A flavoring and deodorizing and functional modification formula and process of air fiber material

By combining multi-component essential oils with reactive antioxidants, the odor problem of air fiber materials when using economical POE raw materials is solved, achieving long-term fragrance retention and antibacterial and anti-mite effects, and enhancing the sensory experience and functionality of the materials.

CN123133018APending Publication Date: 2026-11-20GUIZHOU DAZIRAN TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611266242.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing air fiber materials, when using economical POE raw materials, suffer from plastic odor, making it difficult to balance cost reduction with long-lasting fragrance and antibacterial and anti-mite functions.

Method used

By combining a multi-component essential oil system with reactive antioxidants, the essential oil molecules are chemically anchored to the matrix resin through maleic anhydride grafting onto polyolefins. Odor removal and aroma retention are achieved through hot-air-cold-air treatment, forming a three-dimensional functional network of molecular anchoring, synergistic antioxidant, and gradient release.

Benefits of technology

Without compromising the material's resilience and fatigue performance, it effectively masks odors, prolongs aroma retention time, enhances antibacterial and anti-mite properties, and meets the requirements of a high-end sensory experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The application discloses a kind of air fiber material's flavoring and functional modification formula and process, belong to polyolefin air fiber modification processing technical field.The application sets up two sets of systems of antioxidant compatible masterbatch prefabricated formula and finished product multivariate compound essential oil modification formula, and is matched with masterbatch prefabrication, essential oil blending, extrusion molding, hot air odor removal, cold wind shaping continuous process;Maleic anhydride grafted polyolefin is used to realize essential oil molecule anchoring lock fragrance, and sulfur-phenol and phosphite ester compound antioxidant system inhibits essential oil high-temperature cracking, and through 45~55 DEG C hot air is matched with cold air gradient control fragrance synchronous removal plastic odor.The application realizes long-acting fragrance, broad-spectrum antibacterial and anti-mite under the premise of not destroying fiber resilience fatigue performance, and the modified material is more than 99% to staphylococcus aureus and escherichia coli inhibition rate, and the anti-mite repellent rate is 76%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polyolefin air fiber modification and processing technology, specifically to a fragrance-enhancing, deodorizing, and functional modification formula and process for air fiber materials. Background Technology

[0002] The mainstream substrate for air fiber is polyolefin elastomer (POE), and the production cost is significantly constrained by the grade of raw materials. Low-odor, high-end POE raw materials are expensive, while economical general-purpose POE raw materials are inexpensive, but the resin polymerization process leaves behind small molecule impurities such as alkanes, aldehydes, and ketones, resulting in air fiber products with a noticeable plastic odor. Mid- to low-end products cannot simultaneously balance production costs and sensory user experience. Summary of the Invention

[0003] The purpose of this invention is to provide a fragrance-enhancing, deodorizing, and functional modification formula and process for air fiber materials, which can efficiently remove the inherent plastic odor of raw materials without reducing the resilience and fatigue mechanical properties of air fibers, significantly extend the fragrance retention time, and endow the materials with broad-spectrum antibacterial and mite-repellent functions.

[0004] The technical solution of the present invention:

[0005] A fragrance-enhancing, deodorizing, and functional modification formula for an air-fiber material, comprising, by weight, the following raw material components: 80-120 parts POE base material, 0.3-1.0 parts antioxidant masterbatch, and 0.03-0.12 parts essential oil.

[0006] By weight, the raw material composition is: 90-110 parts POE base, 0.4-0.8 parts antioxidant masterbatch, and 0.05-0.09 parts essential oil.

[0007] By weight, the raw material composition is: 100 parts POE base material, 0.5 parts antioxidant masterbatch, and 0.06 parts essential oil.

[0008] The raw materials for preparing the antioxidant masterbatch comprise, by weight: 70 parts polyolefin elastomer, 8 parts maleic anhydride-grafted polyolefin, 3 parts erucamide, 3 parts thiophenol antioxidant 300, and 6 parts phosphite antioxidant 168.

[0009] The essential oil is a blend of clove bud essential oil and lemongrass essential oil, with a weight ratio of 2:1 between the two.

[0010] The clove bud essential oil has a purity of ≥98% and a thermal decomposition temperature of ≥170℃.

