A method for preparing a bacterial grass cellulose regenerated fiber

By using alkaline treatment and bleaching processes on Juncao straw, combined with a low-temperature dissolution system of sodium hydroxide, urea, and zinc oxide, and modification with tannin-chitosan-silica-alumina complex microgels, the problem of insufficient cellulose purity in Juncao straw was solved, and the preparation of high-performance Juncao straw cellulose regenerated fibers was achieved, which are suitable for continuous and discontinuous fiber reinforced materials.

CN123133015APending Publication Date: 2026-11-20JIANGSU MINGXIN AGRICULTURAL DEVELOPMENT CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611422948.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-14
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In the existing technology, Juncao straw as a cellulose raw material has problems such as high impurity content, insufficient cellulose purity, obvious lignin coating, and uneven fiber structure, resulting in low fiber strength, poor dispersibility, and weak interfacial bonding, which makes it difficult to meet the application requirements of high-performance regenerated fibers and reinforced composite materials.

Method used

Juncao straw is treated with alkali and bleaching processes to form Juncao cellulose pulp. The pulp is then used to form a spinning solution through a low-temperature dissolution system of sodium hydroxide, urea and zinc oxide. Tannin chitosan silica-alumina complex microgel is added for modification. The spinning solution is extruded through a spinneret into a coagulation bath for coagulation and regeneration. Finally, the pulp is washed, dried and wound to form Juncao cellulose regenerated fiber.

Benefits of technology

The method improves the cellulose enrichment and swelling uniformity of Juncao cellulose pulp, enhances the stability and continuous formability of spinning solution, and the resulting Juncao cellulose regenerated fiber has good continuous formability, wet integrity and surface bonding ability, and is suitable for continuous and discontinuous fiber reinforced materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The application discloses the technical field of regenerated cellulose fiber preparation technology and discloses a preparation method of fungus grass cellulose regenerated fiber; fungus grass cellulose pulp is prepared through alkali treatment, hydrogen peroxide bleaching and drying of dried giant fungus grass straw; a low-temperature dissolving system is formed by sodium hydroxide, urea, zinc oxide and deionized water, and tannin chitosan silicon aluminum complex microgel dispersion liquid is added to prepare fungus grass cellulose modified spinning liquid; the modified spinning liquid is jetted, solidified, regenerated, washed, stretched, dried and wound to obtain fungus grass cellulose regenerated fiber. The raw material is easy to obtain, the process is simple, the cost is low, and the obtained fiber has good forming stability, mechanical properties and composite reinforcing applicability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of regenerated cellulose fiber preparation technology, specifically relating to a method for preparing Juncao cellulose regenerated fiber. Background Technology

[0002] Juncao (a type of grass) is a fast-growing, high-biomass, and highly adaptable herbaceous resource, characterized by its wide availability, low cost, and good renewability. Its straw contains abundant cellulose, hemicellulose, and lignin, making it an important raw material for preparing bio-based fiber materials. With the increasing demand for green, low-carbon materials and the high-value utilization of agricultural waste, converting Juncao straw into regenerated cellulose fibers can broaden the application of Juncao resources in textiles, composite reinforcement, biodegradable materials, and functional fibers. However, untreated Juncao straw suffers from high impurity content, insufficient cellulose purity, significant lignin coating, and uneven fiber structure. Direct use in fiber formation or composite reinforcement can easily lead to low fiber strength, poor dispersibility, weak interfacial bonding, and insufficient product stability, making it difficult to meet the application requirements of high-performance regenerated fibers and reinforced composite materials.

[0003] Existing regenerated cellulose fibers typically use wood pulp, cotton pulp, or bamboo pulp as the main raw materials, and obtain fiber products through dissolution, spinning, coagulation regeneration, and post-treatment. While traditional processes are relatively mature, some suffer from issues such as strong dependence on raw materials, high production costs, significant environmental impact, or stringent solvent recovery requirements. Juncao (a type of grass) serves as a low-cost, non-woody cellulose source. If suitable dissolution cellulose pulp can be obtained through alkali treatment and bleaching, and spinning can be performed using a low-temperature dissolution system composed of sodium hydroxide, urea, and zinc oxide, it can reduce raw material costs and process complexity while decreasing dependence on traditional wood pulp resources. However, relying solely on Juncao cellulose pulp to prepare regenerated fibers may still lead to problems such as insufficient spinning solution stability, loose internal fiber structure during coagulation, low wet strength, and increased brittleness after drying, affecting continuous fiber winding and subsequent processing performance.

[0004] Furthermore, when using regenerated Juncao cellulose fibers in continuous or discontinuous fiber-reinforced materials, it is necessary to consider the fiber's bulk strength, surface activity, interfacial bonding, and dispersion stability. Conventional inorganic fillers or single surface additives often fail to simultaneously improve fiber forming stability and composite interfacial properties; excessive addition may also cause spinning solution blockage, increased fiber defects, or higher costs. Therefore, it is necessary to develop a composite modifier that is readily available, has a mild reaction, and is suitable for low-cost scale-up preparation, enabling it to form a stable dispersion and multi-point interaction structure with the Juncao cellulose system, thereby improving the uniformity of the spinning solution, the density of the regenerated fibers, and the fiber surface bonding ability. Based on this, developing a method for preparing Juncao cellulose regenerated fibers containing tannin-chitosan-silica-alumina complex microgels is of great significance for improving the utilization value of Juncao resources and obtaining bio-based regenerated fibers suitable for continuous and discontinuous reinforced composite materials. Summary of the Invention

[0005] In view of the shortcomings of the prior art, the purpose of this invention is to provide a method for preparing regenerated cellulose fiber from Juncao grass.

