Method for the production of hemp-based lyocell fibers and fibers
By treating hemp pulp with heteropoly acids in a one-step process and blending it with high-polymerization-degree wood pulp, the problems of metal ion removal and polymerization degree control in the preparation of Lyocell fiber from hemp pulp were solved. This resulted in the production of high-strength, high-toughness, and long-lasting antibacterial hemp Lyocell fiber, which simplified the process and reduced costs.
Patent Information
- Application Number
- CN202611455073.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-18
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies are difficult to effectively utilize hemp pulp to prepare high-strength, high-toughness, and long-lasting antibacterial Lyocell fibers, due to problems such as difficulty in removing metal ion impurities, difficulty in controlling the degree of polymerization, and easy loss of natural antibacterial components.
Hemp pulp is treated with a one-step heteropoly acid process to remove metal ions and precisely control the degree of polymerization. Combined with high-polymerization wood pulp blending, spinning solution is prepared through dry-jet wet spinning process to retain the natural antibacterial properties of the fiber.
This study achieved the preparation of high-strength, high-toughness, and long-lasting antibacterial Lyocell fibers, simplifying the process, reducing production costs, and maintaining the fiber's high-efficiency antibacterial properties.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of fiber preparation technology. Specifically, it relates to a method for preparing hemp-based Lyocell fiber and the fiber itself, and more particularly to a method for preparing a high-strength, high-toughness, long-lasting, strong antibacterial hemp Lyocell fiber. Background Technology
[0002] Lyocell fiber is currently the most promising new type of regenerated cellulose fiber in the textile industry. With its excellent environmental properties and performance, it is hailed as the green fiber of the 21st century. This fiber is produced using a dry-jet wet spinning process, employing the low-toxicity and environmentally friendly N-methylmorpholine-N-oxide (NMMO) as a dedicated solvent. The entire production process is green and low-carbon, completely avoiding the pollution problems caused by the emission of harmful substances such as CS2 during the production of traditional viscose fibers. Throughout its production and use cycle, Lyocell fiber's environmental advantages are particularly prominent. Waste products can be directly and naturally degraded, preventing environmental pollution accumulation. The NMMO solvent has a recycling rate of up to 99.5%, allowing for repeated use, making it a recognized environmentally friendly production process.
[0003] Currently, commercially produced Lyocell fibers worldwide primarily use virgin wood dissolving pulp as their core raw material, with the degree of polymerization of the pulp produced being consistently between 500 and 700. Virgin wood has uniform texture and highly controllable quality, and with standardized pulping processes, it can precisely produce high-quality wood dissolving pulp suitable for Lyocell spinning. However, wood has a long growth cycle, takes a long time to mature, and has limited natural resources. Furthermore, to protect the environment, most of the wood chips needed for pulping in China's Lyocell fiber production rely on imports, which not only increases production costs but also hinders the industry's large-scale development.
[0004] To overcome the resource bottleneck of wood pulp raw materials, hemp pulp is gradually becoming a new and ideal raw material for Lyocell fiber. Hemp pulp uses natural bast fibers such as ramie, flax, jute, and hemp as its base material, and is purified into high-purity cellulose materials through an environmentally friendly refining pulping process. The cellulose molecules in hemp pulp have a moderate degree of polymerization and a regular molecular structure. The fibers prepared from this pulp possess excellent physical and chemical properties such as high strength and high wet modulus, while also inheriting the functional advantages of natural hemp fibers, including moisture absorption, breathability, and antibacterial properties. Research shows that hemp fibers have a large specific surface area, numerous pores and gaps, and are rich in oxygen, making it impossible for anaerobic bacteria to survive. They also contain a large amount of phenolic substances and their derivatives, which are effective natural antibacterial substances.
[0005] However, the industrial application of hemp pulp still has significant shortcomings. First, the bast fibers of hemp are relatively long, and the raw materials contain high levels of impurities such as pectin, lignin, and metal ions, with a cellulose purity of only 65%-75%, which significantly increases the difficulty and cost of refining and pulping. Second, the presence of metal ions (especially transition metal ions such as iron and copper) can catalyze the decomposition of NMMO solvents, leading to poor stability of the spinning solution and even posing safety risks. Third, hemp pulp has a wide degree of polymerization distribution and low reactivity, resulting in poor solubility and spinnability of the spinning solution when used directly in Lyocell spinning.
[0006] While existing technologies report research on the preparation of Lyocell fibers from hemp pulp, these generally employ multi-step chemical processing, resulting in lengthy processes, high chemical consumption, and difficulties in achieving a balance between strength and toughness in fiber properties. For example, Chinese patent application number 202311844407.8 discloses a method for preparing hemp pulp Lyocell fibers. The preparation method includes the following steps: selection and pretreatment of hemp pulp, activation of hemp pulp raw material, adjustment of the degree of polymerization of hydrated cellulose, swelling of hydrated cellulose fibers, dissolution of the swollen pulp, buffering and settling of the dissolved pulp, and spinning. This scheme employs a multi-step pretreatment process combining chelating agent / acid treatment with hydrogen peroxide bleaching. This process is lengthy, and the high-temperature hydrogen peroxide bleaching destroys the natural antibacterial components of hemp fibers, while also affecting their mechanical properties. Regarding antibacterial properties, existing antibacterial Lyocell fibers are mostly achieved through post-treatment with added antibacterial agents, resulting in poor antibacterial durability and insufficient wash resistance. In addition, the fibrillation tendency of Lyocell fibers is also a major issue restricting their application. How to improve toughness and antibacterial properties while maintaining high strength is a problem that current technology urgently needs to overcome.
[0007] In view of this, the present invention is proposed. Summary of the Invention
[0008] The technical problem to be solved by the present invention is to overcome at least one of the shortcomings of the prior art and provide a method for preparing high-strength, high-toughness, long-lasting, strong antibacterial Lyocell fiber.
[0009] The primary objective of this invention is to use a one-step heteropolyacid process to treat hemp pulp, efficiently removing impurities such as metal ions and precisely controlling the degree of polymerization. Combined with blending with high-polymerization-degree wood pulp, this solves the problems of hemp pulp being unsuitable for Lyocell fiber production and having poor solubility, thus preparing a uniform and stable spinning solution.
[0010] The second objective of this invention is to maximize the preservation of the natural antibacterial components of hemp fiber through a mild heteropoly acid treatment process, so that the fiber has long-lasting and strong antibacterial properties that can withstand washing without the need for external antibacterial agents; at the same time, it optimizes the pulp structure and spinning process to solve the contradiction between the strength and toughness of Lyocell fiber, and achieves a synergistic improvement of the two, resulting in a high-strength, high-toughness fiber with long-lasting and strong antibacterial properties.
[0011] The third objective of this invention is to provide a simple process for preparing hemp-based Lyocell fibers, which has wide applicability of raw materials and can efficiently recycle both heteropoly acids and NMMO, filling a market gap, suitable for large-scale green production, and meeting the application needs of high-end textile fabrics.
[0012] To solve the above-mentioned technical problems, the basic concept of the technical solution adopted by the present invention is as follows:
[0013] In a first aspect, the present invention provides a method for preparing hemp-based Lyocell fibers, comprising:
[0014] (1) The hemp pulp was purified and activated by heteropolyacid in one step to obtain high-quality hemp pulp.
[0015] (2) The high-quality hemp pulp obtained in (1) is mixed with high-polymerization wood dissolving pulp to obtain mixed pulp. The mixed pulp is swollen, dissolved, filtered and degassed in a solvent to obtain a uniform spinning solution.
[0016] (3) Spin the spinning solution obtained in (2) to obtain hemp-based Lyocell fibers.