[0011] A process for enhancing fragrance, removing odors, and functionalizing an air-conditioning fiber material includes the following steps:

[0012] S1. Pre-made antioxidant compatibility masterbatch: The masterbatch raw materials are fed according to the formula. Polyolefin elastomer, maleic anhydride grafted polyolefin, and erucamide are added to the mixing tank and stirred for 10-15 minutes, then fed into the solid material tank of a two-stage granulator. Thiophenolic antioxidant 300 and phosphite antioxidant 168 are fed into the powder material tank. The processing temperature of the two-stage granulator is 160-170℃, the ratio of solid material to powder material feeding rate is 1:4, the screw speed is 30-40 r / min, and the granulation is repeated twice. The granulated product is placed in a 60℃ environment for constant temperature curing for 2 hours to obtain an antioxidant compatibility masterbatch with a total antioxidant content of 10%.

[0013] S2. Material blending, atomization, and fragrance addition: Take the corresponding weight parts of POE base material and antioxidant masterbatch and put them into the mixing tank. Stir at a speed of 30-50 r / min. Use a precision atomization spray system to spray the compounded essential oil and continue stirring for 15 minutes to make the essential oil evenly adsorbed on the surface of the resin particles.

[0014] S3. Extrusion molding: The mixture is fed into the extruder, and the temperature of each heating zone is controlled at 170-180℃. After traction and water cooling, a continuous air fiber roll is obtained.

[0015] S4. Hot air deodorization and fragrance control: The formed air fiber roll is sent into a 45-55℃ hot air circulating oven for constant temperature treatment for 15 minutes to remove small molecules of alkanes, aldehydes and ketones that are inherent in the substrate, and to volatilize excess essential oils on the surface.

[0016] S5. Cold Air Setting: After hot air treatment, the roll material is rapidly cooled and set by blowing room temperature air at a flow rate of 2-5 m / s for 10 minutes, locking in the aromatic antibacterial components within the fibers. Beneficial Effects of this Invention: This invention constructs a three-dimensional functional network of "molecular anchoring-synergistic antioxidant-gradient release":

[0017] (1) Reactive compatibilization and anchoring: Maleic anhydride grafted onto POE is introduced. Its anhydride group can form hydrogen bonds or undergo esterification with the hydroxyl groups (eugenol) in the essential oil, chemically anchoring the essential oil molecules to the molecular chain of the matrix resin, greatly delaying the physical migration and volatilization of the essential oil during long-term use, and extending the aroma retention time.

[0018] (2) Synergistic antioxidant and stabilizing: Thiophenolic antioxidants are the main component, and phosphite antioxidants are the auxiliary component to form an antioxidant system, which inhibits the thermal decomposition of essential oils while ensuring the physical properties of the product.

[0019] (3) "Hot blowing-cold fixing" gradient fragrance control: Utilizing the difference in vapor pressure of different essential oil components, low-boiling-point odor aldehydes and ketones are preferentially removed during the hot air treatment stage, while retaining core antibacterial components such as high-boiling-point eugenol, so as to achieve a dynamic balance between deodorization and fragrance retention.

[0020] To demonstrate the effectiveness of this invention, the applicant conducted the following comparative experiments:

[0021] Performance Testing and Results Analysis

[0022] Mechanical fatigue properties

[0023] According to the industry standard QB / T 2819-2006 "Determination of Long-Term Fatigue Performance of Flexible Foam Materials", constant amplitude fatigue tests were conducted on blank samples (without essential oil) and air fiber samples with three kinds of essential oils (80,000 cycles, 40% hardness load). The results are shown in the table below.

[0024] Table 1 Fatigue performance test results

[0025]

[0026] Tests showed that the hardness index, hardness loss rate, and thickness loss rate of the samples after adding essential oil were not significantly different from those of the blank sample (the deviations were all within the experimental error range), and the surfaces remained dry and oil-free, indicating that the addition of essential oil did not have an adverse effect on the cross-linking network and epidermal properties of the material matrix.

[0027] 4.2 Sensory evaluation of odor

[0028] A blind test was conducted, in which six evaluators with a keen sense of smell evaluated the odor of different samples. The results are summarized in Table 2.

[0029] Table 2 Sensory Evaluation Table of Air Fiber Odor with Added Essential Oils

[0030]

[0031] Samples of multi-component essential oils and single essential oils were placed separately in a 50℃ constant temperature incubator for accelerated aging for 7 days, followed by odor evaluation. The results are summarized in Table 3:

[0032] Table 3. Sensory Evaluation Table of Odor After Accelerated Aging

[0033]

[0034] The evaluation results in Tables 2 and 3 show that all evaluators found the 0.06% essential oil addition level acceptable and comfortable, while the 0.12% level was generally considered too strong, with some experiencing negative reactions. Furthermore, the multi-essential oil blend samples retained a discernible, light fragrance after aging, while the single-essential oil samples almost lost their aroma. This demonstrates that the multi-essential blend and compatibilization anchoring technology effectively improved fragrance longevity. Therefore, 0.06% multi-essential oil blend is the recommended optimal addition ratio, effectively masking odors while providing a pleasant olfactory experience.