[0006] In a first aspect, the present invention provides a method for preparing regenerated cellulose fibers from fungi and grasses, comprising the following steps:

[0007] S1. By weight, cut and crush 100-120 parts of dried giant reed straw into sections, add 800-1200 parts of deionized water and 40-80 parts of sodium hydroxide, stir at 85-95℃, filter, and wash with water to obtain alkali-treated giant reed straw fiber; add 600-1000 parts of deionized water, 20-50 parts of hydrogen peroxide aqueous solution and 0.5-1.5 parts of sodium metasilicate nonahydrate to the alkali-treated giant reed straw fiber, add sodium hydroxide to adjust the pH, bleach at 70-85℃, filter, wash with water, and dry to obtain giant reed straw cellulose pulp;

[0008] S2. Mix 100-120 parts of deionized water, 6.0-8.0 parts of sodium hydroxide, 10.0-14.0 parts of urea, and 0.2-0.6 parts of zinc oxide, and cool to obtain a mixture; pre-disperse 8-20 parts of the mixture with 0.3-1.2 parts of tannin-chitosan-silica-alumina complex microgel to obtain a dispersion; add 96-135 parts of the mixture to 4.0-7.0 parts of Juncao cellulose pulp, stir, and obtain a Juncao cellulose solution; add the dispersion to the Juncao cellulose solution, continue stirring, filter, and degas to obtain a Juncao cellulose modified spinning solution;

[0009] S3. The modified cellulose spinning solution of Juncao grass is extruded into a coagulation bath through a spinneret, and after coagulation regeneration, washing and stretching, Juncao grass cellulose regenerated fiber bundles are obtained.

[0010] S4. Wash the regenerated fiber bundles of Juncao cellulose with water, dry them, and wind them.

[0011] In this invention, during the preparation of regenerated cellulose fiber from giant reed grass, dried giant reed straw is cut into segments and crushed, then treated with deionized water and sodium hydroxide. Sodium hydroxide causes the hemicellulose, lignin, pectin, and wax components in the dried giant reed straw to swell, saponify, and partially dissolve, weakening the coating effect of non-cellulose components on cellulose. After filtration and washing, alkali-treated giant reed grass fiber with increased cellulose content and a loose structure is obtained. The alkali-treated giant reed grass fiber is then further contacted with deionized water, hydrogen peroxide aqueous solution, and sodium metasilicate nonahydrate, and the alkalinity is adjusted to the alkaline range by sodium hydroxide. Under alkaline conditions, hydrogen peroxide ionizes to generate hydrogen peroxide anions, which oxidize the carbonyl structure in the residual lignin and chromophores, causing the chromophores to lose conjugated absorption. Sodium metasilicate nonahydrate acts as a stabilizer and buffer for the hydrogen peroxide aqueous solution, adsorbing and passivating transition metal ions in the system through silicate micelles, reducing the ineffective decomposition of hydrogen peroxide. After bleaching, washing, and drying, giant reed grass cellulose pulp is obtained. A low-temperature dissolution system is formed by mixing deionized water, sodium hydroxide, urea, and zinc oxide and cooling the mixture. Zinc oxide dissolves in the sodium hydroxide aqueous solution to form zincate ions, which further form zinc-containing coordination structures with water molecules in the system. Sodium hydroxide gradually breaks down the hydrogen bond network between cellulose molecular chains. Urea molecules enter the vicinity of the cellulose molecular chains through inclusion bonding, forming new hydrogen bond barriers and inhibiting the re-aggregation of cellulose molecular chains. The zinc-containing coordination structures participate in the coordination environment around the cellulose hydroxyl groups, causing the cellulose pulp to gradually swell and dissolve under low-temperature conditions, yielding a cellulose solution. Tannin-chitosan-silica-alumina complex microgel is pre-dispersed with a portion of the mixture before being added to the cellulose solution. The phenolic hydroxyl, amino, and silanol structures and aluminum coordination nodes in the tannin-chitosan-silica-alumina complex microgel undergo hydrogen bonding association and coordination with the hydroxyl groups on the cellulose molecular chains, forming a modified cellulose spinning solution. After the modified cellulose spinning solution is extruded through a spinneret into a coagulation bath, sulfuric acid neutralizes the sodium hydroxide in the spinning stream, breaking the swollen state of the cellulose molecular chains and reforming the intermolecular hydrogen bond network. The cellulose transforms from a dissolved state to a regenerated solid state. Anhydrous sodium sulfate adjusts the ionic strength and osmotic pressure of the coagulation bath, promoting the diffusion of solvent, urea, zincate, and salts from the spinning stream into the coagulation bath. The coagulation and regeneration process proceeds relatively uniformly along the radial direction of the fiber stream. Water washing removes residual acids, alkalis, urea, and salts. Stretching orients the regenerated cellulose molecular chains along the fiber axis. Tannin-chitosan-silica-alumina complex microgels are uniformly dispersed inside and on the surface of the fiber. After drying, the fiber structure is fixed, and the fiber is wound to obtain regenerated cellulose fibers.

[0012] According to a preferred embodiment of the present invention, in step S1, the material is pulverized to 20-60 mesh, stirred at 85-95°C for 2-4 hours, and bleached at 70-85°C for 1.5-3.0 hours; the mass concentration of the hydrogen peroxide aqueous solution is 27.5-30%; and sodium hydroxide is added to adjust the pH to 10.0-11.0.

[0013] According to a preferred embodiment of the present invention, in step S2, the temperature is lowered to -8~-12℃.

[0014] According to a preferred embodiment of the present invention, in step S3, the coagulation bath comprises, by weight: 100 parts deionized water, 6-12 parts anhydrous sodium sulfate and 2-5 parts sulfuric acid with a mass concentration of 95-98%; the temperature of the coagulation bath is 20-35°C; the orifice diameter of the spinneret is 0.06-0.12 mm; the coagulation regeneration time is 20-80 s; and the draw ratio is 1.2-2.5 times.

[0015] According to a preferred embodiment of the present invention, in step S4, the drying temperature is 60-90°C.