[0017] This invention provides a method for preparing hemp-based Lyocell fibers, comprising three steps: one-step purification and activation pretreatment of hemp pulp using heteropoly acids, preparation of a spinning solution by mixing with high-polymerization-degree wood dissolving pulp, and dry-jet wet spinning. This method overcomes the technical challenges of high metal ion and impurity content, wide polymerization degree distribution, and poor solubility in hemp pulp, which prevent its direct use in Lyocell fiber production. It also overcomes the shortcomings of traditional multi-step chemical treatment processes that severely damage the natural antibacterial components of hemp fibers and result in poor wash resistance of added antibacterial agents.
[0018] This invention utilizes the selective hydrolysis of heteropoly acids to remove metal ions (heavy metal content ≤10ppm) and precisely control the degree of polymerization (350-700), while maximally preserving natural antibacterial components such as phenols and flavonoids in hemp fibers, achieving a synergistic unity of purification, activation, and functional preservation. Through blending with high-polymerization-degree wood pulp, the viscosity of the spinning solution is stably controlled within the ideal spinnable range of 2800-3500 Pa·s. The resulting hemp Lyocell fiber possesses both high strength and toughness in mechanical properties and long-lasting strong antibacterial properties, filling the technological gap in the large-scale production of Lyocell fiber from hemp pulp.
[0019] During ordinary acid hydrolysis of cellulose, H + It randomly attacks all accessible glycosidic bonds, acting on both loose amorphous and tightly packed crystalline regions. This leads to two consequences: first, the degree of polymerization is difficult to control precisely, easily resulting in over-degradation; second, the crystalline region is damaged, ultimately reducing fiber strength. Heteropolyacids possess strong Brønsted acidity, reversible redox properties, a unique heteropolyanion synergistic catalytic mechanism, and excellent metal complexing ability. Specifically, the H+ generated by the dissociation of heteropolyacids... + Heteropoly anions can synergistically act on the amorphous regions of cellulose, selectively hydrolyzing the degree of polymerization from 800-1200 to precisely reduce it to 350-700, while causing minimal damage to the crystalline regions, thus preserving the strength framework of cellulose. These heteropoly anions can also form insoluble complexes with transition metal ions such as iron and copper, achieving efficient removal through precipitation (heavy metal content ≤10ppm), avoiding metal ion-catalyzed NMMO decomposition. Furthermore, the treatment conditions of heteropoly acids are mild, requiring no high-temperature oxidation bleaching, thus maximizing the preservation of naturally occurring antibacterial active ingredients in hemp fibers, such as phenols, flavonoids, and cannabinols, while also preserving their natural porous structure. This triple effect (selective depolymerization, efficient impurity removal, and mild preservation) cannot be simultaneously achieved by ordinary inorganic acids (non-selective, lacking complexing ability) and multi-step chemical methods (high-temperature oxidation destroying antibacterial components), thus laying the raw material foundation for the subsequent preparation of high-strength, high-toughness, and long-lasting antibacterial hemp Lyocell fibers.
[0020] In a further embodiment, in step (1), the heteropolyacid includes at least one of phosphotungstic acid, silicotungstic acid, phosphomolybdic acid, and silicotomolybdic acid. These heteropolyacids possess strong Brønsted acidity, reversible redox properties, and good thermal stability, along with excellent catalytic activity and recyclability. They can effectively hydrolyze β-1,4-glycosidic bonds in cellulose and exhibit high catalytic activity; this not only ensures the high efficiency and selectivity of pretreatment but also provides the recyclability advantage required for industrial applications.
[0021] In a further embodiment, the amount of heteropoly acid used is 0.003-0.3 mol / kg based on the mass of oven-dried cellulose pulp; preferably, the amount of heteropoly acid used is 0.01-0.1 mol / kg; and even more preferably, the amount of heteropoly acid used is 0.05-0.1 mol / kg.
[0022] In this invention, the amount of heteropoly acid used is measured based on the mass of oven-dried cellulose pulp. Specifically, in the one-step purification and activation pretreatment system, 0.003 to 0.3 moles of heteropoly acid are added for every 1 kg of oven-dried cellulose pulp. It should be clarified that in the technical solution of this invention, the cellulose pulp refers to the hemp pulp raw material actually processed in step (1).
[0023] When the dosage is less than 0.003 mol / kg, H + Insufficient concentration leads to incomplete removal of metal ions, limited improvement in whiteness, and a still high degree of polymerization. At concentrations above 0.3 mol / kg, excessive acid causes excessive degradation of cellulose molecular chains, damage to crystalline regions, decreased fiber strength, and excessive destruction of natural antibacterial components. An optimal concentration range of 0.01-0.1 mol / kg maximizes the retention of antibacterial components while ensuring sufficient purification and activation. A further optimized range of 0.05-0.1 mol / kg further balances the relationship between processing efficiency and fiber performance.
[0024] In a further step, step (1) involves a one-step purification and activation pretreatment process, which includes adding hemp pulp to a heteropoly acid solution and heating and maintaining the temperature for a certain period of time. The heteropoly acid can be added all at once or in batches, i.e., the heteropoly acid can be added in 2-3 batches during the pretreatment process to more precisely control the reaction rate and degree of polymerization.
[0025] Further, the concentration of hemp pulp is 1wt%-20wt%, more preferably, the concentration of hemp pulp is 8wt%-15wt%, and even more preferably, the concentration of hemp pulp is 10-12wt%.
[0026] A further embodiment is that the heating and heat preservation temperature is 50-100℃, and more preferably, the heating and heat preservation temperature is 60-90℃.
[0027] Further options have a processing time of 30-120 min, and more preferably, a processing time of 60-90 min.
[0028] Pulp concentration determines the effective contact frequency between heteropolyacids and cellulose; too low a concentration results in low efficiency, while too high a concentration leads to excessive viscosity and uneven mass transfer. Temperature is crucial for controlling the hydrolysis rate and selectivity; below 50°C, the reaction rate is too slow, while above 100°C, selectivity decreases and energy consumption increases. The optimal temperature range of 60-90°C ensures a suitable reaction rate while maintaining the selective attack of heteropolyacids on the amorphous region. Processing time is inversely related to temperature; an optimal time of 60-90 minutes ensures sufficient reaction time. The synergistic effect of these three factors allows the degree of polymerization of hemp pulp to be precisely reduced from 800-1200 to 350-700.
[0029] In a further embodiment, in step (1), the hemp pulp includes at least one of ramie pulp, flax pulp, jute pulp, and hemp pulp.
[0030] Different types of hemp contain different natural antibacterial components. Hemp contains cannabinoids, flax contains flavonoids and berberine hydrochloride, ramie contains tannins, pyrimidines, and purines, and jute contains phytosterols. These components are preserved under mild heteropolyacid treatment conditions. Simultaneously, the hollow structure inside the hemp fiber and the micropores on its surface create an oxygen-rich microenvironment, inhibiting the survival of anaerobic bacteria. In addition to the four types mentioned above, other bast fiber pulps such as sisal pulp and abaca pulp can also be used.
[0031] In a further embodiment, the initial average degree of polymerization of the hemp pulp is 800-1200.
[0032] In a further embodiment, in step (1), the average degree of polymerization of the high-quality hemp pulp is 350-700.
[0033] In a further embodiment, the high-quality hemp pulp contains ≤10 ppm heavy metals and has an ISO whiteness of ≥88%.
[0034] Maintaining the average degree of polymerization of high-quality hemp pulp at 350-700 prepares it for subsequent blending with high-polymer wood pulp. Once the hemp pulp is reduced to this range, it is blended proportionally with wood pulp of ≥700, resulting in a mixed pulp with a degree of polymerization falling precisely within the optimal 500-700 range for Lyocell spinning. A heavy metal content of ≤10ppm is more stringent than the standard Lyocell industrial requirement of ≤15ppm, further enhancing the safety of the NMMO solvent system and preventing side reactions caused by metal ions catalyzing NMMO decomposition. An ISO whiteness of ≥88% ensures the whiteness of the finished fiber and its subsequent dyeing performance.