[0035] Antibacterial and anti-mite properties

[0036] Based on the corresponding antibacterial and anti-mite testing standards (specific methods omitted), the blank sample and the sample containing 0.06% multi-component compound essential oil were compared and tested. The results are shown in Table 4.

[0037] Table 4 Results of antibacterial and anti-mite performance tests

[0038]

[0039] The results showed that the air fiber modified with multi-component essential oils had significantly better antibacterial and anti-mite repellency rates against all tested bacteria than the blank sample, and exceeded the standard effective values, confirming that the process endowed the material with excellent broad-spectrum antibacterial and anti-mite functions.

[0040] in conclusion

[0041] This invention discloses a process for enhancing the fragrance, deodorizing, and functionalizing air-filtering fiber materials, which has the following significant advantages:

[0042] 1. Compound essential oil system: Clove bud essential oil is the main fragrance-enhancing and antibacterial component, supplemented by lemongrass essential oil as a fragrance-carrying agent, to achieve a rich aroma and good processing thermal stability.

[0043] 2. Reactive compatibilization technology: By grafting polyolefins with maleic anhydride, essential oil molecules are chemically anchored to the matrix, which greatly extends the aroma retention time and retains a recognizable fragrance even after accelerated aging.

[0044] 3. Synergistic antioxidant protection: The combination of antioxidants 300 and 168 effectively inhibits the thermal decomposition of essential oils and the oxidative degradation of the POE matrix, ensuring the safety of the processing and the long-term mechanical stability of the product;

[0045] 4. "Hot air-cold air" gradient fragrance control: After treating with hot air at 45-55℃ for 15 minutes, it is combined with cold air blowing to achieve efficient removal of odors and retention of suitable fragrance;

[0046] 5. Excellent hygiene function: With an essential oil content of 0.06%, the material has an antibacterial rate of over 99% against Staphylococcus aureus, Escherichia coli, and Candida albicans, and a mite repellency rate of 76%, far exceeding industry standards.

[0047] 6. Optimal process parameters: The total amount of essential oil added is 0.06% of the base material mass (including 0.04% clove bud essential oil and 0.02% lemongrass essential oil), the antioxidant masterbatch is added at 0.5% (corresponding to an antioxidant net content of about 0.05%), the processing temperature is 170~180℃, the hot air treatment is 45~55℃×15 min, and the cold air is blown for 10 min.

[0048] This process comprehensively solves technical challenges such as odor masking, fragrance retention, antibacterial and anti-mite properties without sacrificing the mechanical properties of air fibers. The process is simple, can be continuously produced, and has broad prospects for industrial application. Detailed Implementation

[0049] The present invention will be further described below with reference to embodiments, but these embodiments are not intended to limit the scope of the invention.

[0050] Example 1.

[0051] 1. Preparation of antioxidant polyolefin masterbatch

[0052] ① Add 70 parts of polyolefin elastomer, 8 parts of maleic anhydride grafted polyolefin and 3 parts of erucamide to a mixing tank and stir for 10-15 minutes. Then, put it into the solid tank of a two-stage granulator. Then, put 3 parts of thiophenol antioxidant 300 and 6 parts of phosphite antioxidant 168 into the powder tank.

[0053] ② The equipment processing temperature is 160-170℃, the powder to solid feeding rate is 1:4, the screw speed is 30-40r / min, and granulation needs to be repeated twice to ensure granulation uniformity;

[0054] ③ Finally, place it in a heated and stirred tank at 60℃ for 2 hours to obtain a polyolefin masterbatch with an antioxidant content of 10%.

[0055] 2. Preparation of Fragrance-Enhancing Air Fibers

[0056] 2.1 Preparation of Air Fibers from Multi-component Essential Oils

[0057] ① Addition and mixing of essential oils and antioxidants: First, add 100 parts of POE base material and 0.5 parts of antioxidant masterbatch to the mixing tank, start the stirrer (speed approximately 30-50 r / min), and then precisely and evenly spray 0.04 parts of clove bud essential oil and 0.02 parts of lemongrass essential oil into the tank using a small atomizing spray bottle. Continue stirring for 15 minutes to ensure that the essential oils form a uniform thin layer on the surface of the particles.