[0016] According to a preferred embodiment of the present invention, the preparation steps of the tannin-chitosan silica-alumina complex microgel include:

[0017] A1. By weight, add 100-140 parts of deionized water, 1.0-2.5 parts of glacial acetic acid, and 4.0-8.0 parts of chitosan to a reactor and stir at 45-55℃ to obtain an acidic chitosan solution; add 3.0-7.0 parts of tannic acid to the acidic chitosan solution, continue stirring, and add 0.2-1.2 parts of sodium bicarbonate to adjust the pH to 4.6-5.2 to obtain a tannin-chitosan composite dispersion;

[0018] A2. Add 3.5-4.0 parts of sodium metasilicate nonahydrate to 25-45 parts of deionized water and stir to obtain a sodium metasilicate solution; add 12-14 parts of 10% hydrochloric acid solution dropwise to the sodium metasilicate solution, adjust the pH to 3.8-4.6, age, and obtain oligomeric silicate sol; add the oligomeric silicate sol to the tannin-chitosan composite dispersion and continue stirring to obtain the tannin-chitosan silicate composite dispersion;

[0019] A3. Add 1.0-3.0 parts of aluminum sulfate octadeca to 15-30 parts of deionized water, stir to dissolve, and obtain an aluminum sulfate solution; add the aluminum sulfate solution to the tannin-chitosan-silicic acid composite dispersion, add 0.2-1.5 parts of sodium bicarbonate to adjust the pH to 3.8-4.5, and react at 45-55℃ to obtain a tannin-chitosan-silica-aluminum complex solution;

[0020] A4. Add 40-80 parts of anhydrous ethanol to the tannin-chitosan-silica-alumina complex solution, stir, let stand, filter, and obtain a wet gel; wash the wet gel with ethanol aqueous solution and deionized water in sequence, vacuum dry, pulverize, and sieve.

[0021] In this invention, during the preparation of tannin-chitosan silica-alumina complex microgels, chitosan in an acidic medium formed by glacial acetic acid and deionized water undergoes protonation of its amino groups, resulting in a positive charge. This weakens the hydrogen bonding between molecular chains, gradually transforming the chitosan from an aggregated state to an aqueous dispersion, forming an acidic chitosan solution. Upon addition of tannic acid to the acidic chitosan solution, numerous hydrogen bonds form between the phenolic hydroxyl groups in the tannic acid molecules and the amino and hydroxyl groups on the chitosan molecular chains. Simultaneously, the partially dissociated phenolic anions of tannic acid electrostatically attract the positively charged protonated amino groups on the chitosan. Hydrophobic association occurs between the aromatic ring structure within the tannic acid molecule and the chitosan backbone, leading to the formation of fine, complex aggregate structures between the chitosan molecular chains. The addition of sodium bicarbonate gradually neutralizes excess glacial acetic acid and releases carbon dioxide, maintaining the system within a weakly acidic range. Chitosan remains in an acidic dispersion state, further strengthening the hydrogen bonding, electrostatic attraction, and hydrophobic association between tannic acid and chitosan, resulting in a tannin-chitosan composite dispersion. When sodium metasilicate nonahydrate is dissolved in deionized water, the silicon-oxygen bonds in its molecules partially hydrolyze, forming an alkaline silicate solution containing silicate ions. When a 10% hydrochloric acid solution is added dropwise to the sodium metasilicate solution, the silicate ions gradually protonate under acidic conditions, transforming into silanol species. During aging, a limited degree of dehydration condensation occurs between adjacent silanols, forming an oligomeric silicate sol linked by silicon and oxygen. When this oligomeric silicate sol is added to a tannin-chitosan composite dispersion, hydrogen bonds form between the silanol structures and the phenolic hydroxyl groups of tannin, the hydroxyl groups on the chitosan molecular chain, and the amino groups. Simultaneously, adjacent silanols continue to undergo dehydration condensation, introducing silicon-oxygen linkages into the gaps between the tannin and chitosan composite framework, resulting in a tannin-chitosan silicate composite dispersion. When aluminum sulfate octadeca is dissolved in deionized water, aluminum ions exist in the aluminum sulfate solution in a hydrated form. When the aluminum sulfate solution is added to a tannin-chitosan-silicic acid composite dispersion, aluminum ions form chelate rings with adjacent phenolic hydroxyl groups in tannic acid, and simultaneously coordinate with oxygen atoms in the amino and silanol structures of the chitosan molecular chain. Sodium bicarbonate is used to gradually adjust the acidity of the system, mitigating the tendency for direct hydrolysis of aluminum ions to form coarse aluminum hydroxide precipitates, ensuring a more uniform distribution of aluminum coordination nodes between the tannin-chitosan composite structure and the silicon-oxygen linkage structure, forming a tannin-chitosan-silica-aluminum complex. The addition of anhydrous ethanol decreases the solvent polarity, disturbing the solvated aqueous layer of the complex structure, causing dehydration and shrinkage, and precipitating a wet gel. After washing with ethanol-water solution and deionized water to remove residual sodium ions, chloride ions, sulfate ions, acetate ions, and unbound small molecules, the gel is vacuum dried, pulverized, and sieved to obtain the tannin-chitosan-silica-aluminum complex microgel.

[0022] According to a preferred embodiment of the present invention, in step A1, the stirring time at 45-55°C is 2-4 hours.

[0023] According to a preferred embodiment of the present invention, in step A2, the aging time is 30-90 minutes.

[0024] According to a preferred embodiment of the present invention, in step A3, the reaction time at 45-55°C is 2-5 hours.

[0025] According to a preferred embodiment of the present invention, in step A4, the standing time is 1-3 hours, the vacuum drying time is 6-12 hours, and the sieve mesh size is 200-500 mesh.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) This invention uses dried giant Napier grass straw as the cellulose source. The dried giant Napier grass straw is treated with deionized water and sodium hydroxide to dissolve or weaken non-cellulose components such as hemicellulose, lignin, pectin, and waxes, resulting in alkali-treated Napier grass fiber. This fiber is then bleached with deionized water, hydrogen peroxide solution, sodium metasilicate nonahydrate, and sodium hydroxide to reduce the impact of residual lignin and color-developing components on subsequent dissolution, filtration, and spinning, yielding Napier grass cellulose pulp. This treatment process improves the cellulose enrichment and swelling uniformity of the Napier grass cellulose pulp, which is beneficial for the subsequent formation of a stable Napier grass cellulose solution.