[0035] In a further step, in step (1), the washing solution after one-step purification and activation pretreatment is regenerated and reused. Heteropolyacids have good water solubility and thermal stability, and their Keggin structure is maintained under mild pretreatment conditions, allowing them to be recycled.
[0036] Specifically, regeneration and recovery can be achieved through heating and evaporation concentration, cooling and crystallization, filtration, washing, and drying. If the washing liquid contains a high concentration of metal ions, solvent extraction can be used to remove the metal ions before evaporation and crystallization. Besides evaporation and crystallization, regeneration can also be achieved through solvent extraction (using organic solvents such as ether and acetone), ion exchange (using cation exchange resin to remove metal ions), or membrane separation (using nanofiltration membranes). Evaporation and crystallization is the simplest and lowest-cost method.
[0037] In a further embodiment, in step (2), the mixing ratio of high-quality hemp pulp to high-polymerization wood dissolving pulp is (1-9):1, preferably (1-5):1.
[0038] When high-quality hemp pulp is spun alone, its degree of polymerization ranges widely from 350 to 700, making it difficult to achieve stable spinnability. Introducing high-polymerization-degree wood pulp (≥700) can stabilize the total degree of polymerization of the mixed pulp within the optimal spinning range of 500-700. At a blending ratio of (1-9):1, the hemp pulp content should not be less than 10% to fully utilize the antibacterial properties and high modulus of hemp fiber; a hemp pulp content of no more than 90% ensures sufficient wood pulp to control the viscosity of the spinning solution. An optimal range of (1-5):1 further balances the synergistic relationship between functionality and spinnability.
[0039] In a further embodiment, the high degree of polymerization of the wood dissolving pulp is ≥700.
[0040] In a further embodiment, the high degree of polymerization wood dissolving pulp is selected from sulfate or sulfite dissolving pulp.
[0041] In a further embodiment, the high degree of polymerization wood dissolving pulp includes at least one of polysulfate softwood dissolving pulp, polysulfate hardwood dissolving pulp, polysulfite softwood dissolving pulp, and polysulfite hardwood dissolving pulp.
[0042] In a further embodiment, in step (2), the mass ratio of the mixed pulp to the solvent is 1:(2-12); preferably, the mass ratio of the mixed pulp to the solvent is 1:(2-10).
[0043] In a further embodiment, the solvent is a 60wt%-82wt% NMMO aqueous solution, preferably, the concentration of the NMMO aqueous solution is 60-80%.
[0044] In a further step, in step (2), antioxidants and stabilizers can be added to the mixed pulp to control the pH value within the range of 8-12.
[0045] In a further embodiment, the antioxidant is selected from one of propyl gallate, ethyl gallate, octyl gallate, and 2,6-di-tert-butyl-4-methylphenol.
[0046] The stabilizer is selected from hydroxylamine, carbamide, and inositol hexaphosphate.
[0047] In a further embodiment, the amount of antioxidant used is 100-500 mg / kg of the solvent mass;
[0048] The amount of stabilizer used is 100-500 mg / kg of solvent mass.
[0049] In a further embodiment, in step (2), the swelling temperature is 70-90℃;
[0050] Preferably, the swelling treatment is carried out at 75-90℃ to form a uniform and delicate porridge.
[0051] In a further step, in step (2), a dissolving machine is used for dissolution, and the dissolution conditions are 90-120℃ and 1.0-15.0 kPa.
[0052] In a further embodiment, in step (2), the degassing pressure is 0.2-1.0 kPa and the degassing time is 30-60 min.
[0053] In a further embodiment, in step (2), the cellulose content in the prepared spinning solution is 9-16 wt%; preferably, the cellulose content in the prepared spinning solution is 10-15 wt%.
[0054] In a further embodiment, in step (2), the viscosity of the prepared spinning solution is 2800-3500 Pa•s.
[0055] In this invention, the viscosity of the spinning solution is determined using a rotational rheometer at a temperature of 90–110°C, employing a steady-state shear mode, with the shear rate approaching zero (0.01–1 s⁻¹). -1 The apparent viscosity value measured within the range.
[0056] In a further embodiment, in step (3), the spinning is carried out using a dry-jet wet spinning process;
[0057] In a further embodiment, in step (3), the spinneret used in the dry-jet wet spinning has an orifice diameter of 0.05-0.2 mm; the spinning temperature is 90-110℃; the air gap height is 20-50 mm; and the spinning speed is ≥50 m / min.
[0058] Preferably, the spinneret orifice diameter is controlled to be 0.05-0.18 mm; the spinning box temperature is 90-108℃; and the air gap height is 20-48 mm.
[0059] Secondly, the present invention provides a hemp-based Lyocell fiber prepared by the aforementioned preparation method;
[0060] Preferably, the hemp-based Lyocell fiber has a dry breaking strength ≥ 4.6 cN / dtex, a dry breaking elongation ≥ 13%, a wet breaking strength ≥ 3.9 cN / dtex, and a wet modulus ≥ 1.3 cN / dtex;
[0061] Preferably, the linear density of the hemp-based Lyocell fiber is 1.29-1.40 dtex;
[0062] Preferably, after 20 washes, the hemp-based Lyocell fiber exhibits an antibacterial rate of ≥99% against Staphylococcus aureus, ≥99% against Escherichia coli, and ≥89% against Candida albicans.
[0063] The hemp Lyocell fiber prepared by this invention has high strength and toughness, and also has long-lasting strong antibacterial properties against Staphylococcus aureus, Escherichia coli and Candida albicans.
[0064] The dry breaking strength of the fiber of this invention is ≥4.6 cN / dtex, thanks to the selective protection of the crystalline region by the heteropoly acid, which maintains high crystalline integrity even when the degree of polymerization drops to 350-700; the dry breaking elongation is ≥13%, which is due to the heteropoly acid selectively removing defects in the amorphous region while retaining the complete length of the molecular chain, and the optimized molecular weight distribution of the high-polymer wood pulp gives the fiber excellent toughness; the wet breaking strength is ≥3.9 cN / dtex and the wet modulus is ≥1.3 cN / dtex (5% elongation), which reflects the excellent resistance to deformation of the fiber in the wet state, ensuring that the fabric has good dimensional stability and shape retention in the wet state.
[0065] Hemp fiber naturally contains antibacterial components such as phenols and flavonoids, and its porous internal structure creates an oxygen-rich microenvironment that inhibits anaerobic bacteria. The heteropolyacid treatment conditions are mild (60-90°C), eliminating the need for high-temperature oxidation and bleaching. These antibacterial components are preserved to the maximum extent and are covalently fixed within the fiber, unlike externally added antibacterial agents (such as nano-silver) which are physically adhered and detached during washing. Even after 20 washes, it maintains a >99% antibacterial rate, demonstrating truly long-lasting and strong antibacterial properties.
[0066] By adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art.
[0067] (1) Traditional purification of hemp pulp requires multiple steps, including acid treatment, alkali treatment, and chelating agent treatment, resulting in a long process and high chemical consumption. This invention uses heteropoly acids to process hemp pulp in a one-step process, achieving precise control of the degree of polymerization while removing metal ions, greatly simplifying the process and reducing production costs. Heteropoly acids can selectively degrade the amorphous regions of cellulose through catalytic oxidation reactions, while causing minimal damage to the crystalline regions, thereby improving reactivity while ensuring fiber strength.
[0068] (2) Existing antibacterial Lyocell fibers are mostly achieved through post-treatment with added antibacterial agents, which has the problems of poor antibacterial durability and insufficient wash resistance. Moreover, the added antibacterial agents may affect the mechanical properties of the fibers. This invention uses a mild heteropolyacid pretreatment process to maximize the retention of natural antibacterial components such as phenolic substances and flavonoids in hemp fibers, as well as the porous structure inside the fibers. This allows the finished fibers to maintain an antibacterial rate of >99% after 20 washes, achieving true long-lasting strong antibacterial effect without the need for added antibacterial agents.