[0058] ② Extrusion molding: Set the temperature range of each heating zone of the extruder to 170~180 ℃, and keep other process parameters (such as screw speed, traction speed, cooling water temperature, etc.) consistent with conventional production.

[0059] ③ Hot air deodorization and cold air setting: The formed air-fiber roll is immediately sent to a hot air treatment device and placed in a constant temperature oven at 45-55 ℃ for 15 minutes. This stage aims to accelerate the volatilization of residual essential oil molecules, while using their entrainment effect to remove low-molecular-weight odor substances such as alkanes and aldehydes contained in the raw material itself. This temperature and time window must be strictly controlled to prevent the fibers from creeping due to excessive heating, which would affect their resilience. Subsequently, the sample is transferred to a cold air device (room temperature air, flow rate 2-5 m / s) and blown for 10 minutes to accelerate the volatilization and cooling of the surface essential oils, ultimately allowing the material to retain a trace of fragrance, achieving a sensory effect of "a subtle fragrance that is not cloying after a long time".

[0060] Example 2

[0061] Antioxidant masterbatch prefabrication

[0062] Take 70 parts by weight of polyolefin elastomer, 8 parts by weight of POE-g-MAH (grafting rate 1.2%), and 3 parts by weight of erucamide and stir for 12 min; the feeding ratio of solid material tank to powder material tank is 4:1, the powder components are 3 parts of antioxidant 300 and 6 parts of antioxidant 168; the extrusion temperature is 165℃, the screw speed is 35 r / min, repeat granulation twice, and cure at 60℃ for 2 h to obtain masterbatch with antioxidant content of 10%.

[0063] Raw material ratio: 80 parts POE base material, 0.3 parts of the above masterbatch, 0.03 parts compound essential oil (clove bud essential oil: lemongrass essential oil = 2:1).

[0064] Processing steps:

[0065] S1 Pre-made masterbatch as above; S2 Stirring speed 30r / min, atomized spray essential oil, stir for 15min; S3 Extrusion temperature 170~180℃ to form roll material; S4 45℃ hot air treatment for 15min; S5 Room temperature airflow 2m / s to blow for 10min, shape and rewind.

[0066] Example 3

[0067] The preparation process of the antioxidant masterbatch is completely consistent with that of Example 1.

[0068] Raw material ratio: 100 parts POE base, 0.6 parts antioxidant masterbatch, 0.07 parts compound essential oil (clove bud essential oil: lemongrass essential oil = 2:1).

[0069] All process parameters for blending, extrusion, hot air, and cold air post-treatment are the same as in Example 1.

[0070] Example 4

[0071] Antioxidant-compatible masterbatch pre-preparation (parts by weight)

[0072] Take 70 parts of POE elastomer, 8 parts of POE-g-MAH with a grafting rate of 1.2%, and 3 parts of erucamide and put them into an automatic mixing tank. Mix and stir for 12 minutes. Send the mixed solid material into the solid material tank of a two-stage granulator. Send 3 parts of thiophenol antioxidant 300 and 6 parts of phosphite antioxidant 168 into the powder material tank.

[0073] The extrusion temperature of the equipment was set at 165℃, the screw speed at 35r / min, the ratio of solid material to powder material feeding rate was 4:1, and the material was granulated twice. After granulation, the material was sent to a 60℃ constant temperature maturation mixing tank for 2 hours to obtain antioxidant compatibility masterbatch with a total antioxidant content of 10%.

[0074] Air fiber modified ingredients

[0075] The composition includes 100 parts of POE base material, 0.5 parts of the antioxidant masterbatch prepared above, and 0.06 parts of compound essential oils, including 0.04 parts of clove bud essential oil and 0.02 parts of lemongrass essential oil; the purity of clove bud essential oil is 98.5%, and the thermal decomposition temperature is 172℃; the grafting rate of POE-g-MAH is 1.2%.

[0076] Processing steps

[0077] The operation of S1 pre-made masterbatch is the same as above;

[0078] S2 Material Blending, Atomization, and Fragrance Addition: Add 100 parts of POE base material and 0.5 parts of antioxidant masterbatch to the mixing tank and stir at 40 r / min; turn on the precision atomizing spray device and evenly spray the mixture of clove bud essential oil and lemongrass essential oil, and continue stirring for 15 minutes to ensure that the essential oils are evenly adsorbed on the surface of the resin particles.

[0079] S3 Extrusion Molding: The mixture is fed into the extruder, and the temperature of each heating zone is controlled at 170-180℃. The traction speed and cooling water temperature follow the factory's conventional production parameters. The mixture is extruded to form a continuous mesh air fiber roll.