[0028] (2) In this invention, a mixture of deionized water, sodium hydroxide, urea, and zinc oxide is formed. The tannin-chitosan-silica-alumina complex microgel is pre-dispersed with a portion of the mixture to obtain a dispersion. The dispersion is then added to a Juncao cellulose solution to obtain a Juncao cellulose modified spinning solution. This addition method makes the tannin-chitosan-silica-alumina complex microgel more evenly distributed in the Juncao cellulose solution, reducing local agglomeration that occurs when added directly. The tannin-chitosan-silica-alumina complex microgel is made from chitosan, tannic acid, sodium metasilicate nonahydrate, hydrochloric acid solution, aluminum sulfate octadecahydrate, sodium bicarbonate, and anhydrous ethanol. Its structure contains phenolic hydroxyl groups, amino groups, silanol structures, and aluminum coordination nodes, which can form hydrogen bonds and coordinate bonds with the cellulose molecular chains in the Juncao cellulose pulp, improving the uniformity, filterability, and continuous forming stability of the Juncao cellulose modified spinning solution.

[0029] (3) In this invention, the modified cellulose spinning solution is extruded through a spinneret into a coagulation bath. The coagulation bath consists of deionized water, anhydrous sodium sulfate, and sulfuric acid. The sulfuric acid promotes the transformation of cellulose from a dissolved state to a regenerated solid state, while the anhydrous sodium sulfate regulates the ionic strength and permeation environment of the coagulation bath, ensuring a stable coagulation and regeneration process. After coagulation and regeneration, washing, and stretching, regenerated cellulose fiber bundles are obtained; after further washing, drying, and winding, regenerated cellulose fibers are obtained. The obtained regenerated cellulose fibers have good continuous formability, wet integrity, structural stability after drying, and surface bonding ability, and can be used in continuous fiber reinforced materials and discontinuous fiber reinforced materials. Detailed Implementation

[0030] To facilitate understanding of the present invention, the following embodiments are provided. Those skilled in the art should understand that these embodiments are merely illustrative and should not be construed as limiting the scope of the invention.

[0031] Example 1

[0032] This embodiment provides a method for preparing regenerated cellulose fiber from Juncao grass, including the following steps:

[0033] S1. Cut 110.0g of dried giant reed straw into 20mm segments, pulverize to 40 mesh, add 1000.0g of deionized water and 60.0g of sodium hydroxide, stir at 400r / min for 3h at 90°C, filter with 200-mesh filter cloth, wash the filter residue with deionized water until the pH of the washing liquid is 8.5 to obtain alkali-treated giant reed straw fiber; add 800.0g of deionized water, 35.0g of 28.8% hydrogen peroxide aqueous solution and 1.0g of sodium metasilicate nonahydrate to the alkali-treated giant reed straw fiber, add 4.0g of sodium hydroxide to adjust the pH to 10.5, bleach at 400r / min for 2.25h at 78°C, filter with 200-mesh filter cloth, wash the filter residue with deionized water until the pH of the washing liquid is 7.0, dry at 60°C until the moisture content is 10.0% to obtain giant reed straw cellulose pulp;

[0034] S2. Mix 110.0 g deionized water, 7.0 g sodium hydroxide, 12.0 g urea, and 0.4 g zinc oxide, stir at 400 r / min for 20 min at 25°C, and cool to -10°C to obtain 129.4 g of mixture; pre-disperse 14.0 g of the mixture with 0.75 g tannin-chitosan-silica-alumina complex microgel at -10°C for 15 min at 500 r / min to obtain dispersion; add 5.5 g of the mixture to the mixture. In the cellulose pulp of Juncao grass, the mixture was stirred at 800 r / min for 15 min at -10°C, then allowed to stand at -10°C for 30 min, and then stirred at 500 r / min for 60 min to obtain a Juncao grass cellulose solution. A dispersion was added to the Juncao grass cellulose solution, and the mixture was stirred at 500 r / min at -10°C for 40 min. The solution was then filtered through a 300-mesh filter and degassed at -0.08 MPa for 30 min to obtain a Juncao grass cellulose modified spinning solution.

[0035] S3. The modified cellulose spinning solution was extruded into a coagulation bath through a spinneret with an aperture of 0.09 mm. The coagulation bath was prepared by mixing 100.0 g of deionized water, 9.0 g of anhydrous sodium sulfate and 3.5 g of sulfuric acid with a mass concentration of 96.5%. When preparing the coagulation bath, anhydrous sodium sulfate was first dissolved in deionized water, then sulfuric acid was added and stirred evenly. The temperature of the coagulation bath was 27.5°C and the coagulation regeneration time was 50 s. After washing with deionized water until the pH of the washing solution was 6.8, the fibers were stretched with a stretch ratio of 1.85 to obtain regenerated cellulose fiber bundles.

[0036] S4. Wash the regenerated cellulose fiber bundles of Juncao grass with deionized water until the pH of the washing solution is 7.0, dry them at 75°C for 2 hours, control the moisture content to be 9.0%, and wind them at 10m / min to obtain Juncao grass regenerated fibers.

[0037] Preparation steps of tannin-chitosan silica-alumina complex microgel:

[0038] A1. Add 120.0g deionized water, 1.75g ​​glacial acetic acid and 6.0g chitosan to a reactor, stir at 300r / min and heat to 50°C, stir at 50°C for 3h to obtain an acidic chitosan solution; add 5.0g tannic acid to the acidic chitosan solution, maintain 50°C and continue stirring at 300r / min for 2h, then add 0.7g sodium bicarbonate in portions over 20min to adjust the pH to 4.9, and continue stirring at 300r / min for 30min to obtain a tannin-chitosan composite dispersion;

[0039] A2. Add 3.75g of sodium metasilicate nonahydrate to 35.0g of deionized water and stir at 300r / min for 20min at 25°C to obtain a sodium metasilicate solution. Add 13.0g of 10% hydrochloric acid solution dropwise to the sodium metasilicate solution over 30min, maintaining stirring at 300r / min and controlling the system temperature at 25°C during the dropwise addition. Adjust the pH to 4.2 and age for 60min to obtain an oligomeric silicate sol. Add the oligomeric silicate sol to the tannin-chitosan composite dispersion and continue stirring at 300r / min for 2h at 50°C to obtain the tannin-chitosan silicate composite dispersion.

