proliferate rapidly alongside these disordered grain boundaries.

[0145] This project proposes an innovative process: using 35μm Si3N4 as a spray coating to cover the surface of quartz powder, and then using this quartz powder as a heterogeneous nucleation material. A mesh-structured coating is laid at the bottom of the crucible as a nucleation layer. Compared with polycrystalline silicon produced by traditional processes, the casting process using a quartz coating as a seed layer can effectively improve the minority carrier lifetime of polycrystalline silicon, resulting in lower and more uniform internal impurity content. The resulting polycrystalline silicon solar cells exhibit a 0.52% increase in photoelectric conversion efficiency.

[0146] The total production time for directional solidification of polycrystalline silicon in industry is 55 hours, of which 40 hours are spent reaching the maximum pull-down distance of 22cm. Before crystallization is completed in the corner area, the heat-insulating base plate is first raised and then sealed by the heat-insulating cage, and then lowered. This process lasts for 11 hours.

[0147] Figure 19 The process curve for directional solidification purification of 610 kg silicon raw material is shown, and this process serves as a control group in this project. During the actual pulling process, the pulling distance exhibits a curved shape with slight variations in the degree of curvature. Larger variations occur when adjusting the distance, possibly due to the mechanical structure itself. When the pulling distance changes abruptly, the solidification interface becomes unstable, affecting impurity distribution and crystal structure, ultimately reducing the quality of polycrystalline silicon. From... Figure 19 It is evident that setting the initial process steps to 5, with a large interval, results in uneven actual stretching rates, leading to an unstable state at the solidification interface.

[0148] To address the above issues, the experiment is designed as follows:

[0149] Control group: Using the original industrial process parameters (5-step procedure, large distance interval).

[0150] Experimental Group 1: Keeping the total pull-down distance constant, the process was increased to 25 steps, starting from 4cm and set at 0.9cm intervals up to 22cm. A stable rate curve was achieved through dense parameter control. Figure 20 Simultaneously, a quartz tube is used to monitor the solidification rate in real time.

[0151] Experimental Group 2: Based on Experimental Group 1, combined with the semi-melting method, a 4cm thick layer of 50 particles / cm was laid at the bottom of the crucible. 3The German Wacker polycrystalline silicon seed crystal (total mass 10kg) was used, and the total charge was still 610kg. Key controls: At the end of melting, the height of the remaining solid was measured through the top observation port, and the bottom temperature was adjusted in conjunction with the TC2 (crucible bottom temperature) parameter to ensure that the bottom temperature was ≤1380°C to preserve the seed crystal layer; polycrystalline silicon plates were placed on the side walls of the crucible to prevent the silicon material from falling and being damaged by impact.

[0152] Samples were prepared using the above experimental methods. The results showed that, compared with experimental group one, the defects such as cracks and edge chipping in the subsequent processed products under the same processing conditions were reduced by 45.6% in experimental group two, and the final pass rate of the samples was increased by 27.3%.

[0153] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for inducing seed crystals and multi-stage temperature control, characterized in that, Including the following steps: S1, Crucible pretreatment and seed crystal induction layer laying: A square quartz ceramic crucible with rounded corners at the bottom is selected. A Si3N4 coating is uniformly sprayed on the inner wall of the crucible as a release layer and heterogeneous nucleation control layer. Spherical granular high-purity polycrystalline silicon seed crystals are uniformly laid at the bottom of the crucible to form a seed crystal induction layer. S2, Raw material loading and furnace atmosphere preparation: Load electronic-grade high-purity polycrystalline silicon raw material into the crucible, and add dopants according to the target resistivity requirements; close the ingot casting furnace chamber, evacuate to high vacuum and then fill with a protective atmosphere to maintain a slightly positive pressure environment inside the furnace; S3, Heating and Melting and Half-Melting Shape Preservation Control: Gradually increase the heater power to raise the furnace temperature to 1420~1450℃, ensuring that the upper silicon material in the crucible is completely melted to form a uniform silicon melt; By dynamically adjusting the heater power in real time, the temperature at the bottom of the crucible is stably controlled at 1360~1380℃, so that the bottom seed crystal layer is kept in a half-melted state. S4, Multi-stage Temperature-Controlled Directional Solidification Growth: Employing a 25-step insulated base plate pull-down process, a stable longitudinal temperature gradient of 3~8℃ / mm is constructed within the silicon melt by gradient-controlling the downward movement rate of the insulated base plate, guiding the crystal to grow directionally from bottom to top along the temperature gradient. The entire process is divided into four stages of speed control. The solidification ratio is 0-25%, corresponding to a pull-down distance of 0-8cm, and a pull-down rate of 1.3-1.5cm / h. The solidification ratio is 25% to 50%, corresponding to a pull-down distance of 8 to 18 cm, and the pull-down rate is 1.1 to 1.3 cm / h. The solidification ratio is 50% to 85%, corresponding to a pull-down distance of 18 to 22 cm, and a pull-down rate of 0.9 to 1.1 cm / h. The solidification ratio is 85%–100%, and the pulling speed is 0.6–0.8 cm / h; S5, multi-stage annealing and cooling: After the silicon ingot is completely solidified, the heater power is gradually reduced in 3 to 5 stages to perform multi-stage secondary annealing on the silicon ingot, gradually releasing the thermal stress accumulated during crystal growth; after the temperature inside the furnace naturally cools to room temperature, the vacuum is broken, air is introduced, and the furnace is opened to take out the complete columnar polycrystalline silicon ingot.