[0069] (3) Single hemp pulp has a wide degree of polymerization distribution and poor solubility, making it difficult to obtain a uniform and stable spinning solution through direct spinning. This invention mixes treated high-quality hemp pulp with high-polymerization wood dissolving pulp in a specific ratio, which can not only control the degree of polymerization of the mixed pulp to the ideal range of 500-700, but also improve the rheological properties of the spinning solution, so that the viscosity of the spinning solution is stabilized at 2800-3500 Pa·s, ensuring the smooth progress of the dry-jet wet spinning process.
[0070] (4) This invention opens the molecular chains of hemp pulp cellulose and homogenizes the degree of polymerization by pretreatment with heteropoly acids, promotes the full dissolution of hemp pulp cellulose by NMMO solvent, and introduces high-polymer wood pulp to optimize the structure of spinning solution, so that the prepared hemp Lyocell fiber has a dry breaking strength ≥4.6 cN / dtex and a dry breaking elongation ≥13%, which significantly improves toughness while maintaining high strength, and solves the contradiction that it is difficult to balance strength and toughness in the prior art.
[0071] (5) This invention processes and adjusts the characteristics of different types of hemp pulp to adapt it to the processing requirements of Lyocell fiber, and successfully prepares hemp Lyocell fiber that combines the antibacterial properties of hemp fiber with the soft and delicate advantages of Lyocell fiber. Detailed Implementation
[0072] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments will be clearly and completely described below in conjunction with the embodiments of the present invention. The following embodiments are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0073] The main raw materials and reagents used in the embodiments and comparative examples of this invention are sourced as follows:
[0074] Ramie pulp, flax pulp, jute pulp, and hemp pulp all come from Hebei Jigao Chemical Fiber Co., Ltd., and have a cellulose content of ≥92%.
[0075] Polysulfate softwood dissolving pulp, polysulfate hardwood dissolving pulp, polysulfite softwood dissolving pulp, and polysulfite hardwood dissolving pulp were all supplied by China Textile Academy Green Fiber Co., Ltd., and are all Lyocell fiber-grade special pulps.
[0076] N-Methylmorpholine (NMMO, purity ≥99.5%) was purchased from Beijing Zhongfang Chemical Co., Ltd., and was prepared into an aqueous solution of the required concentration before use.
[0077] Phosphotungstic acid (H3PW) 12 O 40 • xH2O (analytical grade), silicotungstic acid (H4SiW) 12 O 40 • xH2O (analytical grade), phosphomolybdic acid (H3PMo) 12 O 40 • xH2O (analytical grade), molybdenum silicate (H4SiMo) 12 O 40 xH2O (analytical grade) was purchased from Maclean Chemical Reagent Co., Ltd.
[0078] Propyl gallate (PG, purity ≥98%) was purchased from Anhui Xinsheng Biotechnology Co., Ltd., and hydroxylamine (HA, purity ≥98%) was prepared in-house by China Textile Research Institute Co., Ltd.
[0079] All other chemical reagents whose sources were not specified were commercially available analytical grade.
[0080] In this invention, the dosage of heteropoly acid is measured based on the mass of oven-dried cellulose pulp. Taking Example 1 as an example, if the dosage of heteropoly acid is 0.1 mol / kg, it means that 0.1 mol of heteropoly acid is added for every 1 kg of oven-dried hemp pulp. The specific amount added is calculated proportionally based on the actual mass of oven-dried pulp fed into the plant.
[0081] Detection methods
[0082] 1. In this invention, the degree of polymerization of the hemp pulp, the degree of polymerization of high-quality hemp pulp, and the degree of polymerization of high-polymerization wood dissolving pulp are all determined according to the copper ethylenediamine (CED) method in GB / T 1548-2016 "Determination of Pulp Viscosity".
[0083] 2. In this invention, the heavy metal content is determined by inductively coupled plasma optical emission spectrometry (ICP-OES).
[0084] 3. In this invention, the ISO whiteness is measured according to GB / T 7974-2013 "Determination of blue diffuse reflectance factor D65 luminance of paper, paperboard and pulp (ISO luminance)".
[0085] 4. In this invention, the fiber linear density is determined according to GB / T 14335-2008 "Chemical Fibers - Test Method for Linear Density of Short Fibers".
[0086] 5. In this invention, the dry breaking strength and dry breaking elongation of the fiber are determined according to GB / T 14337-2008 "Test Method for Tensile Properties of Chemical Fibers - Short Fibers".
[0087] 6. In this invention, the wet breaking strength and wet modulus of the fiber are determined according to the wet tensile properties test method in GB / T 14463-2008 "Viscose Fiber Short Fiber". The wet modulus is the secant modulus of the fiber when the elongation in the wet state is 5%.
[0088] 7. In this invention, the antibacterial rate is determined according to GB / T 20944.3-2008 "Evaluation of antibacterial properties of textiles - Part 3: Shaking method", and the washing method is carried out according to GB / T 8629-2017 "Home washing and drying procedures for textile testing", with 20 washing cycles.
[0089] 8. In this invention, the viscosity of the spinning solution is determined using a rotational rheometer at 90°C and a shear rate approaching zero (0.01~1 s⁻¹). -1 The apparent viscosity value measured under conditions within the specified range.
[0090] Example 1
[0091] A method for preparing high-strength, high-toughness, long-lasting, strong antibacterial Lyocell fiber includes the following steps:
[0092] Step (1): Preparation of high-quality hemp pulp
[0093] Ramie pulp with an initial degree of polymerization of 882 was used, and after being loosened, pressed, concentrated, dispersed and moisture balanced, it was ready for use.
[0094] Weigh the above-mentioned pulp (based on oven-dry weight) and place it in a reaction vessel. Add deionized water to prepare a pulp system with a pulp concentration of 8 wt%. Weigh 0.1 mol of phosphomolybdic acid per kilogram of oven-dry pulp, dissolve it in deionized water, and add it to the reaction vessel. Stir until homogeneous. Incubate at 80°C for 70 min, stirring slowly and continuously to ensure sufficient contact between the heteropolyacids and the pulp.
[0095] After treatment, the pulp was repeatedly washed with deionized water until neutral (pH=6.5~7.5). The washing liquid could be recycled after regeneration to recover heteropoly acids. The washed pulp was then pressed, concentrated, dispersed, and air-dried for later use. The heavy metal content of the treated pulp was determined to be 10 ppm, the ISO whiteness was 90%, and the average degree of polymerization was 680.
[0096] The high-quality hemp pulp prepared above was mixed with polysulfate softwood dissolving pulp (degree of polymerization 708) and polysulfate hardwood dissolving pulp (degree of polymerization 720) at a mass ratio of 5:3:2 to obtain mixed pulp.
[0097] Step (2): Preparation of spinning solution
[0098] Take the mixed pulp prepared in step (1) and mix it with 74% NMMO aqueous solution at a mass ratio of 1:8.6. Add antioxidant (propyl gallate, amount of which is 200 mg / kg of solvent mass) and stabilizer (hydroxylamine, amount of which is 100 mg / kg of solvent mass), adjust the pH to 10, and swell at 80°C for 30 min to form a uniform and delicate cellulose porridge.
[0099] Cellulose slurry was dissolved at 120°C and 7.7 kPa for 60 min to prepare a spinning solution with a cellulose concentration of 11 wt%. The viscosity of the spinning solution at 100°C was measured to be 3300 Pa·s.
[0100] Step (3): Spinning and forming
[0101] The spinning solution was deaerated at 90°C and 0.8 kPa for 45 min.
[0102] The spinning process was carried out using a dry-jet wet spinning method, with the spinneret orifice diameter controlled at 0.085 mm, the spinning box temperature at 108°C, the air gap height at 20 mm, the spinning speed at 60 m / min, the blowing speed at 25 m / min, the blowing temperature at 12.5°C, and the blowing humidity at 67.3%.