[0040] A3. Add 2.0g of aluminum sulfate octadeca to 22.5g of deionized water and stir at 300r / min for 15min at 25°C to obtain an aluminum sulfate solution. Add the aluminum sulfate solution to the tannin-chitosan-silicic acid composite dispersion within 20min, while maintaining stirring at 300r / min during the addition process. Then, add 0.85g of sodium bicarbonate in portions over 15min to adjust the pH to 4.1. React at 300r / min for 3.5h at 50°C to obtain a tannin-chitosan-silica-aluminum complex solution.

[0041] A4. Add 60.0 g of anhydrous ethanol to the tannin-chitosan silica-alumina complex solution, stir at 300 r / min for 30 min at 25°C, let stand for 2 h, filter with 200 mesh filter cloth to obtain wet gel; wash the wet gel successively with 20.0 g of ethanol aqueous solution and 20.0 g of deionized water until the pH of the washing solution is 6.5, vacuum dry at 50°C and -0.08 MPa for 9 h, pulverize, and pass through a 350 mesh sieve to obtain tannin-chitosan silica-alumina complex microgel.

[0042] Example 2

[0043] The difference between this embodiment and Embodiment 1 is that this embodiment provides a method for preparing regenerated cellulose fiber from Juncao grass, including the following steps:

[0044] S1. Cut 100.0g of dried giant reed straw into 20mm segments, pulverize to 20 mesh, add 800.0g of deionized water and 40.0g of sodium hydroxide, stir at 400r / min for 2h at 85°C, filter with a 200-mesh filter cloth, wash the filter residue with deionized water until the pH of the washing liquid is 8.5, and obtain alkali-treated giant reed straw fiber; add 600.0g of deionized water, 20.0g of 27.5% hydrogen peroxide aqueous solution and 0.5g of sodium metasilicate nonahydrate to the alkali-treated giant reed straw fiber, add 2.0g of sodium hydroxide to adjust the pH to 10.0, bleach at 400r / min for 1.5h at 70°C, filter with a 200-mesh filter cloth, wash the filter residue with deionized water until the pH of the washing liquid is 7.0, dry at 60°C until the moisture content is 10.0%, and obtain giant reed straw cellulose pulp;

[0045] S2. Mix 100.0g deionized water, 6.0g sodium hydroxide, 10.0g urea, and 0.2g zinc oxide, stir at 400r / min for 20min at 25°C, and cool to -8°C to obtain 116.2g of mixture; pre-disperse 8.0g of mixture with 0.3g tannin-chitosan-silica-alumina complex microgel at -8°C for 15min at 500r / min to obtain dispersion; add 4.0g of bacteria to 96.0g of mixture. In grass cellulose pulp, the mixture is stirred at 800 rpm for 15 min at -8°C, then allowed to stand at -8°C for 30 min, followed by stirring at 500 rpm for 60 min to obtain a grass cellulose solution. A dispersion is added to the grass cellulose solution, and the mixture is stirred at 500 rpm for 40 min at -8°C. The solution is then filtered through a 300-mesh filter and degassed at -0.08 MPa for 30 min to obtain a grass cellulose modified spinning solution.

[0046] S3. The modified cellulose spinning solution was extruded into a coagulation bath through a spinneret with an aperture of 0.06 mm. The coagulation bath was prepared by mixing 100.0 g of deionized water, 6.0 g of anhydrous sodium sulfate and 2.0 g of 95% sulfuric acid. When preparing the coagulation bath, anhydrous sodium sulfate was first dissolved in deionized water, then sulfuric acid was added and stirred evenly. The temperature of the coagulation bath was 20°C and the coagulation regeneration time was 20 s. After washing with deionized water until the pH of the washing solution was 6.8, the fibers were stretched with a stretching ratio of 1.2 to obtain regenerated cellulose fiber bundles.

[0047] S4. Wash the regenerated cellulose fiber bundles of Juncao grass with deionized water until the pH of the washing solution is 7.0, dry them at 60°C for 2 hours, control the moisture content to be 9.0%, and wind them at 10m / min to obtain Juncao grass regenerated fibers.

[0048] Preparation steps of tannin-chitosan silica-alumina complex microgel:

[0049] A1. Add 100.0g deionized water, 1.0g glacial acetic acid and 4.0g chitosan to a reactor, stir at 300r / min and heat to 45°C, stir at 45°C for 2h to obtain an acidic chitosan solution; add 3.0g tannic acid to the acidic chitosan solution, maintain 45°C and continue stirring at 300r / min for 2h, then add 0.2g sodium bicarbonate in portions over 20min to adjust the pH to 4.6, and continue stirring at 300r / min for 30min to obtain a tannin-chitosan composite dispersion;

[0050] A2. Add 3.5g of sodium metasilicate nonahydrate to 25.0g of deionized water and stir at 300r / min for 20min at 25°C to obtain a sodium metasilicate solution. Add 12.0g of 10% hydrochloric acid solution dropwise to the sodium metasilicate solution over 30min, maintaining stirring at 300r / min and controlling the system temperature at 25°C during the dropwise addition. Adjust the pH to 3.8 and age for 30min to obtain an oligomeric silicate sol. Add the oligomeric silicate sol to the tannin-chitosan composite dispersion and continue stirring at 300r / min for 2h at 45°C to obtain the tannin-chitosan silicate composite dispersion.

[0051] A3. Add 1.0g of aluminum sulfate octadeca to 15.0g of deionized water and stir at 300r / min for 15min at 25°C to obtain an aluminum sulfate solution. Add the aluminum sulfate solution to the tannin-chitosan-silicic acid composite dispersion within 20min, while maintaining stirring at 300r / min during the addition process. Then, add 0.2g of sodium bicarbonate in portions over 15min to adjust the pH to 3.8. React at 300r / min at 45°C for 2h to obtain a tannin-chitosan-silica-aluminum complex solution.

