A method for preparing a spherical single-crystal lithium-rich manganese-based positive electrode material by using a high-entropy molten salt system to assist reaction
By using a high-entropy molten salt system to assist the reaction, the problem of easy grain boundary cracking in lithium-rich manganese-based cathode materials during high-voltage charge and discharge was solved, achieving single crystallization and regular spherical morphology, and improving the cycle stability and voltage retention capability of the material.
Patent Information
- Application Number
- CN202611286573.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-24
- Publication Date
- 2026-11-20
AI Technical Summary
Existing lithium-rich manganese-based cathode materials suffer from grain boundary cracking, rapid voltage decay, and poor cycle stability during high-voltage charge-discharge and long-term cycling, making it difficult to achieve synergistic control of single-crystal structure and regular spherical morphology through traditional methods.
A high-entropy molten salt system was used to assist the reaction, and a liquid phase environment was constructed at low temperature. A quasi-spherical single crystal precursor was formed through a co-precipitation reaction. Under liquid phase conditions, the diffusion of lithium ions and transition metal ions and crystal reconstruction were carried out to obtain a grain boundary-free quasi-spherical single crystal material.
The single crystallization and regular spherical particle morphology of lithium-rich manganese-based cathode materials were achieved, which significantly suppressed particle cracking and voltage decay, and improved the cycle stability and applicable process window of the materials.
Smart Images

Figure CN123132999A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery cathode material technology, specifically to a method for preparing spherical single-crystal lithium-rich manganese-based cathode materials using a high-entropy molten salt system-assisted reaction. Background Technology
[0002] Lithium-rich manganese-based cathode materials are considered crucial for achieving high-energy-density lithium-ion batteries due to their theoretical specific capacity exceeding 250 mAh / g. However, existing lithium-rich manganese-based cathode materials are mostly prepared using traditional high-temperature solid-state reaction methods, resulting in polycrystalline secondary particles formed by the aggregation of multiple primary grains, with numerous grain boundaries within these particles. During high-voltage charge-discharge and long-term cycling, these grain boundaries readily become preferential sites for stress concentration, electrolyte erosion, and structural phase transitions, leading to particle cracking, rapid voltage decay, and reduced cycle stability, severely hindering the practical application of lithium-rich manganese-based cathode materials.
[0003] While single-crystal cathode materials can effectively avoid grain boundary-related failures, lithium-rich manganese-based materials, due to their complex composition and diverse reaction pathways, present challenges in achieving synergistic control of single-crystal structure and regular spherical morphology using traditional solid-state reaction methods, ensuring sufficient reaction. Therefore, a novel preparation method is urgently needed to achieve the controllable fabrication of near-spherical single-crystal lithium-rich manganese-based cathode materials. Summary of the Invention
[0004] The purpose of this invention is to provide a method for preparing a spherical single-crystal lithium-rich manganese-based cathode material. By introducing a high-entropy molten salt system during the calcination process, a liquid-phase assisted reaction environment is constructed, and sufficient mass transport and crystal rearrangement are achieved at a lower temperature, thereby obtaining a spherical lithium-rich manganese-based cathode material with a regular morphology composed of a single crystal.
[0005] This invention provides a method for preparing spherical single-crystal lithium-rich manganese-based cathode materials using a high-entropy molten salt system-assisted reaction, comprising the following steps: (1) Dissolve nickel salt and / or cobalt salt, and manganese salt in a solvent to obtain a mixed transition metal salt solution; (2) The transition metal mixed salt solution and the precipitant solution are added to the reactor simultaneously to form precursor particles through a co-precipitation reaction; (3) The obtained precursor is subjected to aging treatment so that the precursor nuclei continue to grow under the condition that no secondary nucleation occurs, forming spherical single crystal precursor particles. (4) The quasi-spherical single crystal precursor is mixed with a lithium source and a high-entropy molten salt system, wherein the high-entropy molten salt system is a multi-component eutectic system containing three or more components, formed by the combination of different cations and anions, and the high-entropy molten salt system must satisfy 2.5R≤ ≤3.5R, where, ΔS mix denoted as , where is the mixing entropy of cations and anions in the molten salt system, in J / mol / K; R is the gas constant, R = 8.314 J / mol / K; and n is the number of effective components participating in the mixing of the molten salt system. The mole fraction of anions in the i-th salt component; Let be the mole fraction of cations in the j-th salt component; ln is the natural logarithm. (5) Heating in an oxygen atmosphere or an air atmosphere to melt the high-entropy molten salt system and promoting the diffusion, rearrangement and crystal structure reconstruction of lithium ions and transition metal ions under liquid-phase assisted conditions; (6) After being cooled by high temperature treatment in step (5), the residual molten salt is removed by water washing to obtain a spherical single crystal lithium-rich manganese-based cathode material.