[0103] After spinning, the fibers are coagulated in a coagulation bath (15% NMMO concentration, 25°C), washed, dried, and wound to obtain hemp Lyocell fibers.
[0104] The obtained hemp Lyocell fiber has long-lasting and strong antibacterial properties. The fiber properties are shown in Table 1.
[0105] Example 2
[0106] The preparation of a high-strength, high-toughness, long-lasting, strong antibacterial Lyocell fiber includes the following steps:
[0107] Step (1): Preparation of high-quality hemp pulp
[0108] Flax pulp with an initial degree of polymerization of 1008 is used, and is prepared for use after being loosened, pressed, concentrated, dispersed and moisture balanced.
[0109] Weigh the above-mentioned pulp (based on oven-dry weight) and place it in a reaction vessel. Add deionized water to prepare a pulp system with a pulp concentration of 10 wt%. Weigh 0.08 mol of phosphomolybdic acid and 0.02 mol of silicotungstic acid per kilogram of oven-dry pulp, dissolve them in deionized water, and add them to the reaction vessel. Stir until homogeneous. Incubate at 65°C for 65 min with continuous slow stirring.
[0110] After treatment, the pulp is repeatedly washed with deionized water until neutral (pH=6.5~7.5). The washing liquid can be recycled after regeneration to recover heteropoly acids. The washed pulp is then pressed, concentrated, dispersed, and air-dried for later use.
[0111] The heavy metal content of the treated pulp was measured to be 6 ppm, the ISO whiteness was 95%, and the average degree of polymerization was 535.
[0112] The high-quality hemp pulp prepared above was mixed with high-polymer sulfite needlewood dissolving pulp (polymerization degree 740) at a mass ratio of 2:1 to obtain mixed pulp.
[0113] Step (2): Preparation of spinning solution
[0114] Take the mixed pulp prepared in step (1) and mix it with 73.5% NMMO aqueous solution at a mass ratio of 1:7.3. Add antioxidant (octyl gallate, amount of which is 250 mg / kg of solvent mass) and stabilizer (inositol hexaphosphate, amount of which is 300 mg / kg of solvent mass) to adjust the pH to 10, and swell at 80°C for 30 min to form cellulose porridge.
[0115] Cellulose slurry was dissolved at 105°C and 6.0 kPa to prepare a spinning solution with a cellulose concentration of 12 wt%. The viscosity of the spinning solution at 100°C was measured to be 3000 Pa·s.
[0116] Step (3): Spinning and forming
[0117] The spinning solution was deaerated at 90°C and 0.6 kPa for 60 min.
[0118] The spinning process was carried out using a dry-jet wet spinning method, with the spinneret orifice diameter controlled at 0.085 mm, the spinning box temperature at 100°C, the air gap height at 20 mm, the spinning speed at 70 m / min, the air blowing speed at 25 m / min, the air blowing temperature at 16.2°C, and the air blowing humidity at 62.5%. Subsequent solidification, washing, drying, and winding were the same as in Example 1.
[0119] The obtained hemp Lyocell fiber has long-lasting and strong antibacterial properties. The fiber properties are shown in Table 1.
[0120] Example 3
[0121] The preparation of a high-strength, high-toughness, long-lasting, strong antibacterial Lyocell fiber includes the following steps:
[0122] Step (1): Preparation of high-quality hemp pulp
[0123] Jute pulp with an initial degree of polymerization of 1200 is used, and is prepared for use after being loosened, pressed, concentrated, dispersed and moisture balanced.
[0124] Weigh the above-mentioned pulp (based on oven-dry weight) and place it in a reaction vessel. Add deionized water to prepare a pulp system with a pulp concentration of 10 wt%. Weigh 0.05 mol of phosphotungstic acid and 0.05 mol of molybdic acid per kilogram of oven-dry pulp, dissolve them in deionized water, and add them to the reaction vessel. Stir until homogeneous. Incubate at 65°C for 75 min with continuous slow stirring.
[0125] After treatment, the pulp is repeatedly washed with deionized water until neutral (pH=6.5~7.5). The washing liquid can be recycled after regeneration to recover heteropoly acids. The washed pulp is then pressed, concentrated, dispersed, and air-dried for later use.
[0126] The heavy metal content of the treated pulp was measured to be 9 ppm, the ISO whiteness was 85%, and the average degree of polymerization was 423.
[0127] The high-quality hemp pulp prepared above was mixed with polysulfate broadleaf dissolving pulp (degree of polymerization 782) at a mass ratio of 4:1 to obtain mixed hemp pulp meal.
[0128] Step (2): Preparation of spinning solution
[0129] Take the mixed hemp pulp prepared in step (1) and mix it with 74.5% NMMO aqueous solution at a mass ratio of 1:8.5. Add antioxidant (2,6-di-tert-butyl-4-methylphenol, amount of 180 mg / kg of pulp mass) and stabilizer (carbamide, amount of 320 mg / kg of pulp mass), adjust the pH to 10, and swell at 80°C for 30 min to form cellulose porridge.
[0130] Cellulose slurry was dissolved at 106°C and 5.7 kPa to prepare a spinning solution with a cellulose concentration of 12.5 wt%. The viscosity of the spinning solution at 100°C was measured to be 2900 Pa·s.
[0131] Step (3): Spinning and forming
[0132] The spinning solution was deaerated at 90°C and 0.7 kPa for 60 min.
[0133] The spinning process was carried out using a dry-jet wet spinning method, with the spinneret orifice diameter controlled at 0.075 mm, the spinning box temperature at 106°C, the air gap height at 20 mm, the spinning speed at 50 m / min, the air blowing speed at 25 m / min, the air blowing temperature at 16.8°C, and the air blowing humidity at 54.9%. Subsequent solidification, washing, drying, and winding were the same as in Example 1.
[0134] The obtained hemp Lyocell fiber has long-lasting and strong antibacterial properties. The fiber properties are shown in Table 1.
[0135] Example 4
[0136] The preparation of a high-strength, high-toughness, long-lasting, strong antibacterial Lyocell fiber includes the following steps:
[0137] Step (1): Preparation of high-quality hemp pulp
[0138] Hemp pulp with an initial degree of polymerization of 1093 was used and then processed through decomposition, pressing, concentration, dispersion, and moisture balancing before use.
[0139] Weigh the above pulp (based on oven-dry weight) and place it in a reaction vessel. Add deionized water to prepare a pulp system with a pulp concentration of 12 wt%. Weigh 0.1 mol of phosphotungstic acid per kilogram of oven-dry pulp, dissolve it in deionized water, and add it to the reaction vessel. Stir until homogeneous. Incubate at 70°C for 80 min with continuous slow stirring.
[0140] After treatment, the pulp is repeatedly washed with deionized water until neutral (pH=6.5~7.5). The washing liquid can be recycled after regeneration to recover heteropoly acids. The washed pulp is then pressed, concentrated, dispersed, and air-dried for later use.
[0141] The heavy metal content of the treated pulp was measured to be 11 ppm, the ISO whiteness was 90%, and the average degree of polymerization was 682.
[0142] The high-quality hemp pulp prepared above was mixed with polysulfite broadleaf dissolving pulp (degree of polymerization 710) and polysulfite softwood dissolving pulp (degree of polymerization 755) at a mass ratio of 3:1:1 to obtain mixed pulp.
[0143] Step (2): Preparation of spinning solution
[0144] Take the mixed pulp prepared in step (1) and mix it with 74% NMMO aqueous solution at a mass ratio of 1:7.2. Add antioxidant (ethyl gallate, amount of which is 350 mg / kg of solvent mass) and stabilizer (hydroxylamine, amount of which is 280 mg / kg of solvent mass), adjust the pH to 10, and swell at 80°C for 30 min to form cellulose porridge.
[0145] Cellulose slurry was dissolved at 110°C and 5.2 kPa to prepare a spinning solution with a cellulose concentration of 14 wt%. The viscosity of the spinning solution at 100°C was measured to be 3180 Pa·s.