[0052] A4. Add 40.0 g of anhydrous ethanol to the tannin-chitosan silica-alumina complex solution, stir at 300 r / min for 30 min at 25°C, let stand for 1 h, filter with a 200 mesh filter cloth to obtain a wet gel; wash the wet gel successively with 18.0 g of ethanol aqueous solution and 18.0 g of deionized water until the pH of the washing solution is 6.5, vacuum dry at 50°C and -0.08 MPa for 6 h, pulverize, and pass through a 200 mesh sieve to obtain tannin-chitosan silica-alumina complex microgel.

[0053] Example 3

[0054] The difference between this embodiment and Embodiment 1 is that this embodiment provides a method for preparing regenerated cellulose fiber from Juncao grass, including the following steps:

[0055] S1. Cut 120.0g of dried giant reed straw into 20mm segments, pulverize to 60 mesh, add 1200.0g of deionized water and 80.0g of sodium hydroxide, stir at 400r / min for 4h at 95°C, filter with 200-mesh filter cloth, wash the filter residue with deionized water until the pH of the washing liquid is 8.5 to obtain alkali-treated giant reed straw fiber; add 1000.0g of deionized water, 50.0g of 30% hydrogen peroxide aqueous solution and 1.5g of sodium metasilicate nonahydrate to the alkali-treated giant reed straw fiber, add 6.0g of sodium hydroxide to adjust the pH to 11.0, bleach at 400r / min for 3h at 85°C, filter with 200-mesh filter cloth, wash the filter residue with deionized water until the pH of the washing liquid is 7.0, dry at 60°C until the moisture content is 10.0% to obtain giant reed straw cellulose pulp;

[0056] S2. Mix 120.0 g deionized water, 8.0 g sodium hydroxide, 14.0 g urea, and 0.6 g zinc oxide, stir at 400 rpm for 20 min at 25°C, and cool to -12°C to obtain 142.6 g of mixture; pre-disperse 20.0 g of the mixture with 1.2 g tannin-chitosan-silica-alumina complex microgel at -12°C for 15 min at 500 rpm to obtain a dispersion; add 7.0 g of the 122.6 g mixture to... In the cellulose pulp of Juncao grass, the mixture was stirred at 800 r / min for 15 min at -12°C, then allowed to stand at -12°C for 30 min, and then stirred at 500 r / min for 60 min to obtain a Juncao grass cellulose solution. A dispersion was added to the Juncao grass cellulose solution, and the mixture was stirred at 500 r / min at -12°C for 40 min. The solution was then filtered through a 300-mesh filter and degassed at -0.08 MPa for 30 min to obtain a Juncao grass cellulose modified spinning solution.

[0057] S3. The modified cellulose spinning solution was extruded into a coagulation bath through a spinneret with an aperture of 0.12 mm. The coagulation bath was prepared by mixing 100.0 g of deionized water, 12.0 g of anhydrous sodium sulfate and 5.0 g of 98% sulfuric acid. When preparing the coagulation bath, anhydrous sodium sulfate was first dissolved in deionized water, then sulfuric acid was added and stirred evenly. The temperature of the coagulation bath was 35°C and the coagulation regeneration time was 80 s. After washing with deionized water until the pH of the washing solution was 6.8, the fibers were stretched with a stretching ratio of 2.5 to obtain regenerated cellulose fiber bundles.

[0058] S4. Wash the regenerated cellulose fiber bundles of Juncao grass with deionized water until the pH of the washing solution is 7.0, dry them at 90°C for 2 hours, control the moisture content to be 9.0%, and wind them at 10m / min to obtain Juncao grass regenerated fibers.

[0059] Preparation steps of tannin-chitosan silica-alumina complex microgel:

[0060] A1. Add 140.0g deionized water, 2.5g glacial acetic acid and 8.0g chitosan to the reactor, stir at 300r / min and heat to 55°C, stir at 55°C for 4h to obtain an acidic chitosan solution; add 7.0g tannic acid to the acidic chitosan solution, maintain 55°C and continue stirring at 300r / min for 2h, then add 1.2g sodium bicarbonate in portions over 20min to adjust the pH to 5.2, and continue stirring at 300r / min for 30min to obtain a tannin-chitosan composite dispersion;

[0061] A2. Add 4.0g of sodium metasilicate nonahydrate to 45.0g of deionized water and stir at 300r / min for 20min at 25°C to obtain a sodium metasilicate solution. Add 14.0g of 10% hydrochloric acid solution dropwise to the sodium metasilicate solution over 30min, maintaining stirring at 300r / min and controlling the system temperature at 25°C during the dropwise addition. Adjust the pH to 4.6 and age for 90min to obtain an oligomeric silicate sol. Add the oligomeric silicate sol to the tannin-chitosan composite dispersion and continue stirring at 300r / min for 2h at 55°C to obtain the tannin-chitosan silicate composite dispersion.

[0062] A3. Add 3.0g of aluminum sulfate octadeca to 30.0g of deionized water and stir at 300r / min for 15min at 25°C to obtain an aluminum sulfate solution. Add the aluminum sulfate solution to the tannin-chitosan-silicic acid composite dispersion within 20min, while maintaining stirring at 300r / min during the addition process. Then, add 1.5g of sodium bicarbonate in portions over 15min to adjust the pH to 4.5. React at 300r / min for 5h at 55°C to obtain a tannin-chitosan-silica-aluminum complex solution.

[0063] A4. Add 80.0 g of anhydrous ethanol to the tannin-chitosan silica-alumina complex solution, stir at 300 r / min for 30 min at 25°C, let stand for 3 h, filter with 200 mesh filter cloth to obtain wet gel; wash the wet gel successively with 22.0 g of ethanol aqueous solution and 22.0 g of deionized water until the pH of the washing solution is 6.5, vacuum dry at 50°C and -0.08 MPa for 12 h, pulverize, and pass through a 500 mesh sieve to obtain tannin-chitosan silica-alumina complex microgel.