[0006] Preferably, the co-precipitation reaction in step (2) is carried out under conditions of pH 10.5~11.5 and temperature 40~70℃.
[0007] Preferably, the aging treatment time in step (3) is 6~24 h.
[0008] Preferably, the lithium source is selected from lithium carbonate, lithium hydroxide, or a combination thereof.
[0009] Preferably, in the high-entropy molten salt system, the cation is selected from Li + Na + K + Mg 2+ Ca 2+ Al 3+ Cs + One or more of the following; the anion is selected from Cl. - NO3 - CO3 2- SO4 2- PO4 3- F - One or more of them.
[0010] Preferably, the high-entropy molten salt system is any one of the following five-membered salt components: LiNO3-NaCl-K2CO3-MgSO4-CaCl2, LiNO3-NaNO3-KCl-Li2SO4-CaCO3, LiCl-NaCl-KNO3-MgCl2-CaSO4, LiF-NaNO3-KCl-MgSO4-CaCO3, and LiNO3-NaCl-K2CO3-MgSO4-Li3PO4.
[0011] Preferably, the high-entropy molten salt system is any one of the quaternary salt components selected from LiNO3-NaCl-K2CO3-CaSO4, LiNO3-NaCl-K2SO4-MgCO3, LiF-NaNO3-KCl-CaSO4, LiNO3-NaF-KCl-MgSO4, and LiCl-NaNO3-K2CO3-CaSO4.
[0012] The ΔS / R values for the above pentagonal and tetravalent salt components are shown in Table 1.
[0013] Table 1. ΔS / R values of different pentagonal and quaternary salt components. Preferably, the melting temperature of the high-entropy molten salt system is below 650°C.
[0014] Preferably, the mass ratio of the high-entropy molten salt system to the spherical single crystal precursor is 0.05 to 3:1.
[0015] Preferably, in step (5), the temperature is heated to 650~950°C in an oxygen atmosphere or an air atmosphere.
[0016] In this invention, by introducing a high-entropy molten salt system, the calcination process is transformed from a traditional solid-solid reaction to a solid-liquid-solid reaction. During heating, the molten salt forms a continuous liquid phase, which significantly increases the diffusion rate of lithium ions and transition metal ions, lowers the diffusion barrier of the solid-phase reaction, and thus avoids the formation of polycrystalline structures due to incomplete local reactions. Simultaneously, the molten salt liquid produces a uniform wetting effect on the precursor particle surface, forming a relatively uniform interfacial tension field on the particle surface. To reduce the total surface energy of the system, the crystals tend to grow isotropically during growth, thereby suppressing preferential growth along specific crystal orientations and avoiding the formation of plate-like or irregular morphologies, ultimately causing the particles to spontaneously evolve into a quasi-spherical structure. Because the liquid phase environment significantly reduces mass transfer resistance, individual crystal nuclei can continue to grow without secondary nucleation, thus obtaining a quasi-spherical single-crystal lithium-rich manganese-based cathode material without internal grain boundaries.