[0146] Step (3): Spinning and forming
[0147] The spinning solution was deaerated at 90°C and 0.9 kPa for 60 min.
[0148] The spinning process was carried out using a dry-jet wet spinning method, with the spinneret orifice diameter controlled at 0.085 mm, the spinning box temperature at 105°C, the air gap height at 20 mm, the spinning speed at 65 m / min, the air blowing speed at 25 m / min, the air blowing temperature at 18.2°C, and the air blowing humidity at 34.8%. Subsequent solidification, washing, drying, and winding were the same as in Example 1.
[0149] The obtained hemp Lyocell fiber has long-lasting and strong antibacterial properties. The fiber properties are shown in Table 1.
[0150] Example 5
[0151] The preparation of a high-strength, high-toughness, long-lasting, strong antibacterial Lyocell fiber includes the following steps:
[0152] Step (1): Preparation of high-quality hemp pulp
[0153] Ramie pulp with an initial degree of polymerization of 900 is used, and is then processed through loosening, pressing, concentration, dispersion, and moisture balancing before use.
[0154] Weigh the above-mentioned pulp (based on oven-dry weight) and place it in a reaction vessel. Add deionized water to prepare a pulp system with a consistency of 11 wt%. Weigh 0.1 mol of molybdic acid and 0.03 mol of silicotungstic acid per kilogram of oven-dry pulp, dissolve them in deionized water, and add them to the reaction vessel. Stir until homogeneous. Incubate at 80°C for 68 min with continuous slow stirring.
[0155] After treatment, the pulp is repeatedly washed with deionized water until neutral (pH=6.5~7.5). The washing liquid can be recycled after regeneration to recover heteropoly acids. The washed pulp is then pressed, concentrated, dispersed, and air-dried for later use.
[0156] The heavy metal content of the treated pulp was measured to be 9 ppm, the ISO whiteness was 91%, and the average degree of polymerization was 577.
[0157] The high-quality hemp pulp prepared above was mixed with polysulfate needlewood dissolving pulp (degree of polymerization 750) at a mass ratio of 3:1 to obtain mixed pulp.
[0158] Step (2): Preparation of spinning solution
[0159] Take the mixed pulp prepared in step (1) and mix it with 75% NMMO aqueous solution at a mass ratio of 1:7.7. Add antioxidant (octyl gallate, amount of which is 280 mg / kg of solvent mass) and stabilizer (carbamide, amount of which is 350 mg / kg of solvent mass) to adjust the pH to 10, and swell at 80°C for 30 min to form cellulose porridge.
[0160] Cellulose slurry was dissolved at 104°C and 5.7 kPa to prepare a spinning solution with a cellulose concentration of 12 wt%. The viscosity of the spinning solution at 100°C was measured to be 2950 Pa·s.
[0161] Step (3): Spinning and forming
[0162] The spinning solution was deaerated at 90°C and 0.7 kPa for 60 min.
[0163] The spinning process was carried out using a dry-jet wet spinning method, with the spinneret orifice diameter controlled at 0.085 mm, the spinning box temperature at 108°C, the air gap height at 20 mm, the spinning speed at 70 m / min, the air blowing speed at 25 m / min, the air blowing temperature at 17.4°C, and the air blowing humidity at 60.5%. Subsequent solidification, washing, drying, and winding were the same as in Example 1.
[0164] The obtained hemp Lyocell fiber has long-lasting and strong antibacterial properties. The fiber properties are shown in Table 1.
[0165] Example 6
[0166] The preparation of a high-strength, high-toughness, long-lasting, strong antibacterial Lyocell fiber includes the following steps:
[0167] Step (1): Preparation of high-quality hemp pulp
[0168] Jute pulp with an initial degree of polymerization of 1110 was used, and after being loosened, pressed, concentrated, dispersed and moisture balanced, it was ready for use.
[0169] Weigh the above pulp (based on oven-dry weight) and place it in a reaction vessel. Add deionized water to prepare a pulp system with a consistency of 15 wt%. Weigh 0.08 mol of silicotungstic acid and 0.03 mol of phosphotungstic acid per kilogram of oven-dry pulp, dissolve them in deionized water, and add them to the reaction vessel. Stir until homogeneous. Incubate at 80°C for 80 min with continuous slow stirring.
[0170] After treatment, the pulp is repeatedly washed with deionized water until neutral (pH=6.5~7.5). The washing liquid can be recycled after regeneration to recover heteropoly acids. The washed pulp is then pressed, concentrated, dispersed, and air-dried for later use.
[0171] The heavy metal content of the treated pulp was measured to be 5 ppm, the ISO whiteness was 92%, and the average degree of polymerization was 590.
[0172] The high-quality hemp pulp prepared above was mixed with polysulfate needlewood dissolving pulp (degree of polymerization 724) at a mass ratio of 1:1 to obtain mixed pulp.
[0173] Step (2): Preparation of spinning solution
[0174] Take the mixed pulp prepared in step (1) and mix it with 73% NMMO aqueous solution at a mass ratio of 1:8.3. Add antioxidant (propyl gallate, amount of which is 340 mg / kg of solvent mass) and stabilizer (inositol hexaphosphate, amount of which is 290 mg / kg of solvent mass) to adjust the pH to 10, and swell at 80°C for 30 min to form cellulose porridge.
[0175] Cellulose slurry was dissolved at 103°C and 4.7 kPa to prepare a spinning solution with a cellulose concentration of 12.5 wt%. The viscosity of the spinning solution at 100°C was measured to be 3530 Pa·s.
[0176] Step (3): Spinning and forming
[0177] The spinning solution was deaerated at 90°C and 0.8 kPa for 60 min.
[0178] The spinning process was carried out using a dry-jet wet spinning method, with the spinneret orifice diameter controlled at 0.075 mm, the spinning box temperature at 98°C, the air gap height at 20 mm, the spinning speed at 80 m / min, the air blowing speed at 25 m / min, the air blowing temperature at 23.3°C, and the air blowing humidity at 40.4%. Subsequent solidification, washing, drying, and winding were the same as in Example 1.
[0179] Comparative Example 1 (fibers prepared from pure wood pulp)
[0180] Step (1): Use high polysulfite needle dissolving pulp (degree of polymerization 740) for Lyocell fiber production as raw material, without heteropoly acid pretreatment.
[0181] Step (2): The above pulp was mixed with a 73.5% NMMO aqueous solution at a mass ratio of 1:7.3. An antioxidant (octyl gallate, 250 mg / kg of solvent mass) and a stabilizer (inositol hexaphosphate, 300 mg / kg of solvent mass) were added to adjust the pH to 10. The mixture swelled at 80°C for 30 min to form a cellulose pulp. This pulp was then dissolved at 105°C and 6.0 kPa to prepare a spinning solution with a cellulose concentration of 10.8 wt%. The viscosity of the spinning solution at 100°C was measured to be 3070 Pa·s.
[0182] Step (3): The spinning and forming conditions are the same as in Example 2. Finally, pure wood pulp Lyocell fibers were obtained, and the fiber properties are shown in Table 1.
[0183] Comparative Example 2 (Preparation of Fiber from Pure Hemp Pulp)
[0184] Step (1): Jute pulp with an initial degree of polymerization of 1200 is used for decomposition, pressing, concentration, dispersion and moisture balancing before use.
[0185] Weigh the above-mentioned pulp (based on oven-dry weight) and place it in a reaction vessel. Add deionized water to prepare a pulp system with a pulp concentration of 10 wt%. Weigh 0.05 mol of phosphotungstic acid and 0.05 mol of molybdic acid per kilogram of oven-dry pulp, dissolve them in deionized water, and add them to the reaction vessel. Stir until homogeneous. Incubate at 65°C for 75 min with continuous slow stirring.
[0186] After processing, the pulp is repeatedly washed with deionized water until neutral. The washed pulp is then pressed, concentrated, dispersed, and air-dried for later use.