[0064] Comparative Example 1

[0065] The difference between this comparative example and Example 1 is that tannin-chitosan silica-alumina complex microgel is not added in step S2, while the rest is the same as in Example 1.

[0066] Comparative Example 2

[0067] The difference between this comparative example and Example 1 is that step A1 is omitted in the preparation of the tannin-chitosan silica-alumina complex microgel; otherwise, the process is the same as in Example 1.

[0068] Comparative Example 3

[0069] The difference between this comparative example and Example 1 is that steps A2 and A3 are not performed in the preparation process of the tannin-chitosan silica-alumina complex microgel; the rest is the same as in Example 1.

[0070] A series of standardized tests were conducted on the regenerated cellulose fibers prepared by the methods described in Examples 1-3 and Comparative Examples 1-3.

[0071] The regenerated cellulose fibers prepared by Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were used as test samples. Before testing, each group of samples was placed in a standard environment with a temperature of 20°C and a relative humidity of 65% for 24 hours to acclimate. After acclimation, fuzz, broken fibers, oil stains, joints and obviously mechanically damaged sections were removed.

[0072] During the evenness test, three roll samples were taken for each group. The length of continuous fiber cut from each roll was not less than 100m. The samples were tested on a capacitive evenness tester. Before the test, the fiber was passed through the test area with constant tension. The mass fluctuation of the fiber along the length direction was recorded, and the coefficient of variation of mass unevenness was calculated. The result was the average value of the three roll samples, and the unit was .

[0073] For dry breaking strength and dry breaking elongation tests, 20 valid samples were randomly selected from each group. First, the linear density of the samples in the same group was determined according to the filament linear density test method as the basis for strength conversion. Then, a single filament tensile test was carried out in an environment with a temperature of 20°C and a relative humidity of 65%. The clamping distance was 250 mm, the tensile speed was 250 mm / min, and the pre-tension was set according to the sample linear density to straighten the sample without pre-elongation. The breaking strength and breaking elongation were recorded. Invalid data such as clamp breakage, clamp slippage, and abnormal fracture points were discarded. The dry breaking strength was converted from the breaking strength to the linear density, and the unit was cN / dtex. The dry breaking elongation was calculated as a percentage of the breaking elongation to the initial clamping distance, and the unit was cN / dtex.

[0074] For wet fracture strength and wet fracture elongation tests, 20 valid specimens were randomly selected from each group. The specimens were completely immersed in 20°C deionized water for 30 minutes. After removal, the surface free water was removed by gently touching with absorbent paper, and the tensile test was performed immediately in the wet state. The clamping distance was 250 mm, and the tensile speed was 250 mm / min. The wet fracture strength and wet fracture elongation were recorded. The wet fracture strength was converted according to the linear density of the same group, and the unit was cN / dtex. The wet fracture elongation was calculated as a percentage of the wet fracture elongation to the initial clamping distance, and the unit was cN / dtex.

[0075] During the moisture regain test, approximately 5g of conditioned fiber sample was taken from each group. After weighing the equilibrium mass, the sample was placed in an oven and dried until the difference between two adjacent weighings was no greater than 0.05%. After being removed, the sample was placed in a desiccator to cool to room temperature and the dried mass was weighed. The moisture regain was calculated as a percentage of the difference between the equilibrium mass and the dried mass to the dried mass, in units of 0.5g.

[0076] Each test yielded at least 5 valid data points, and the results in the table are the average of the valid data points.

[0077] The performance test data above are shown in Table 1.

[0078] Table 1: Performance Test Results

[0079]

[0080] As can be seen from the above, the unevenness rate of yarn in Examples 1-3 was 2.6-3.1%, which was significantly lower than that of Comparative Examples 1-3 (4.9-6.8%). This indicates that the uniformity of dispersion and the stability of spinning of modified Juncao cellulose were improved after using tannin-chitosan-silica-alumina complex microgel. This can reduce the quality fluctuation of fibers along the length direction and solve the problem of insufficient yarn uniformity of existing Juncao cellulose regenerated fibers due to pulp impurities, uneven dissolution, and poor dispersion of modified components.

[0081] The dry breaking strength of Examples 1-3 was 2.78-3.05 cN / dtex, and the wet breaking strength was 1.68-1.92 cN / dtex, both higher than the dry breaking strength of Comparative Examples 1-3 (2.15-2.46 cN / dtex and 1.05-1.34 cN / dtex). This indicates that the tannin-chitosan composite structure and the silica-alumina complex structure in the tannin-chitosan silica-alumina complex microgel can jointly improve the bonding strength between regenerated cellulose segments and the wet structural integrity, thus solving the problems of insufficient dry strength, significant wet strength decay, and easy breakage during subsequent processing of existing Juncao cellulose regenerated fibers.

[0082] The dry breaking elongation of Examples 1-3 was 13.6-15.2%, and the wet breaking elongation was 18.4-20.1%, which was lower than the dry breaking elongation of 16.8-18.9% and the wet breaking elongation of 22.4-25.8% of Comparative Examples 1-3. This indicates that the fibers in the Examples have higher structural constraints and orientation stability under stress, and no longer rely mainly on loose structural deformation to prolong the breaking process, but exhibit more stable load-bearing capacity.

[0083] The moisture regain of Examples 1-3 was 10.8-11.5%, lower than that of Comparative Examples 1-3 (12.6-13.9%), indicating that the composite network formed by the tannin-chitosan-silica-alumina complex microgel reduced the exposure of free hydrophilic sites inside the fiber, thus improving the structural stability and moisture-resistant dimensional stability after drying. Comparative Example 1, which did not include the tannin-chitosan-silica-alumina complex microgel, had the highest yarn unevenness and the lowest dry-wet breaking strength, indicating that a simple cellulose system is difficult to balance spinning uniformity and fiber strength. Comparative Example 2 lacked the tannin-chitosan composite component, and Comparative Example 3... The absence of the silica-alumina complex resulted in lower performance for both components compared to Examples 1-3. This indicates that the tannin-chitosan composite structure primarily improves the interfacial association and dispersion stability of cellulose, while the silica-alumina complex structure mainly enhances the internal network and wet stability of the fiber. The synergistic effect of these two components enabled Examples 1-3 to simultaneously achieve lower yarn unevenness, higher dry and wet breaking strength, and lower moisture regain. This solves the problems of poor uniformity in the forming of regenerated cellulose fibers, low strength, insufficient wet stability, and insufficient interfacial bonding ability when used as continuous or discontinuous fiber reinforcement materials in the prior art.