[0017] Compared with the prior art, the present invention has the following beneficial effects: (1) Achieve single crystallization of lithium-rich manganese-based cathode material; (2) Obtain regular spherical particle morphology; (3) Significantly suppress particle cracking and voltage decay; (4) The method is applicable to a wide process window and has high stability. Attached Figure Description
[0018] Figure 1 This is a particle morphology diagram of the near-spherical single-crystal precursor of Embodiment 1 of the present invention; Figure 2This is a particle morphology diagram of the near-spherical single-crystal lithium-rich manganese-based cathode material of Embodiment 1 of the present invention; Figure 3 This is a comparison chart of the cycle performance of the monocrystalline lithium-rich manganese-based cathode material of Example 1 and the polycrystalline lithium-rich manganese-based cathode material of Comparative Example 1; Figure 4 The diagram shows a comparison of the discharge voltage of the monocrystalline lithium-rich manganese-based cathode material in Example 1 and the polycrystalline lithium-rich manganese-based cathode material in Comparative Example 1. Detailed Implementation
[0019] To facilitate understanding of the technical solution of the present invention, the present invention will be further described in detail below through specific embodiments.
[0020] Example 1 Manganese sulfate, nickel sulfate, and cobalt sulfate were dissolved in deionized water at a molar ratio of Mn:Ni:Co = 0.60:0.20:0.20 to prepare a mixed salt solution with a total metal ion concentration of 2 mol / L. This mixed salt solution was then simultaneously added to a reaction vessel along with a sodium hydroxide-ammonia composite precipitant. A co-precipitation reaction was carried out at 50°C. The pH of the reaction system was controlled to be 11.0 ± 0.1 by adjusting the precipitant addition rate. The stirring speed was 400 rpm, and the reaction was continued for 6 h, followed by aging for 12 h. After solid-liquid separation, washing with deionized water, and drying at 120°C for 10 h, a near-spherical single-crystal precursor was obtained.
[0021] The obtained precursor was mixed with lithium carbonate at a molar ratio of Li:(Mn+Ni+Co)=1.20:1, and then added to a high-entropy molten salt system. The high-entropy molten salt system consisted of LiNO3, NaCl, K2CO3, and CaSO4, with a molar ratio of 1:1:1:1.
[0022] The co-configurational entropy of the anions and cations was calculated as: ΔS mix = 2.72R, satisfying the high-entropy molten salt condition. The mass ratio of high-entropy molten salt to precursor is 1:1. The mixture is thoroughly ground and mixed, then placed in a corundum crucible. Under air atmosphere, the temperature is increased to 850℃ at 5℃ / min and held for 10 h. After natural cooling, the molten salt is removed by washing with deionized water, and the mixture is dried at 100℃ for 8 h to obtain a near-spherical single-crystal lithium-rich manganese-based cathode material.
[0023] Example 2 A spherical single-crystal precursor was prepared according to the method in Example 1. The obtained precursor was mixed with lithium carbonate at a molar ratio of Li:(Mn+Ni+Co)=1.20:1, and then added to a high-entropy molten salt system. The high-entropy molten salt system consisted of LiF, NaNO3, KCl, MgSO4, and CaCO3, with a molar ratio of 1:1:1:1:1. The cations in the system included Li... + Na+ K + Mg 2+ and Ca 2+ Anions include F - NO3 - Cl - SO4 2- and CO3 2- The calculation yields: ΔS mix =3.21R.
[0024] The mass ratio of the high-entropy molten salt to the precursor is 1:1. The sintering conditions are the same as in Example 1.
[0025] Example 3 The precursor was prepared according to the method in Example 1. The precursor was mixed with lithium carbonate at a ratio of Li:(Mn+Ni+Co)=1.20:1, and then added to a high-entropy molten salt system. The high-entropy molten salt system consisted of LiF, Na₂SO₄, K₂CO₃, and CsCl in a molar ratio of 1:1:1:1. The cation was Li₂. + Na + K + Cs + The anion is F - Cl - CO3 2- SO4 2- The calculation yields: ΔS mix =2.77R.
[0026] The mass ratio of the high-entropy molten salt to the precursor is 1:1. The sintering conditions are the same as in Example 1.