[0080] S4 Hot Air Deodorization and Fragrance Control: The fiber roll is sent into a 50℃ hot air circulating oven for 15 minutes to remove residual small molecule odors from the substrate and volatilize excess essential oils on the surface.

[0081] S5 Cold Air Setting: The hot air treated roll material is transferred to the cold air channel and blown for 10 minutes at a room temperature air flow rate of 3m / s to cool, set, and rewind, thus obtaining the finished modified air fiber.

[0082] Comparative Example 1: Blank Air Fiber Sample

[0083] Using only 100 parts of POE base material for direct extrusion molding, with the addition of existing conventional antioxidant masterbatch and no added essential oils, and following the existing extrusion process, it serves as a performance blank control sample.

Claims

1. A fragrance-enhancing, deodorizing, and functional modification formula for an air-fiber material, characterized in that, By weight, it consists of the following raw material components: 80-120 parts POE base, 0.3-1.0 parts antioxidant masterbatch, and 0.03-0.12 parts essential oil.

2. The fragrance-enhancing, deodorizing, and functional modification formula for air-conditioning fiber materials according to claim 1, characterized in that, By weight, the raw material composition is: 90-110 parts POE base, 0.4-0.8 parts antioxidant masterbatch, and 0.05-0.09 parts essential oil.

3. The fragrance-enhancing, deodorizing, and functional modification formula for air-fiber materials according to claim 2, characterized in that, By weight, the raw material composition is: 100 parts POE base material, 0.5 parts antioxidant masterbatch, and 0.06 parts essential oil.

4. The fragrance-enhancing, deodorizing, and functional modification formula for an air-conditioning fiber material according to any one of claims 1 to 3, characterized in that, The raw materials for preparing the antioxidant masterbatch comprise, by weight: 70 parts polyolefin elastomer, 8 parts maleic anhydride-grafted polyolefin, 3 parts erucamide, 3 parts thiophenol antioxidant 300, and 6 parts phosphite antioxidant 168.

5. The fragrance-enhancing, deodorizing, and functional modification formula for an air-conditioning fiber material according to any one of claims 1 to 3, characterized in that, The essential oil is a blend of clove bud essential oil and lemongrass essential oil, with a weight ratio of 2:1 between the two.

6. The fragrance-enhancing, deodorizing, and functional modification formula for air-conditioning fiber materials according to claim 5, characterized in that, The clove bud essential oil has a purity of ≥98% and a thermal decomposition temperature of ≥170℃.

7. A fragrance-enhancing, deodorizing, and functional modification process for air-fiber materials, characterized in that, Processing using any of the modified formulations according to claims 1 to 6 includes the following steps: S1. Pre-made antioxidant compatibility masterbatch: The masterbatch raw materials are fed according to the formula. Polyolefin elastomer, maleic anhydride grafted polyolefin, and erucamide are added to the mixing tank and stirred for 10-15 minutes, then fed into the solid material tank of a two-stage granulator. Thiophenolic antioxidant 300 and phosphite antioxidant 168 are fed into the powder material tank. The processing temperature of the two-stage granulator is 160-170℃, the ratio of solid material to powder material feeding rate is 1:4, the screw speed is 30-40 r / min, and the granulation is repeated twice. The granulated product is placed in a 60℃ environment for constant temperature curing for 2 hours to obtain an antioxidant compatibility masterbatch with a total antioxidant content of 10%. S2. Material blending, atomization, and fragrance addition: Take the corresponding weight parts of POE base material and antioxidant masterbatch and put them into the mixing tank. Stir at a speed of 30-50 r / min. Use a precision atomization spray system to spray the compounded essential oil and continue stirring for 15 minutes to make the essential oil evenly adsorbed on the surface of the resin particles. S3. Extrusion molding: The mixture is fed into the extruder, and the temperature of each heating zone is controlled at 170-180℃. After traction and water cooling, a continuous air fiber roll is obtained. S4. Hot air deodorization and fragrance control: The formed air fiber roll is sent into a 45-55℃ hot air circulating oven for constant temperature treatment for 15 minutes to remove small molecules of alkanes, aldehydes and ketones that are inherent in the substrate, and to volatilize excess essential oils on the surface. S5. Cold air setting: After the hot air treatment, room temperature air at a flow rate of 2-5 m / s is used to blow the roll material for 10 minutes to quickly cool and set the shape, locking in the aromatic antibacterial components inside the fiber.