Claims

1. A method for preparing regenerated cellulose fiber from Juncao grass, characterized in that, Includes the following steps: S1. By weight, cut and crush 100-120 parts of dried giant reed straw into sections, add 800-1200 parts of deionized water and 40-80 parts of sodium hydroxide, stir at 85-95℃, filter, and wash with water to obtain alkali-treated giant reed straw fiber; add 600-1000 parts of deionized water, 20-50 parts of hydrogen peroxide aqueous solution and 0.5-1.5 parts of sodium metasilicate nonahydrate to the alkali-treated giant reed straw fiber, add sodium hydroxide to adjust the pH, bleach at 70-85℃, filter, wash with water, and dry to obtain giant reed straw cellulose pulp; S2. Mix 100-120 parts of deionized water, 6.0-8.0 parts of sodium hydroxide, 10.0-14.0 parts of urea, and 0.2-0.6 parts of zinc oxide, and cool to obtain a mixture; pre-disperse 8-20 parts of the mixture with 0.3-1.2 parts of tannin-chitosan-silica-alumina complex microgel to obtain a dispersion; add 96-135 parts of the mixture to 4.0-7.0 parts of Juncao cellulose pulp, stir, and obtain a Juncao cellulose solution; add the dispersion to the Juncao cellulose solution, continue stirring, filter, and degas to obtain a Juncao cellulose modified spinning solution; S3. The modified cellulose spinning solution of Juncao grass is extruded into a coagulation bath through a spinneret, and after coagulation regeneration, washing and stretching, Juncao grass cellulose regenerated fiber bundles are obtained. S4. Wash the regenerated fiber bundles of Juncao cellulose with water, dry them, and wind them.

2. The method for preparing regenerated cellulose fiber from Juncao (a type of fungus) according to claim 1, characterized in that, In step S1, the material is pulverized to 20-60 mesh, stirred at 85-95℃ for 2-4 hours, and bleached at 70-85℃ for 1.5-3.0 hours; the mass concentration of the hydrogen peroxide aqueous solution is 27.5-30%; and sodium hydroxide is added to adjust the pH to 10.0-11.

0.

3. The method for preparing regenerated cellulose fiber from Juncao (a type of fungus) according to claim 1, characterized in that, In step S2, the temperature is lowered to -8~-12℃.

4. The method for preparing regenerated cellulose fiber according to claim 1, characterized in that, In step S3, the coagulation bath comprises, by weight: 100 parts deionized water, 6-12 parts anhydrous sodium sulfate, and 2-5 parts sulfuric acid with a mass concentration of 95-98%; the temperature of the coagulation bath is 20-35℃; the orifice diameter of the spinneret is 0.06-0.12mm; the coagulation regeneration time is 20-80s; and the draw ratio is 1.2-2.5 times.

5. The method for preparing regenerated cellulose fiber according to claim 1, characterized in that, In step S4, the drying temperature is 60-90℃.

6. The method for preparing regenerated cellulose fiber according to any one of claims 1-5, characterized in that, The preparation steps of the tannin-chitosan-aluminosilicate complex microgel include: A1. By weight, add 100-140 parts of deionized water, 1.0-2.5 parts of glacial acetic acid, and 4.0-8.0 parts of chitosan to a reactor and stir at 45-55℃ to obtain an acidic chitosan solution; add 3.0-7.0 parts of tannic acid to the acidic chitosan solution, continue stirring, and add 0.2-1.2 parts of sodium bicarbonate to adjust the pH to 4.6-5.2 to obtain a tannin-chitosan composite dispersion; A2. Add 3.5-4.0 parts of sodium metasilicate nonahydrate to 25-45 parts of deionized water and stir to obtain a sodium metasilicate solution; add 12-14 parts of 10% hydrochloric acid solution dropwise to the sodium metasilicate solution, adjust the pH to 3.8-4.6, age, and obtain oligomeric silicate sol; add the oligomeric silicate sol to the tannin-chitosan composite dispersion and continue stirring to obtain the tannin-chitosan silicate composite dispersion; A3. Add 1.0-3.0 parts of aluminum sulfate octadeca to 15-30 parts of deionized water, stir to dissolve, and obtain an aluminum sulfate solution; add the aluminum sulfate solution to the tannin-chitosan-silicic acid composite dispersion, add 0.2-1.5 parts of sodium bicarbonate to adjust the pH to 3.8-4.5, and react at 45-55℃ to obtain a tannin-chitosan-silica-aluminum complex solution; A4. Add 40-80 parts of anhydrous ethanol to the tannin-chitosan-silica-alumina complex solution, stir, let stand, filter, and obtain a wet gel; wash the wet gel with ethanol aqueous solution and deionized water in sequence, vacuum dry, pulverize, and sieve.

7. The method for preparing regenerated cellulose fiber according to claim 6, characterized in that, In step A1, the stirring time at 45-55℃ is 2-4 hours.

8. The method for preparing regenerated cellulose fiber according to claim 6, characterized in that, In step A2, the aging time is 30-90 minutes.

9. The method for preparing regenerated cellulose fiber according to claim 6, characterized in that, In step A3, the reaction time is 2-5 hours at 45-55℃.

10. The method for preparing regenerated cellulose fiber according to claim 6, characterized in that, In step A4, the standing time is 1-3 hours, the vacuum drying time is 6-12 hours, and the sieve mesh size is 200-500 mesh.