[0027] Example 4 The precursor was prepared according to the method in Example 1. The precursor was mixed with lithium carbonate at a ratio of Li:(Mn+Ni+Co)=1.20:1, and then added to a high-entropy molten salt system. The high-entropy molten salt system consisted of LiF, NaCl, KNO3, MgSO4, CaCO3, and Li3PO4 in a molar ratio of 1:1:1:1:1:1. The cation was Li. + Na + K + Mg 2+ and Ca 2+ The anion is F - Cl - CO3 2- NO3 - PO4 3- SO4 2- The calculation yields: ΔS mix =3.62R.
[0028] The mass ratio of the high-entropy molten salt to the precursor is 1:1. The sintering conditions are the same as in Example 1.
[0029] Comparative Example 1 The precursor was prepared according to the method in Example 1. The precursor was mixed with lithium carbonate at a ratio of Li:(Mn+Ni+Co)=1.20:1, with only LiNO3 added as the molten salt medium. The LiNO3 contained only Li. + and NO3 - There are two types of ions, and no ion mixing occurs. The calculated value is: ΔS mix =0. The mass ratio of LiNO3 to precursor was 1:1. The same sintering conditions as in Example 1 were used. The resulting material was used as a low-entropy molten salt control sample.
[0030] like Figure 3 As shown, the polycrystalline cathode material prepared in Comparative Example 1 retained 91.1% of its capacity after 100 cycles; while the monocrystalline cathode material obtained in Example 1 retained 99% of its capacity after 100 cycles at 1C. These results indicate that the monocrystalline cathode material prepared in Example 1 exhibits superior cycle stability.
[0031] like Figure 4 As shown, the polycrystalline cathode material prepared in Comparative Example 1 exhibits a voltage decay of 0.55 mV / cycle during cycling; the single-crystal cathode material prepared in Example 1 shows a voltage decay of only 0.16 mV / cycle during cycling at a 1C rate. The comparative results demonstrate that Example 1 can significantly suppress voltage decay during cycling and possesses excellent voltage cycling stability.
[0032] Comparative Example 2 The precursor was prepared according to the method in Example 1. The precursor was mixed with lithium carbonate and then added to a LiCl-KCl binary molten salt system. The molar ratio of LiCl to KCl was 1:1. The cation in this system was Li. + K + The anion is Cl. - Therefore, we can calculate ΔS. mix =0.693R. A comparative material was obtained using the same sintering conditions as in Example 1.
[0033] Comparative Example 3 The precursor was prepared according to the method in Example 1. A ternary molten salt system of LiCl-NaCl-KCl was added. The molar ratio of the three salts was 1:1:1, and the cation in this system was Li. + Na + K + The anion is Cl. - The calculation yields: ΔS mix =1.099R. A comparative material was obtained using the same sintering conditions as in Example 1.
[0034] Comparative Example 4 A NaNO3-KNO3 binary nitrate molten salt system with a molar ratio of 1:1 was used. The cation in this system is Na. + K + The anion is NO3. - The calculation yields: ΔS mix = 0.693R. The remaining processes are the same as in Example 1, and the comparative material is obtained.
[0035] Table 2 Performance data for examples and comparative examples As shown in Table 2, with the increase of the co-configurational entropy of the cations and anions in the molten salt system (ΔS)... mix As the concentration of ΔS increases, the degree of single crystallization and cycle stability of the material initially increase and then decrease. Traditional single-salt or low-entropy molten salt systems (ΔS) mix <1.5R) Due to the single type of ions, a uniform and stable liquid phase environment cannot be formed, resulting in a low single crystal ratio of the obtained material and significant voltage decay during cycling.
[0036] When ΔS mix When the R value is increased to the range of 2.5R to 3.5R, the synergistic effect of various cations and anions forms a high-entropy ionic environment, which can effectively improve the wettability of molten salt and the uniformity of ion transport, and promote the directional growth of grains. Therefore, the material exhibits a higher single crystal ratio (above 97%), lower voltage decay and better cycle stability.