[0187] The heavy metal content of the treated pulp was measured to be 9 ppm, the ISO whiteness was 85%, and the average degree of polymerization was 423.
[0188] This comparative example does not involve blending with high-polymer wood pulp; the processed hemp pulp is used directly for spinning.
[0189] Step (2): Mix the above-mentioned hemp pulp with a 74.5% NMMO aqueous solution at a mass ratio of 1:8.5. Add an antioxidant (2,6-di-tert-butyl-4-methylphenol, 180 mg / kg of solvent mass) and a stabilizer (carbamide, 320 mg / kg of solvent mass), adjust the pH to 10, and swell at 80°C for 30 min to form a cellulose slurry. Dissolve at 106°C and 5.7 kPa to prepare a spinning solution with a cellulose concentration of 12.5 wt%. The viscosity of the spinning solution at 100°C was measured to be 1470 Pa·s.
[0190] Step (3): The spinning and forming conditions are the same as in Example 3. Finally, hemp Lyocell fibers were obtained, and the fiber properties are shown in Table 1.
[0191] Comparative Example 3 (using a multi-step chemical treatment process)
[0192] Step (1): Preparation of pulp
[0193] Ramie pulp with an initial degree of polymerization of 882 was used, and after being loosened, pressed, concentrated, dispersed and moisture balanced, it was ready for use.
[0194] Weigh the above pulp (by oven-dry weight) and place it in a reaction vessel, then proceed with the following multi-step chemical treatment:
[0195] Chelating acid treatment: Add deionized water to prepare a pulp system with a consistency of 8 wt%. Add 0.5 wt% sodium hexametaphosphate as a chelating agent based on the oven-dry weight of the pulp. Adjust the pH to 2-3 with hydrochloric acid and incubate at 60°C for 60 min. After treatment, wash the pulp with deionized water until neutral.
[0196] Bleaching treatment: The pulp was reformulated to a pulp consistency of 8 wt%, and 0.1 wt% sodium silicate was added as a stabilizer, followed by 0.5 wt% hydrogen peroxide (H2O2) as a bleaching agent. The mixture was then treated at 90°C for 70 min. After treatment, the pulp was washed with deionized water until neutral.
[0197] Enzyme activation treatment: The above pulp was reconstituted into a pulp system with a pulp concentration of 8 wt%. The pH was adjusted to 5.0 with acid, and 1.0 wt% of a cellulase complex (liquid cellulase) was added. The mixture was then activated at 55°C for 90 min. After activation, the pH was adjusted to 10-11 with an alkaline solution (sodium hydroxide) to terminate the enzyme reaction. The pulp was washed with deionized water until neutral.
[0198] The washed pulp was pressed, concentrated, dispersed, and air-dried for later use. The heavy metal content of the treated pulp was measured to be 12 ppm, the ISO whiteness was 88%, and the average degree of polymerization was 553.
[0199] The high-quality hemp pulp prepared above was mixed with polysulfate softwood dissolving pulp (degree of polymerization 750) and polysulfate hardwood dissolving pulp (degree of polymerization 720) at a mass ratio of 5:3:2 to obtain mixed pulp.
[0200] The steps and conditions in steps (2) and (3) are the same as in Example 1. The properties of the obtained ramie Lyocell fibers are shown in Table 1.
[0201] Comparative Example 4
[0202] The difference between this comparative example and Example 1 is that the heteropoly acid in step (1) is replaced with ordinary hydrochloric acid, specifically including:
[0203] Step (1): Preparation of pulp
[0204] Ramie pulp with an initial degree of polymerization of 882 was used, and after being loosened, pressed, concentrated, dispersed and moisture balanced, it was ready for use.
[0205] Weigh the above pulp (by oven-dry weight) and place it in a reaction vessel. Add deionized water to prepare a pulp system with a pulp concentration of 8%. Follow the same H... + Concentration (compared to the heteropolyacid H in Example 1) + (Concentration consistent), hydrochloric acid (HCl) was used instead of heteropoly acid, and the mixture was treated at 80°C for 70 min. After treatment, the pulp was repeatedly washed with deionized water until neutral, then pressed, concentrated, dispersed, and air-dried for later use.
[0206] The treated pulp was found to have a heavy metal content of 18 ppm, an ISO whiteness of 82%, and an average degree of polymerization of 380. The treated hemp pulp was then mixed with polysulfate softwood dissolving pulp (degree of polymerization 750) and polysulfate hardwood dissolving pulp (degree of polymerization 720) at a mass ratio of 5:3:2.
[0207] Steps (2) and (3): Same as in Example 1. Fiber properties are shown in Table 1.
[0208] Comparative Example 5 (Insufficient amount of heteropolyacid)
[0209] This comparative example uses the exact same conditions and steps as Example 1, the only difference being that the amount of heteropoly acid (phosphomolybdic acid) used is 0.002 mol / kg.
[0210] Step (1) The heavy metal content of the treated pulp was determined to be 20 ppm, the ISO whiteness was 79%, and the average degree of polymerization was 768.
[0211] The fiber properties are shown in Table 1.
[0212] Comparative Example 6 (excessive use of heteropolyacids)
[0213] This comparative example uses the exact same conditions and steps as Example 1, the only difference being that the amount of heteropoly acid (phosphomolybdic acid) used is 0.35 mol / kg.
[0214] Step (1) The heavy metal content of the treated pulp was determined to be 10 ppm, the ISO whiteness was 88%, and the average degree of polymerization was 280.
[0215] The fiber properties are shown in Table 1.
[0216] Comparative Example 7 (One-step purification and activation pretreatment of heteropolyacids at a lower temperature)
[0217] This comparative example uses the same conditions and steps as Example 1, the only difference being that after adding phosphomolybdic acid in step (1), it is kept at 50°C for 70 min.
[0218] Step (1) The heavy metal content of the treated pulp was determined to be 11 ppm, the ISO whiteness was 79%, and the average degree of polymerization was 790.
[0219] Comparative Example 8 (One-step purification and activation pretreatment of heteropolyacids at a higher temperature)
[0220] This comparative example uses the same conditions and steps as Example 1, the only difference being that after adding phosphomolybdic acid in step (1), it is kept at 100°C for 70 min.
[0221] Step (1) The heavy metal content of the treated pulp was determined to be 8 ppm, the ISO whiteness was 80%, and the average degree of polymerization was 320.
[0222] The fiber properties are shown in Table 1.
[0223] Comparative Example 9 (using other heteropoly acids)
[0224] The difference between this comparative example and Example 1 is that phosphovanadic acid (H5PV2Mo) was used in step (1). 10 O 40 (This is a substitute for phosphomolybdic acid.) Other conditions and procedures are the same as in Example 1.
[0225] Step (1) The heavy metal content of the treated pulp was determined to be 10 ppm, the ISO whiteness was 80%, and the average degree of polymerization was 209.
[0226] The heavy metal content, ISO whiteness, and average degree of polymerization of the pulp obtained in step (1) of each embodiment and comparative example are summarized as follows:
[0227] Table 1
[0228]
[0229] The properties of the fibers prepared in each embodiment and comparative example are shown below.
[0230] Table 2
[0231]
[0232] Based on the analysis of data from Table 1 (heavy metal content, ISO whiteness, and average degree of polymerization) and Table 2 (fiber mechanical properties and antibacterial rate), the conclusions are as follows:
[0233] As shown in Table 1, after the pulp of Examples 1-6 was treated with heteropoly acid in one step, the heavy metal content was controlled within the range of 5-11 ppm, with Examples 2, 5, and 6 reaching ≤9 ppm; the ISO whiteness was between 85% and 95%, except for Example 3 which was 85%, the rest were all above 90%; the average degree of polymerization was in the range of 350-700 (423-682).