2. The method for inducing and multi-stage temperature control of grain seed crystals according to claim 1, characterized in that, In step S1, the quartz ceramic crucible has an inner cavity size of 840×840×510mm and is a square quartz ceramic crucible for a G5 type ingot casting furnace; the bottom of the crucible is provided with a rounded corner with a radius of 30~40mm.

3. The method for inducing and multi-stage temperature control of grain seed crystals according to claim 1, characterized in that, In step S1, the particle size of the Si3N4 coating is 35μm; spherical high-purity polycrystalline silicon seed crystals with a thickness of 2~4cm are uniformly laid at the bottom of the crucible, the particle size of the polycrystalline silicon seed crystals is controlled at 1~3mm, and the nucleation density is 40~60 particles / cm³; the purity of the high-purity polycrystalline silicon seed crystals is ≥7N.

4. The method for inducing and multi-stage temperature control of grain seed crystals according to claim 1, characterized in that, In step S1, a polycrystalline silicon baffle is placed vertically on the side wall of the crucible.

5. The method for inducing and multi-stage temperature control of grain seed crystals according to claim 1, characterized in that, In step S2, the total charge of a single furnace is 600~650kg; the dopant is boron or phosphorus, and the amount added is calculated based on the segregation theory to achieve customized control of the resistivity range.

6. The method for grain seed induction and multi-stage temperature control according to claim 1, characterized in that, In step S2, the protective atmosphere is high-purity argon.

7. The method for grain seed induction and multi-stage temperature control according to claim 1, characterized in that, In step S3, real-time temperature and melting state are monitored by optical observation at the top of the crucible and thermocouple TC2 at the bottom of the crucible, and the heater power is dynamically adjusted to maintain the semi-molten state of the bottom seed crystal.

8. The method for inducing and multi-stage temperature control of grain seed crystals according to claim 1, characterized in that, In step S3, the specific implementation process of the gradient increase heater power includes: low temperature preheating stage, rapid heating stage, full melting and heat preservation stage and semi-melting steady state control stage, corresponding to 25~1200℃, 1200℃~1410℃, 1410~1450℃ and 1360~1380℃ respectively.

9. The method for grain seed induction and multi-stage temperature control according to claim 1, characterized in that, In step S4, the 25-step heat insulation base plate pull-down program starts from a pull-down distance of 4cm, and is set at intervals of 0.9cm up to a pull-down endpoint of 22cm, so as to achieve smooth and stable pull-down rate control.

10. The method for grain seed induction and multi-stage temperature control according to claim 1, characterized in that, In step S5, a four-stage annealing process is adopted, and the cooling rate and temperature are controlled in each stage as follows: First stage: Control the cooling rate to 2~3℃ / min, and keep it at a constant temperature for 2~3 hours after reaching 1250~1300℃; Second stage: Control the cooling rate to 1.5~2℃ / min, and after reaching 1000~1100℃, maintain the temperature for 1.5~2 hours; Third stage: Control the cooling rate to 1~1.5℃ / min, and after reaching 600~800℃, maintain the temperature for 1~1.5h. Fourth stage: Control the cooling rate at 0.8~1℃ / min, and after reaching 300~400℃, allow the furnace to cool naturally to room temperature.