[0037] When ΔS mix Beyond 3.5R, although the variety of ions increases, the excessively complex molten salt structure leads to enhanced competition between ions, reducing the effective lithium-ion migration efficiency and affecting grain growth. Consequently, the single crystal yield and cycle performance actually decrease. Therefore, high-entropy molten salts are not necessarily better the higher the entropy value, but rather there is an optimal entropy range, with 2.5R to 3.5R representing the best window for balancing ion disorder and crystal growth control.
[0038] The above description is merely a preferred embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention specification, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.
Claims
1. A method for preparing spherical single-crystal lithium-rich manganese-based cathode materials using a high-entropy molten salt system-assisted reaction, characterized in that, Includes the following steps: (1) Dissolve nickel salt and / or cobalt salt, and manganese salt in a solvent to obtain a mixed transition metal salt solution; (2) The transition metal mixed salt solution and the precipitant solution are added to the reactor simultaneously to form precursor particles through a co-precipitation reaction; (3) The obtained precursor is subjected to aging treatment so that the precursor nuclei continue to grow under the condition that no secondary nucleation occurs, forming spherical single crystal precursor particles. (4) The quasi-spherical single crystal precursor is mixed with a lithium source and a high-entropy molten salt system, wherein the high-entropy molten salt system is a multi-component eutectic system containing three or more components, formed by the combination of different cations and anions, and the high-entropy molten salt system must satisfy 2.5R≤ ≤3.5R, where, ΔS mix denoted as , where is the mixing entropy of cations and anions in the molten salt system, in J / mol / K; R is the gas constant, R = 8.314 J / mol / K; and n is the number of effective components participating in the mixing of the molten salt system. The mole fraction of anions in the i-th salt component; Let be the mole fraction of cations in the j-th salt component; ln is the natural logarithm. (5) Heating in an oxygen atmosphere or an air atmosphere to melt the high-entropy molten salt system and promoting the diffusion, rearrangement and crystal structure reconstruction of lithium ions and transition metal ions under liquid-phase assisted conditions; (6) After being cooled by high temperature treatment in step (5), the residual molten salt is removed by water washing to obtain a spherical single crystal lithium-rich manganese-based cathode material.
2. The method according to claim 1, characterized in that, Step (2) The co-precipitation reaction is carried out under the conditions of pH 10.5~11.5 and temperature 40~70℃.
3. The method according to claim 1, characterized in that, The aging process in step (3) takes 6 to 24 hours.
4. The method according to claim 1, characterized in that, The lithium source is selected from lithium carbonate, lithium hydroxide, or a combination thereof.
5. The method according to claim 1, characterized in that, In the high-entropy molten salt system, the cations are selected from Li + Na + K + Mg 2+ Ca 2+ Al 3+ Cs + One or more of the following; the anion is selected from Cl. - NO3 - CO3 2- SO4 2- PO4 3- F - One or more of them.
6. The method according to claim 1, characterized in that, The high-entropy molten salt system is any one of the following five-membered salt components: LiNO3-NaCl-K2CO3-MgSO4-CaCl2, LiNO3-NaNO3-KCl-Li2SO4-CaCO3, LiCl-NaCl-KNO3-MgCl2-CaSO4, LiF-NaNO3-KCl-MgSO4-CaCO3, and LiNO3-NaCl-K2CO3-MgSO4-Li3PO4.
7. The method according to claim 1, characterized in that, The high-entropy molten salt system is any one of the quaternary salt components among LiNO3-NaCl-K2CO3-CaSO4, LiNO3-NaCl-K2SO4-MgCO3, LiF-NaNO3-KCl-CaSO4, LiNO3-NaF-KCl-MgSO4, and LiCl-NaNO3-K2CO3-CaSO4.
8. The method according to claim 1, characterized in that, The melting temperature of the high-entropy molten salt system is below 650°C.
9. The method according to claim 1, characterized in that, The mass ratio of the high-entropy molten salt system to the spherical single crystal precursor is 0.05 to 3:
1.
10. The method according to claim 1, characterized in that, In step (5), the temperature is heated to 650~950°C in an oxygen atmosphere or an air atmosphere.