[0234] Comparative Example 4 replaced the heteropoly acid with hydrochloric acid, although the same H+ was controlled. + The concentration was low, but heavy metal removal was incomplete (18 ppm), the degree of polymerization was excessively degraded to 380, and the whiteness was only 82%, indicating that ordinary inorganic acids cannot achieve the dual functions of selective hydrolysis and metal complexation. Comparative Example 5 (acid dosage 0.002 mol / kg) resulted in heavy metal residue of 20 ppm, whiteness of 79%, and the degree of polymerization only decreased to 768, indicating insufficient degradation and impurity removal. Comparative Example 6 (acid dosage 0.35 mol / kg) resulted in excessive degradation to the degree of polymerization of 280, the wet modulus decreased to 1.00 cN / dtex, 5%, and the fiber strength decreased significantly. Comparative Example 7 (50℃) showed insufficient reaction, with a degree of polymerization of 790 and a dry elongation of only 10.23%. Comparative Example 8 (100℃) showed decreased selectivity, with a degree of polymerization of 320 and a wet modulus of 0.95 cN / dtex, 5%. Comparative Example 9 replaced phosphomolybdic acid with phosphovanadic acid, and due to excessive oxidizing power, the degree of polymerization was severely reduced to 209, resulting in comprehensive deterioration of fiber properties.
[0235] As shown in Table 2, the dry breaking strength of Examples 1-6 is 4.60-4.95 cN / dtex, the wet breaking strength is 3.93-4.31 cN / dtex, the dry breaking elongation is 13.2%-14.8%, the wet modulus is 1.31-1.52 cN / dtex (5%), and the linear density is 1.29-1.40 dtex, indicating that the fibers possess high strength and high toughness mechanical properties. After 20 washes, the antibacterial rate against Staphylococcus aureus and Escherichia coli is ≥99%, and the antibacterial rate against Candida albicans is ≥89%, demonstrating long-lasting and strong antibacterial properties.
[0236] Comparative Example 1 (pure wood pulp) had a dry strength of 4.76 cN / dtex and a wet strength of 4.16 cN / dtex, but its dry elongation was only 11.5% and wet modulus was only 1.28 cN / dtex, and its antibacterial rate was significantly reduced (75% for Staphylococcus aureus and 60% for Alternanthera philoxeroides), indicating that fibers without hemp pulp lack antibacterial properties. Comparative Example 2 (pure hemp pulp) had excellent antibacterial properties (99 / 99 / 98), but its dry strength was only 3.51 cN / dtex, wet strength was 3.09 cN / dtex, dry elongation was 10.8%, and wet modulus was 1.04 cN / dtex, 5%, indicating that hemp pulp alone cannot balance strength and toughness. Comparative Example 3 (multi-step chemical method) reduced the antibacterial rate of Alternanthera philoxeroides to 80%, and its dry strength was 3.93 cN / dtex and wet modulus was 1.13 cN / dtex, 5%, both lower than Example 1, proving that multi-step chemical treatment destroys natural antibacterial components and damages fiber mechanical properties. The fiber properties of Comparative Examples 4-9 were also lower than those of the corresponding embodiments, further demonstrating the superiority of the heteropolyacid one-step method and its parameter range of the present invention.
[0237] In summary, the data in Tables 1 and 2 together show that: suitable heteropolyacid treatment conditions can prepare high-quality hemp pulp with moderate degree of polymerization, low heavy metal content, and high whiteness; fibers containing hemp pulp have antibacterial properties, fibers containing high-polymer wood pulp have high strength properties, and after hemp pulp and high-polymer wood pulp are mixed, the fibers have both high strength and high toughness mechanical properties and long-lasting strong antibacterial properties.
[0238] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-described technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A method for preparing hemp-based Lyocell fibers, characterized in that, include: (1) The hemp pulp was purified and activated by heteropolyacid in one step to obtain high-quality hemp pulp. (2) The high-quality hemp pulp obtained in (1) is mixed with high-polymerization wood dissolving pulp to obtain mixed pulp. The mixed pulp is swollen, dissolved, filtered and degassed in a solvent to obtain a uniform spinning solution. (3) Spin the spinning solution obtained in (2) to obtain hemp-based Lyocell fibers.
2. The preparation method according to claim 1, characterized in that, In step (1), the heteropolyacid includes at least one of phosphotungstic acid, silicotungstic acid, phosphotomolybdic acid, and silicotomolybdic acid; Preferably, the amount of heteropoly acid used is 0.003-0.3 mol / kg based on the mass of oven-dried cellulose pulp; Preferably, the amount of heteropoly acid used is 0.01-0.1 mol / kg based on the mass of the oven-dried cellulose pulp.
3. The preparation method according to claim 1 or 2, characterized in that, In step (1), the one-step purification and activation pretreatment includes: adding hemp pulp into a heteropoly acid solution and heating and keeping it warm for a certain period of time; Preferably, the concentration of hemp pulp is 1wt%-20wt%, more preferably, the concentration of hemp pulp is 8wt%-15wt%. Preferably, the heating and heat preservation temperature is 50-100℃, and more preferably, the heating and heat preservation temperature is 60-90℃; Preferably, the processing time is 30-120 min, and more preferably, the processing time is 60-90 min.
4. The preparation method according to any one of claims 1-3, characterized in that, In step (1), the hemp pulp includes at least one of ramie pulp, flax pulp, jute pulp, and hemp pulp; Preferably, the initial average degree of polymerization of the hemp pulp is 800-1200.
5. The preparation method according to any one of claims 1-4, characterized in that, In step (1), the average degree of polymerization of the high-quality hemp pulp is 350-700; Preferably, the high-quality hemp pulp contains ≤10 ppm heavy metals and has an ISO whiteness of ≥88%.
6. The preparation method according to any one of claims 1-5, characterized in that, In step (1), the washing liquid, after being purified and activated by a one-step method, is regenerated and then recycled.
7. The preparation method according to any one of claims 1-6, characterized in that, In step (2), the mixing ratio of high-quality hemp pulp and high-polymerization degree wood dissolving pulp is (1-9):1, preferably (1-5):1; Preferably, the high degree of polymerization of the wood dissolving pulp has an average degree of polymerization ≥ 700; Preferably, the high degree of polymerization wood dissolving pulp is selected from sulfate or sulfite dissolving pulp; Preferably, the high degree of polymerization wood dissolving pulp includes at least one of polysulfate softwood dissolving pulp, polysulfate hardwood dissolving pulp, polysulfite softwood dissolving pulp, and polysulfite hardwood dissolving pulp.
8. The preparation method according to any one of claims 1-7, characterized in that, In step (2), the mass ratio of the mixed pulp to the solvent is 1:(2-12). Preferably, the solvent is a 60wt%-82wt% NMMO aqueous solution.
9. The preparation method according to any one of claims 1-8, characterized in that, In step (2), the swelling temperature is 70-90℃; Preferably, the dissolution conditions are 90-120°C and 1.0-15.0 kPa; Preferably, the degassing pressure is 0.2-1.0 kPa and the degassing time is 30-60 min; Preferably, the cellulose content in the prepared spinning solution is 9-16 wt%; Preferably, the viscosity of the prepared spinning solution is 2800-3500 Pa•s.
10. A hemp-based Lyocell fiber prepared by the preparation method according to any one of claims 1-9; Preferably, the hemp-based Lyocell fiber has a dry breaking strength ≥ 4.6 cN / dtex, a dry breaking elongation ≥ 13%, a wet breaking strength ≥ 3.9 cN / dtex, and a wet modulus ≥ 1.3 cN / dtex; Preferably, the linear density of the hemp-based Lyocell fiber is 1.29-1.40 dtex; Preferably, after 20 washes, the hemp-based Lyocell fiber exhibits an antibacterial rate of ≥99% against Staphylococcus aureus, ≥99% against Escherichia coli, and ≥89% against Candida albicans.
Citation Information
Patent Citations
Hemp pulp lyocell fiber and preparation method thereof
CN117822140A